Shape memory nano enzyme sponge as well as preparation method and application thereof

Through the drop-extrusion operation of the shape memory nanozyme sponge and the catalytic reaction of the noble metal nanozyme, the problem of amplification and reuse of the nanozyme colorimetric sensing detection signal is solved, and the quantitative detection and reproducibility of low-concentration hydrogen peroxide are achieved. Multiplexing detection reduces detection costs.

CN118755142AActive Publication Date: 2024-10-11XI AN JIAOTONG UNIV

Patent Information

Application Number
CN202410830277.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-11
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

Existing nanozyme-based colorimetric sensing assays are difficult to amplify or reuse sensing signals, and are difficult to detect trace amounts of analytes.

Method used

A shape memory nanozyme sponge composed of chitosan, polyN,N'-methylenebisacrylamide and polyacrylic acid is used, and noble metal nanozymes are distributed. Positively charged dyes are enriched and utilized through a dropping-extrusion operation. The noble metal nanozyme catalyzes the reaction to generate colored products, achieving signal amplification and reusable detection signals.

Benefits of technology

It achieves quantitative detection and reusable detection of low-concentration hydrogen peroxide, reduces detection costs, and improves the performance and deviceization of sensing detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755142A_ABST
    Figure CN118755142A_ABST
Patent Text Reader

Abstract

The invention discloses shape memory nano enzyme sponge as well as a preparation method and application thereof, and belongs to the technical field of functional materials. The main structure of the shape memory nano-enzyme sponge is composed of chitosan, poly N, N '-methylene bisacrylamide and polyacrylic acid, and precious metal nano-enzymes are distributed in the main structure; the nano-enzyme sponge is prepared from hydrogel, and the precious metal nano-enzyme is combined with the shape memory sponge, so that reusable sensing of the nano-enzyme and amplification of a detection signal are realized, meanwhile, instrumentation of nano-enzyme sensing detection is facilitated, and the device is hydrogen peroxide detection equipment which is simple to prepare, stable in property, light in weight and portable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of functional materials, and in particular relates to a shape memory nanoenzyme sponge and a preparation method and application thereof. Background Art

[0002] Nanozymes are a class of nanomaterials with similar activities to natural enzymes. Since the early use of ferroferric oxide nanoparticles as peroxidase (POD) for enzyme-linked immunosorbent assay, nanozymes have been widely explored in many aspects such as catalytic mechanism, material composition, and application scenarios. From an application perspective, the development of analyte detection strategies based on nanozymes is the most popular. Generally speaking, the general process of using the nanozyme sensor is to disperse the nanozyme into a sample containing the analyte and the auxiliary substrate (such as TMB or ABTS). After the enzyme-catalyzed reaction is completed, the signal from the oxidation product of the auxiliary substrate, such as the absorbance of oxTMB or oxABTS, is recorded and converted into the concentration of the analyte by calculation. For example, there have been many studies based on peroxidase nanozymes to detect substances such as hydrogen peroxide (H2O2), glucose, and uric acid.

[0003] At present, almost all nanozyme-based detection strategies are carried out directly in aqueous solution. Despite the good results, there are still some problems. First, the acquisition of sensor signals relies more on spectrometers, which is not conducive to the development of point-of-care testing (POCT) equipment. Secondly, due to the good dispersibility of nanozymes, it is difficult to use the same system for reusable detection. Third, it is difficult to further amplify the sensor signal to detect trace analytes in the sample. Although the traditional lateral flow test paper method can meet the requirements of POCT, it is difficult to reuse or further amplify the detection signal.

[0004] Gel is a loose and porous material, and its macroporous surface can provide a wide space for the loading of nanozymes. Some studies have tried to use agarose hydrogel to load nanozymes for analyte sensing in gel, but it is difficult for this type of hydrogel to use its own characteristics to assist nanozymes in achieving repeatable and signal-amplified detection. In addition, metal aerogels have also been shown to have nanozyme activity and can be used to detect analytes, but their nearly black appearance may mask color signals and make it difficult to amplify detection signals; therefore, it is still difficult to directly apply gels to the detection of nanozymes. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a shape memory nanozyme sponge and a preparation method and application thereof, so as to solve the problems in the prior art that nanozyme colorimetric sensing detection is difficult to amplify or further process the sensing signal, and nanozyme colorimetric sensing is difficult to reuse.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A shape memory nanozyme sponge, the main body of which is composed of chitosan, poly-N,N'-methylenebisacrylamide and polyacrylic acid, and noble metal nanozymes are distributed in the main body.

[0008] A method for preparing a shape memory nanozyme sponge comprises the following steps:

[0009] Step 1, adding a protective agent solution and a noble metal solution to water, and then adding a reducing agent solution, to obtain a noble metal nanozyme solution after reaction; the noble metal solution is a noble metal salt solution or a noble metal acid solution;

[0010] Step 2, the acrylic acid aqueous solution of N,N'-methylenebisacrylamide, the chitosan solution and the noble metal nanozyme solution are mixed and precooled, and then ammonium persulfate solution and potassium pyrosulfite solution are added dropwise after precooling, and the mixture is thawed after freeze polymerization, and dried to obtain a shape memory nanozyme sponge.

[0011] A further improvement of the present invention is:

[0012] Preferably, in step 1, the mixing volume ratio of the protective agent solution, the noble metal solution, the reducing agent solution and water is (4-7): (1-10): (3-5): (28-42).

[0013] Preferably, in step 1, the noble metal acid solution is chloroplatinic acid or chloroauric acid, and the noble metal salt solution is ruthenium trichloride.

[0014] Preferably, in step 2, the volume ratio of the aqueous solution of N,N'-methylenebisacrylamide in acrylic acid, the chitosan solution and the noble metal nanozyme solution is (120-180):(60-100):(1-50).

[0015] An application of the shape memory nanozyme sponge, wherein the shape memory nanozyme sponge is used to adsorb positively charged dye molecules or negatively charged dye molecules.

[0016] The positively charged dye is toluidine blue O, crystal violet, methylene blue or 3,3',5,5'-tetramethylbenzidine oxidation product.

[0017] The negatively charged dye includes bromophenol blue, thymol blue, litmus or 2,2'-azinobis-(3-ethylbenzothiazoline-6-sulfonic acid) oxidation product.

[0018] Preferably, the shape memory nanozyme sponge is enriched with positively charged dye molecules on the sponge body by repeatedly performing a "drip-squeeze" operation.

[0019] Preferably, the noble metal nanozyme in the shape memory nanozyme sponge can catalyze the reaction of 3,3',5,5'-tetramethylbenzidine and hydrogen peroxide to generate blue oxTMB, and the blue oxTMB is used to reflect the concentration of hydrogen peroxide.

[0020] Preferably, the reaction of TMB and hydrogen peroxide is as follows: TMB solution, hydrogen peroxide solution and NaAc-HAc buffer solution are evenly mixed and then dripped onto the nanozyme sponge, and the "drip-squeeze" operation is repeated until all the reaction solutions are dripped, and the concentration of hydrogen peroxide is judged by the color on the nanozyme sponge.

[0021] The volume ratio of TMB, hydrogen peroxide solution, and NaAc-HAc buffer solution is (1-10):(1-10):(280-300).

[0022] Preferably, the shape memory nanozyme sponge is subjected to a "dripping-squeezing-washing" operation to separate the negatively charged dye molecules originally contained in the sponge body from the sponge body.

[0023] Preferably, the noble metal nanozyme in the shape memory nanozyme sponge can catalyze the reaction of 2,2'-azinobis-(3-ethylbenzothiazoline-6-sulfonic acid) and hydrogen peroxide to generate oxATBS, and the oxATBS is used to reflect the concentration of hydrogen peroxide.

[0024] Preferably, the steps of reacting ABTS and hydrogen peroxide are: uniformly mixing ABTS solution, hydrogen peroxide solution and NaAc-HAc buffer solution in proportion and then dripping the mixture onto the nanozyme sponge; after the reaction is complete, judging the concentration of hydrogen hydroxide by the color on the nanozyme sponge; squeezing and washing the nanozyme sponge;

[0025] The steps of dripping, squeezing and washing are repeated, and the nanozyme sponge is used repeatedly;

[0026] The mixing volume ratio of ABTS solution, hydrogen peroxide solution and NaAc-HAc buffer solution is (1-10):(1-10):(280-300).

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The present invention discloses a shape memory nanozyme sponge, the main structure of which is composed of chitosan, poly N, N'-methylenebisacrylamide and polyacrylic acid, and noble metal nanozymes are distributed in the main structure. The nanozyme sponge is prepared from hydrogel, which is a material with a porous network structure formed by cross-linking of macromolecular substances or high molecular polymers. After freeze drying, a sponge-like substance can be formed. Its conventional shape memory process can be described as follows: in a water-containing state, the water contained in the shape memory sponge can be pressed and squeezed out, and presents a compressed state. In this state, re-absorption of water can make it expand to its original shape. Repeatedly, the shape memory sponge can complete multiple rounds of shape memory effect. The main structure of the present invention is distributed with noble metal nanozymes with POD-like activity, which can catalyze the co-reaction of hydrogen peroxide and auxiliary substrates (such as TMB and ABTS) to generate colored products (such as oxTMB and oxABTS), and the quantitative test of hydrogen peroxide concentration is completed by the optical signal of the colored product. At the same time, the nanozyme sponge in the present invention has a strong adsorption effect on positively charged dye molecules (such as oxTMB), but has a weak adsorption capacity for negatively charged dye molecules (such as oxABTS), so that the "enrichment amplification" or "clearance to zero" of specific detection signals can be achieved. Finally, by organically combining the catalytic function of precious metal nanozymes, the adsorption capacity of nanozyme sponges for different enzyme catalytic products, and its own shape memory effect, the reusable sensing of nanozymes and the amplification of detection signals are realized, and the deviceization of nanozyme sensing detection is also facilitated. It is a hydrogen peroxide detection equipment with simple preparation, stable properties, light weight and portability.

[0029] The present invention expands the types of nanozyme materials from a broad category. The porous structure of the sponge can adsorb the analyte, and the difference in the type of analyte molecules makes its capacity to accommodate in the sponge different. Based on these characteristics, it is expected to achieve cumulative detection of analytes or achieve repeatable detection. Specifically, the shape memory nanozyme sponge can be used to adsorb positively and negatively charged dye molecules, wherein the positively charged dye molecules will not be separated from the sponge body due to being washed by an aqueous solution, and the negatively charged dye molecules will be separated from the sponge body due to being washed by an aqueous solution. The sensor improves the performance of sensing detection, and hydrogen peroxide detection is selected as a representative application to evaluate its detection effect. The shape memory nanozyme sponge described in the present invention has excellent peroxidase activity, and different detection effects of hydrogen peroxide are achieved by reacting with different chromogenic substrates. The specific analysis is:

[0030] (1) The shape memory nanozyme sponge described in the present invention, after catalyzing the reaction of hydrogen peroxide and TMB, can enrich and accumulate the oxTMB color signal on the sponge through repeated "drip-squeeze" method due to the strong adsorption of the generated oxTMB on the sponge, thereby realizing the quantitative detection of low-concentration hydrogen peroxide that cannot be accomplished by the traditional nanozyme sensor in a pure aqueous medium, and ultimately improving the detection capability of low-concentration hydrogen peroxide.

[0031] The shape memory nanozyme sponge of the present invention, after catalyzing the reaction of hydrogen peroxide and ABTS, quantitatively detects the concentration of hydrogen peroxide by the color intensity of the oxidation product oxABTS. Due to the weak adsorption of the generated oxABTS on the sponge, the newly generated oxABTS on the sponge is completely eluted each time by the "squeezing-washing" method, so that the sponge returns to its initial state, so that the next round of detection can be continued without interference. The above process is repeated cyclically to achieve reusable quantitative detection of hydrogen peroxide that cannot be completed by nanozyme sensors in traditional pure aqueous media. Ultimately, the purpose of multiple detection of hydrogen peroxide using the same detection device is achieved, reducing the overall cost of detection. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Schematic diagram of the process of nanozyme sponge achieving shape memory, namely the initial state of the nanozyme sponge, the deformation state of the nanozyme sponge, and the shape recovery state of the nanozyme sponge.

[0033] Figure 2 Cyclic compression performance of shape memory nanozyme sponge.

[0034] Figure 3 This is the adsorption effect of 8 dye molecules with different electrical properties on the nanozyme sponge.

[0035] Figure 4 The zeta potential of 8 dye molecules with different electrical properties and their respective adsorption efficiency on the nanozyme sponge.

[0036] Figure 5 The standard curve for the detection of hydrogen peroxide by the shape memory nanozyme sponge based on the chromogenic substrate TMB;

[0037] Figure 6 It is a general operation flow chart of the signal enrichment process in the accumulation detection.

[0038] Figure 7 This is a visual effect diagram of the shape memory nanozyme sponge detecting hydrogen peroxide based on the accumulation of the chromogenic substrate TMB;

[0039] Figure 8 It is based on repeated "drip-squeeze" enrichment operation and single operation detection of hydrogen peroxide sample and comparison with theoretical value.

[0040] Fig. 9 The standard curve for the detection of hydrogen peroxide by shape memory nanozyme sponge based on the chromogenic substrate ABTS;

[0041] Fig.10 The general operation flow chart of the reusable detection of hydrogen peroxide.

[0042] Fig.11 This is a visual effect diagram of the shape memory nanozyme sponge based on the colorimetric substrate ABTS for reusable detection of hydrogen peroxide;

[0043] Fig.12 To determine the accuracy of a reproducible assay for hydrogen peroxide based on a “squeeze-and-clean” procedure. DETAILED DESCRIPTION

[0044] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0045] The first aspect of the present invention discloses a shape memory nanozyme sponge, the main body of which is composed of chitosan, poly-N,N'-methylenebisacrylamide and polyacrylic acid, and noble metal nanozymes are distributed therein.

[0046] The freeze-drying process described in the present invention is carried out in a mold, and the initial shape of the prepared shape memory nanozyme sponge is the shape of the mold, and after molding, it can be cut into small pieces for standby use.

[0047] The second aspect of the present invention discloses a method for preparing a shape memory nanozyme sponge, comprising the following steps:

[0048] Step 1, preparation of noble metal nanozymes stabilized by different protective agents:

[0049] The protective agent molecules are dissolved in water to prepare a protective agent solution with a concentration of 1 to 50 mg / mL; the precious metal salt or precious metal acid is dissolved in deionized water to prepare a precious metal salt solution or precious metal acid solution with a concentration of 1 to 100 mM; the protective agent solution and the precious metal salt solution or precious metal acid solution are gradually added to the deionized water; a reducing agent solution with a concentration of 10 to 200 mM is added dropwise to the above mixed solution, and the reaction is carried out at room temperature for 30 to 60 minutes to obtain a precious metal nanozyme solution.

[0050] Step 2, dissolving N,N'-methylenebisacrylamide (MBA) in an aqueous solution of acrylic acid (AA) to prepare an MBA AA solution with a concentration of 1 to 20 mg / mL; then adding a pre-prepared chitosan (CS) solution; then, adding the precious metal nanozyme solution prepared in step 1 to the above mixed solution, placing it at -20°C for precooling, and adding ammonium persulfate solution and potassium metabisulfite solution dropwise at room temperature to obtain a final solution, which is frozen and polymerized at -20°C, taken out for thawing, soaked and cleaned with deionized water, and dried to obtain a nanozyme sponge with shape memory.

[0051] Preferably, in step 1, the protective agent is chitosan, polyvinyl pyrrolidone, glutathione, polydopamine or albumin.

[0052] Preferably, in step 1, the noble metal salt or acid is chloroplatinic acid, ruthenium trichloride or chloroauric acid.

[0053] Preferably, in step 1, the reducing agent is ascorbic acid, sodium borohydride, sodium citrate, hydroxylamine or hydrazine hydrate, etc., and the reducing agent can reduce the noble metal salt or noble metal acid into metal element nanozyme particles with enzyme activity.

[0054] Preferably, in step 1, the volume ratio of the protective agent solution, the noble metal salt or acid solution, the reducing agent solution and the deionized water is (4-7): (1-10): (3-5): (28-42).

[0055] Preferably, in step 2, the volume ratio of the MBA AA solution, CS solution and noble metal nanozyme solution is (120-180): (60-100): (1-50).

[0056] Preferably, in step 2, the concentration of CS in the final solution is 4-10 mg / mL;

[0057] Preferably, in step 2, the volume concentration of the metal nanozyme solution in the final solution is 0.3-25%;

[0058] Preferably, in step 2, the concentrations of the ammonium persulfate solution and the potassium metabisulfite solution in the final solution are both 0.5-2 mg / mL.

[0059] Preferably, in step 2, the precooling time is 10 to 60 minutes.

[0060] Preferably, in step 2, the freezing polymerization time is 5 to 20 hours.

[0061] The third aspect of the present invention discloses an application of a shape memory nanozyme sponge, which can be used to adsorb dye molecules, wherein positively charged dye molecules will not be separated from the sponge body due to being washed by an aqueous solution, and negatively charged dye molecules will be separated from the sponge body due to being washed by an aqueous solution. The shape memory nanozyme sponge can enrich the positively charged dye molecules contained in the sponge body by repeatedly performing the "drip-squeeze" operation, and can separate the negatively charged dye molecules originally contained in the sponge body from the sponge body by the "squeeze-wash" operation.

[0062] Exemplarily, the positively charged dye can be toluidine blue O (TBO), crystal violet (CV), methylene blue (MB) or 3,3',5,5'-tetramethylbenzidine oxidation product (oxTMB).

[0063] Exemplarily, the negatively charged dye can be bromophenol blue (BB), thymol blue (TB), litmus or 2,2'-azinobis-(3-ethylbenzothiazoline-6-sulfonic acid) oxidation product (oxABTS).

[0064] In some embodiments of the present invention, the steps of enriching the positively charged dye molecules in the sponge body by repeatedly performing the "drip-squeeze" operation are:

[0065] (1) preparing positively charged dye molecules into corresponding aqueous solutions;

[0066] (2) During the enrichment process, the dye solution in step (1) is evenly dripped onto the nanozyme sponge, and after squeezing out excess water, the same dye solution is dripped again. By repeatedly performing the "drip-squeeze" operation, the positively charged dye molecules are enriched in the nanozyme sponge.

[0067] In some embodiments of the present invention, the step of removing negatively charged dye molecules from the sponge body by performing a "squeeze-wash" operation is:

[0068] (1) preparing negatively charged dye molecules into corresponding aqueous solutions;

[0069] (2) The dye solution in step (1) is evenly dripped onto the nanozyme sponge. During the cleaning process, excess water is removed by squeezing, and then the nanozyme sponge is cleaned with pure water until the nanozyme sponge returns to its initial colorless state. The same operation steps are performed, and the negatively charged dye molecules can be removed from the nanozyme sponge each time during multiple cycles.

[0070] The fourth aspect of the present invention discloses a sensing detection application of a shape memory nanozyme sponge, which detects hydrogen peroxide through the color change of the oxidation product of 3,3',5,5'-tetramethylbenzidine (TMB) or 2,2'-azinobis-(3-ethylbenzothiazoline-6-sulfonic acid) (ABTS).

[0071] In some embodiments of the present invention, based on the single detection of hydrogen peroxide by TMB, the reaction of TMB and hydrogen peroxide is catalyzed by precious metal nanozymes, so that the concentration of hydrogen peroxide can be displayed by the color intensity on the sponge. The specific steps are:

[0072] (1) dissolving TMB in dimethyl sulfoxide to prepare a TMB solution;

[0073] (2) During the detection process, the TMB solution, hydrogen peroxide solutions of different concentrations, and NaAc-HAc buffer solution were mixed evenly in proportion, and then dropped on the nanozyme sponge to react completely at a certain temperature. A smartphone was used to take a photo to collect the color signal of the shape memory nanozyme sponge, and the green value was analyzed using ImageJ software. The green value of the unreacted sponge image was recorded as G0, and the green value of the sponge image after the reaction was recorded as G. The ΔG value (ΔG = (G0-G) / G) had a good linear relationship with the hydrogen peroxide concentration.

[0074] Preferably, the concentration of TMB solution is 10-80 mM;

[0075] Preferably, the concentration of the NaAc-HAc buffer solution is 20 mM and the pH is 3.0 to 7.0;

[0076] Preferably, the concentration of hydrogen peroxide ranges from 20 to 1000 μM;

[0077] Preferably, the volume ratio of TMB solution, hydrogen peroxide solution and NaAc-HAc buffer solution is (1-10):(1-10):(280-300).

[0078] Preferably, the reaction temperature is room temperature, and the reaction time is 5 to 30 minutes.

[0079] In some embodiments of the present invention, the step of detecting hydrogen peroxide based on TMB accumulation is:

[0080] (1) dissolving TMB in DMSO to prepare a TMB solution;

[0081] (2) During the detection process, the TMB solution, hydrogen peroxide solutions of different concentrations and NaAc-HAc buffer solution were mixed evenly in proportion and then dripped on the nanozyme sponge, and the "drip-squeeze" operation was repeated until all the reaction solutions were dripped. After complete reaction at a certain temperature, a smartphone was used to take a photo to collect the color signal of the shape memory nanozyme sponge, and the green value was analyzed using ImageJ software. The green value of the unreacted sponge image was recorded as G0, and the green value of the sponge image after the reaction was recorded as G. The ΔG value (ΔG = (G0-G) / G0) has a good linear relationship with the hydrogen peroxide concentration.

[0082] Preferably, the concentration of TMB in DMSO solution is 10-80 mM;

[0083] Preferably, the concentration of the NaAc-HAc buffer solution is 20 mM and the pH is 3.0 to 7.0;

[0084] Preferably, the concentration of hydrogen peroxide ranges from 20 to 1000 μM;

[0085] Preferably, the volume ratio of TMB solution, hydrogen peroxide solution and NaAc-HAc buffer solution is (1-10):(1-10):(280-300).

[0086] Preferably, the "dropping-extrusion" operation is completed within 5 minutes.

[0087] Preferably, the reaction temperature is room temperature, and the reaction time is 5 to 30 minutes.

[0088] In some embodiments of the present invention, based on the single detection of hydrogen peroxide by ABTS, the noble metal nanozyme can catalyze the reaction of ABTS and hydrogen peroxide, so that the concentration of hydrogen peroxide can be displayed by the color intensity on the sponge. The specific steps are:

[0089] ABTS solution was prepared by dissolving ABTS in deionized water;

[0090] During the detection process, ABTS solution, hydrogen peroxide solution of different concentrations and NaAc-HAc buffer solution were mixed evenly in proportion and then dropped on the nanozyme sponge. After complete reaction at a certain temperature, a smartphone was used to take a photo to collect the color signal of the shape memory nanozyme sponge, and the green value was analyzed by ImageJ software. The green value of the unreacted sponge image was recorded as G0, and the green value of the sponge image after the reaction was recorded as G. The ΔG value (ΔG = (G0-G) / G0) has a good linear relationship with the hydrogen peroxide concentration.

[0091] Preferably, the concentration of the ABTS aqueous solution is 10-80 mM;

[0092] Preferably, the concentration of the NaAc-HAc buffer solution is 20 mM and the pH is 2.0 to 5.0;

[0093] Preferably, the concentration of hydrogen peroxide ranges from 10 to 1000 μM;

[0094] Preferably, the usage ratio of ABTS solution, hydrogen peroxide solution and NaAc-HAc buffer solution is (1-10):(1-10):(280-300).

[0095] In some embodiments of the present invention, the steps of reproducibly detecting hydrogen peroxide based on ABTS are:

[0096] ABTS solution was prepared by dissolving ABTS in deionized water;

[0097] During the detection process, the ABTS solution, hydrogen peroxide solutions of different concentrations and NaAc-HAc buffer solution are mixed evenly in proportion and then dripped on the nanozyme sponge. After complete reaction, a smartphone is used to take pictures to collect the color signal of the shape memory nanozyme sponge, and the green value is analyzed by ImageJ software. The green value of the unreacted sponge image is recorded as G0, and the green value of the sponge image after the reaction is recorded as G. The ΔG value (ΔG = (G0-G) / G0) has a good linear relationship with the hydrogen peroxide concentration. By performing the "squeeze-wash" operation, the dye on the sponge can be washed off, thereby restoring the nanozyme sponge to its original state. By cycling the above steps, multiple hydrogen peroxide detections can be achieved using the same sensing device.

[0098] Preferably, the concentration of the ABTS aqueous solution is 10-80 mM;

[0099] Preferably, the concentration of the NaAc-HAc buffer solution is 20 mM and the pH is 2.0 to 5.0;

[0100] Preferably, the concentration of hydrogen peroxide ranges from 10 to 1000 μM;

[0101] Preferably, the usage ratio of ABTS solution, hydrogen peroxide solution and NaAc-HAc buffer solution is (1-10):(1-10):(280-300).

[0102] Preferably, the "dripping-squeezing-cleaning" operation is completed within 5 minutes.

[0103] Preferably, the reaction temperature is room temperature, and the reaction time is 5 to 30 minutes.

[0104] Preferably, the molecular weight of the chitosan described in the present invention is preferably 30 KDa, 50 KDa, 200 KDa and 500 KDa.

[0105] The following is further described in conjunction with specific embodiments.

[0106] Example 1: Preparation of shape memory nanozyme sponge sample 1

[0107] Step 1: Preparation of CS-Pt nanozymes

[0108] First, 10 mg of chitosan was dissolved in 10 mL of 0.4% (v / v) acetic acid aqueous solution; then, 100 μL of chloroplatinic acid solution (H2PtCl6, 20 mM) and 680 μL of deionized water were added to 120 μL of chitosan solution; 100 μL of sodium borohydride (NaBH4, 0.1 M) solution was added dropwise to the above mixed solution and reacted at room temperature for 30 minutes to obtain CS-Pt nanozyme solution.

[0109] Step 2: Preparation of shape memory CS-Pt nanozyme sponge

[0110] First, 125 mg of MBA was dissolved in 16 mL of 6% (v / v) AA aqueous solution, followed by the addition of 7.5 mL of 2% (m / m) chitosan solution; then, the CS-Pt nanozyme solution prepared in step 1 was added to the above mixed solution; after mixing, it was placed at -20 ° C for 10 minutes for freeze polymerization and then taken out, and ammonium persulfate solution and potassium pyrosulfite solution were added dropwise at room temperature. In the final mixed solution, the final concentration of chitosan was 6 mg / mL, the final concentration of CS-Pt nanozyme was 2% (v / v), and the final concentrations of ammonium persulfate and potassium pyrosulfite were 0.8 mg / mL. The above uniform mixed solution was placed at -20 ° C for 15 hours, then taken out, soaked and washed with a large amount of deionized water, and dried to obtain a shape memory nanozyme sponge.

[0111] Example 2: Preparation of shape memory nanozyme sponge sample 2

[0112] Step 1: Preparation of CS-Pt nanozymes

[0113] First, 10 mg of chitosan was dissolved in 10 mL of 0.4% (v / v) acetic acid aqueous solution; then, 100 μL of chloroplatinic acid solution (H2PtCl6, 20 mM) and 700 μL of deionized water were added to 100 μL of chitosan solution; 100 μL of ascorbic acid (0.1 M) solution was added dropwise to the above mixed solution, and the mixture was reacted at room temperature for 30 minutes to obtain a CS-Pt nanozyme solution.

[0114] Step 2: Preparation of shape memory CS-Pt nanozyme sponge

[0115] Same as step 2 of Example 1.

[0116] Example 3: Preparation of shape memory nanozyme sponge sample 3

[0117] Step 1 is the same as step 1 of Example 1.

[0118] Step 2: Preparation of shape memory CS-Pt nanozyme sponge

[0119] First, 125 mg of MBA was dissolved in 16 mL of 6% (v / v) AA aqueous solution, followed by the addition of 7.5 mL of 2% (m / m) chitosan solution; then, the CS-Pt nanozyme solution prepared in step 1 was added to the above mixed solution; after mixing, it was placed at -20 ° C for 10 minutes for freeze polymerization and then taken out, and ammonium persulfate solution and potassium pyrosulfite solution were added dropwise at room temperature. In the final mixed solution, the final concentration of chitosan was 6 mg / mL, the final concentration of CS-Pt nanozyme was 4% (v / v), and the final concentrations of ammonium persulfate and potassium pyrosulfite were 0.8 mg / mL. The above uniform mixed solution was placed at -20 ° C for 15 hours, then taken out, soaked and washed with a large amount of deionized water, and dried to obtain a shape memory nanozyme sponge.

[0120] Example 4: Preparation of shape memory nanozyme sponge sample 4.

[0121] Step 1 is the same as step 1 of Example 1.

[0122] Step 2: Preparation of shape memory CS-Pt nanozyme sponge

[0123] First, 125 mg of MBA was dissolved in 16 mL of 6% (v / v) AA aqueous solution, followed by the addition of 7.5 mL of 2% (m / m) chitosan solution; then, the CS-Pt nanozyme solution prepared in step 1 was added to the above mixed solution; after mixing, it was placed at -20 ° C for 10 minutes for freeze polymerization and then taken out, and ammonium persulfate solution and potassium pyrosulfite solution were added dropwise at room temperature. In the final mixed solution, the final concentration of chitosan was 6 mg / mL, the final concentration of CS-Pt nanozyme was 6% (v / v), and the final concentrations of ammonium persulfate and potassium pyrosulfite were 0.8 mg / mL. The above uniform mixed solution was placed at -20 ° C for 15 hours, then taken out, soaked and washed with a large amount of deionized water, and dried to obtain a shape memory nanozyme sponge.

[0124] Example 5: Preparation of shape memory nanozyme sponge sample 5.

[0125] Step 1: Preparation of CS-Ru nanozyme

[0126] First, 10 mg of chitosan was dissolved in 10 mL of 0.4% (v / v) acetic acid aqueous solution; then, 100 μL of ruthenium chloride solution (RuCl3, 20 mM) and 680 μL of deionized water were added to 120 μL of chitosan solution; 100 μL of sodium borohydride (NaBH4, 0.1 M) solution was added dropwise to the above mixed solution, and the mixture was reacted at room temperature for 30 minutes to obtain a CS-Pt nanozyme solution.

[0127] Step 2: Preparation of shape memory CS-Ru nanozyme sponge

[0128] First, 125 mg of MBA was dissolved in 16 mL of 6% (v / v) AA aqueous solution, followed by the addition of 7.5 mL of 2% (m / m) chitosan solution; then, the CS-Ru nanozyme solution prepared in step 1 was added to the above mixed solution; after mixing, it was placed at -20 ° C for 10 minutes for freeze polymerization and then taken out, and ammonium persulfate solution and potassium pyrosulfite solution were added dropwise at room temperature. In the final mixed solution, the final concentration of chitosan was 6 mg / mL, the final concentration of CS-Ru nanozyme was 2% (v / v), and the final concentrations of ammonium persulfate and potassium pyrosulfite were 0.8 mg / mL. The above uniform mixed solution was placed at -20 ° C for 15 hours, then taken out, soaked and washed with a large amount of deionized water, and dried to obtain a shape memory nanozyme sponge.

[0129] Example 6: Preparation of shape memory nanozyme sponge sample 6

[0130] Step 1: Preparation of CS-Au nanozyme

[0131] First, 10 mg of chitosan was dissolved in 10 mL of 0.4% (v / v) acetic acid aqueous solution; then, 100 μL of chloroauric acid solution (HAuCl4, 20 mM) and 680 μL of deionized water were added to 120 μL of chitosan solution; 100 μL of sodium borohydride (NaBH4, 0.1 M) solution was added dropwise to the above mixed solution and reacted at room temperature for 30 minutes to obtain CS-Au nanozyme solution.

[0132] Step 2: Preparation of shape memory CS-Au nanozyme sponge

[0133] First, 125 mg of MBA was dissolved in 16 mL of 6% (v / v) AA aqueous solution, and then

[0134] 7.5mL 2% (m / m) chitosan solution; then, add the CS-Au nanozyme solution prepared in step 1 to the above mixed solution; after mixing, place it at -20°C for 10 minutes for freeze polymerization and then take it out, and add ammonium persulfate solution and potassium pyrosulfite solution dropwise at room temperature. In the final mixed solution, the final concentration of chitosan is 6mg / mL, the final concentration of CS-Au nanozyme is 2% (v / v), and the final concentrations of ammonium persulfate and potassium pyrosulfite are 0.8mg / mL. The above uniform mixed solution is placed at -20°C for reaction for 15 hours, then taken out, soaked and washed with a large amount of deionized water, and dried to obtain a shape memory nanozyme sponge.

[0135] Example 7: Characterization of shape memory function of shape memory nanozyme sponge

[0136] Example 1 was selected to characterize the shape memory function. Figure 1 It can be seen that the shape of the freeze-dried nanozyme sponge hardly changes after being soaked in water. After the absorbed water is removed by squeezing, the nanozyme sponge becomes an oblate cylinder, and its shape changes to a large extent. When the squeezed nanozyme sponge is soaked in water again, it can quickly return to its original shape. Figure 2 This is the cyclic compression stress-strain curve. It can be seen that when the compression strength is 80%, the nanozyme sponge can still return to its original state after 10 cycles of compression, indicating that the nanozyme sponge has excellent shape memory function, which is beneficial to the application of nanozyme sponge in multiple cumulative detection and repeatable detection.

[0137] Example 8: Testing of shape memory nanozyme sponge for adsorption of dyes with different electrical properties

[0138] Example 1 was selected to test the adsorption of different electrical dyes by the shape memory nanozyme sponge.

[0139] Four positively charged dye molecules, toluidine blue O, crystal violet, methylene blue, and oxTMB, were selected for adsorption test. The steps of enriching positively charged dye molecules in the sponge body by repeatedly performing the "dropping-squeezing" operation are as follows:

[0140] (1) preparing positively charged dye molecules into corresponding aqueous solutions;

[0141] (2) During the enrichment process, the dye solution in step (1) is evenly dripped onto the nanozyme sponge, and after squeezing out excess water, the same dye solution is dripped again. By repeatedly performing the "drip-squeeze" operation, the positively charged dye molecules are enriched in the nanozyme sponge.

[0142] Bromophenol blue, thymol blue, litmus, and oxABTS were selected for elution test. The steps of removing negatively charged dye molecules from the sponge body by repeatedly performing the "dropping-squeezing-washing" operation are as follows:

[0143] (1) preparing negatively charged dye molecules into corresponding aqueous solutions;

[0144] (2) The dye solution in step (1) is evenly dripped onto the nanozyme sponge. During the cleaning process, excess water is removed by squeezing, and then the nanozyme sponge is cleaned with pure water until the nanozyme sponge returns to its initial colorless state. The same operation steps are performed, and the negatively charged dye molecules can be removed from the nanozyme sponge each time during multiple cycles.

[0145] The adsorption effects of the above 8 different electrical dye molecules on the nanozyme sponge are as follows: Figure 3 shown. Figure 4 The zeta potential of the above 8 different electrically charged dye molecules and their respective adsorption efficiency on the nanozyme sponge are demonstrated.

[0146] Example 9: Single Detection of Hydrogen Peroxide Based on TMB

[0147] Example 1 was selected to perform a single detection of hydrogen peroxide based on TMB.

[0148] The reaction temperature was fixed at room temperature, the reaction system was NaAc-HAc buffer solution (pH 5.5), and the reaction time was 10 minutes.

[0149] Take a certain concentration of hydrogen peroxide solution, 40mM TMB solution and NaAc-HAc buffer solution (pH5.5) and mix them evenly to prepare the test solution. The volume ratio of hydrogen peroxide solution, TMB solution and NaAc-HAc buffer solution (pH 5.5) is 6:3:290. 300μL of the mixed solution was dripped on a shape memory CS-Pt nanozyme sponge disc with a diameter of 1cm and a thickness of 0.5cm. After reacting at room temperature for 10 minutes, a smartphone was used to take a photo to collect the color signal of the shape memory nanozyme sponge, and the green value was analyzed using ImageJ software. The green value of the unreacted sponge image is recorded as G0, and the green value of the sponge image after the reaction is recorded as G. The ΔG value (ΔG=(G0-G) / G0) has a good linear relationship with the hydrogen peroxide concentration. The linear equation of the standard curve of the CS-Pt nanozyme sponge for hydrogen peroxide detection based on TMB is ΔG=0.1496+0.1931C H2O2 , the correlation coefficient is 0.9957, such as Figure 5 shown.

[0150] Example 10: TMB-based detection of hydrogen peroxide accumulation

[0151] Example 1 was selected to perform TMB-based hydrogen peroxide accumulation detection.

[0152] The reaction temperature was fixed at room temperature, the reaction system was NaAc-HAc buffer solution (pH 5.5), and the reaction time was 10 minutes.

[0153] Take a certain concentration of hydrogen peroxide solution, 40mM TMB solution and NaAc-HAc buffer solution (pH5.5) and mix them evenly to prepare a series of test solutions. The volume ratio of hydrogen peroxide solution, TMB solution and NaAc-HAc buffer solution (pH 5.5) is 6:3:290. Add 300μL of the above mixed solution on a shape memory CS-Pt nanozyme sponge disc with a diameter of 1cm and a thickness of 0.5cm. After fully squeezing, remove the reaction solution and add new test solution. Repeat the above steps until the test solution is added ( Figure 6 ). The process of dripping-squeezing-dripping the test solution was completed within 1 minute. After reacting at room temperature for 10 minutes, a smartphone was used to take pictures to collect the color signal of the shape memory nanozyme sponge, and the green value was analyzed using ImageJ software. The green value of the unreacted sponge image is recorded as G0, and the green value of the sponge image after the reaction is recorded as G. The total content of hydrogen peroxide in the test solution can be calculated based on the linear relationship between the ΔG value (ΔG = (G0-G) / G0) obtained in Example 7 and the concentration of hydrogen peroxide, divided by the cumulative number of detections, to calculate the content of hydrogen peroxide in the test solution.

[0154] Figure 7 These are color development photos of the CS-Pt nanozyme sponge obtained after 7 repeated dripping-squeezing operations of the test solution containing 100 μM hydrogen peroxide. It can be seen from the figure that the color gradually deepens after 7 repeated dripping-squeezing operations.

[0155] Figure 8 It is based on repeated dripping-extrusion enrichment operations and a comparison of the single-operation detection of hydrogen peroxide samples with the theoretical value (the final concentration of hydrogen peroxide after enrichment is the same as the single hydrogen peroxide concentration). From the data in the figure, it can be seen that the enrichment detection is close to the theoretical value, indicating that its detection results are reliable.

[0156] Example 11: Single Detection of Hydrogen Peroxide Based on ABTS

[0157] Example 1 was selected to perform a single detection of hydrogen peroxide based on ABTS.

[0158] The reaction temperature was fixed at room temperature, the reaction system was NaAc-HAc (pH 3.0), and the reaction time was fixed at 10 minutes.

[0159] Take a certain concentration of hydrogen peroxide solution, 50mM ABTS solution and NaAc-HAc buffer solution (pH 3.0) and mix them evenly to prepare the test solution. The volume ratio of hydrogen peroxide solution, TMB solution and NaAc-HAc buffer solution (pH 3.0) is 6:3:290. 300μL of the mixed solution was dripped on a shape memory CS-Pt nanozyme sponge disc with a diameter of 1cm and a thickness of 0.5cm. After reacting at room temperature for 10 minutes, a smartphone was used to take a photo to collect the color signal of the shape memory nanozyme sponge, and the green value was analyzed using ImageJ software. The green value of the unreacted sponge image is recorded as G0, and the green value of the sponge image after the reaction is recorded as G. According to the good linear relationship between the ΔG value (ΔG=(G0-G) / G0) and the hydrogen peroxide concentration, the linear equation of the standard curve of the CS-Pt nanozyme sponge for hydrogen peroxide detection based on ABTS is ΔG=0.0680+0.0894C H2O2 , the correlation coefficient is 0.9994, such as Fig. 9 shown.

[0160] Example 12: Reusable ABTS-based detection of hydrogen peroxide

[0161] Example 1 was selected to perform reusable detection of hydrogen peroxide based on ABTS.

[0162] The reaction temperature was fixed at room temperature, the reaction system was NaAc-HAc (pH 3.0), and the reaction time was fixed at 10 minutes.

[0163] Take a certain concentration of hydrogen peroxide solution, 50mM ABTTS solution and NaAc-HAc buffer solution (pH 3.0) and mix them evenly to prepare a series of test solutions. The volume ratio of hydrogen peroxide solution, TMB solution and NaAc-HAc buffer solution (pH 3.0) is 6:3:290. 300μL of the mixed solution was dripped on a shape memory CS-Pt nanozyme sponge disc with a diameter of 1cm and a thickness of 0.5cm. After reacting at room temperature for 10 minutes, a smartphone was used to take a photo to collect the color signal of the shape memory nanozyme sponge, and the green value was analyzed using ImageJ software. The green value of the unreacted sponge image is recorded as G0, and the green value of the sponge image after the reaction is recorded as G. The content of hydrogen peroxide in the test solution can be calculated based on the linear relationship between the ΔG value (ΔG=(G0-G) / G0) obtained in Example 9 and the concentration of hydrogen peroxide. Soak the nanozyme sponge after the reaction in deionized water, squeeze and clean it thoroughly to restore the original shape and color of the nanozyme sponge, and then add a new test solution ( Fig.10 ). Each detection was carried out at room temperature for 10 minutes, and the above steps of color signal acquisition and analysis were repeated.

[0164] Fig.11 These are color development photos of the CS-Pt nanozyme sponge obtained after 10 times of washing and repeated dripping of the test solution containing 500 μM hydrogen peroxide. It can be seen from the figure that after 10 times of washing and repeated dripping, the CS-Pt nanozyme sponge still has excellent color development performance.

[0165] Fig.12 This is a color quantitative diagram of repeatable detection of hydrogen peroxide based on the "squeeze-clean" operation. It can be seen from the figure that in each repeated detection cycle, the initial value and the endpoint value remain basically consistent, indicating that the repeated detection effect is good.

[0166] Embodiment 13

[0167] In this embodiment, the mixing volume ratio of chitosan solution, chloroplatinic acid solution, sodium borohydride and deionized water is: 70 μL: 100 μL: 40 μL: 350 μL to obtain CS-Pt nanozyme solution;

[0168] The mixing volume ratio of MBA AA solution, chitosan solution and noble metal nanozyme solution is 18 mL: 10 mL: 0.5 mL, and a mixed solution for preparing noble metal nanozyme sponge is obtained;

[0169] The remaining parts not involved are the same as those in Example 1

[0170] Embodiment 14

[0171] In this embodiment, the mixing volume ratio of chitosan solution, chloroplatinic acid solution, sodium borohydride, sodium borohydride and deionized water is: 40 μL: 10 μL: 30 μL: 400 μL, and CS-Pt nanozyme solution 1 is obtained.

[0172] The mixing volume ratio of MBA AA solution, chitosan solution and noble metal nanozyme solution is 12 mL: 6 mL: 3 mL, and a mixed solution for preparing noble metal nanozyme sponge is obtained;

[0173] The remaining parts not involved are the same as those in Example 1.

[0174] Embodiment 15

[0175] In this embodiment, the mixing volume ratio of chitosan solution, chloroplatinic acid solution, sodium borohydride and deionized water is: 70 μL: 100 μL: 40 μL: 420 μL to obtain CS-Pt nanozyme solution;

[0176] The mixing volume ratio of MBA AA solution, chitosan solution and noble metal nanozyme solution is 12 mL: 10 mL: 5 mL, and a mixed solution for preparing noble metal nanozyme sponge is obtained;

[0177] The remaining parts not involved are the same as those in Example 1

[0178] Example 16

[0179] In this embodiment, the mixing volume ratio of chitosan solution, chloroplatinic acid solution, sodium borohydride, sodium borohydride and deionized water is: 40 μL: 10 μL: 30 μL: 280 μL, and CS-Pt nanozyme solution 1 is obtained.

[0180] The mixing volume ratio of MBA AA solution, chitosan solution and noble metal nanozyme solution is 16 mL: 7.5 mL: 0.1 mL, and a mixed solution for preparing noble metal nanozyme sponge is obtained;

[0181] The remaining parts not involved are the same as those in Example 1.

[0182] Embodiment 17

[0183] In this embodiment, the final concentration of chitosan is 4 mg / mL, the final concentration of the metal nanoenzyme solution is 0.5%, the final concentration of the ammonium persulfate solution and the potassium metabisulfite solution is 0.5 mg / mL, and the rest of the unrelated parts are the same as in Example 1.

[0184] Embodiment 18

[0185] In this embodiment, the final concentration of chitosan is 10 mg / mL, the final concentration of the metal nanoenzyme solution is 10%, the final concentration of the ammonium persulfate solution and the potassium pyrosulfite solution is 2 mg / mL, and the rest of the unrelated parts are the same as in Example 1.

[0186] Embodiment 19

[0187] In this embodiment, the protective agent is polyvinyl pyrrolidone, the noble metal is ruthenium trichloride, the reducing agent is sodium borohydride, and the remaining parts not involved are the same as those in Example 1.

[0188] Embodiment 20

[0189] In this embodiment, the protective agent is glutathione, the noble metal is ruthenium trichloride, the reducing agent is hydroxylamine, and the remaining parts not involved are the same as those in Example 1.

[0190] Embodiment 21

[0191] In this embodiment, the protective agent is sodium citrate, the reducing agent is hydrazine hydrate, and the remaining parts not involved are the same as those in Example 1.

[0192] Embodiment 22

[0193] In this embodiment, the volume ratio of TMB solution, hydrogen peroxide solution and NaAc-HAc buffer solution is 1:1:280, and the rest of the parts not involved are the same as those in Example 7.

[0194] Embodiment 23

[0195] In this embodiment, the volume ratio of TMB solution, hydrogen peroxide solution and NaAc-HAc buffer solution is 10:10:300, and the remaining parts not involved are the same as those in Example 7.

[0196] Embodiment 24

[0197] In this embodiment, the volume ratio of TMB solution, hydrogen peroxide solution and NaAc-HAc buffer solution is 4:2:290, and the rest of the parts not involved are the same as those in Example 7.

[0198] Embodiment 25

[0199] In this embodiment, the volume ratio of TMB solution, hydrogen peroxide solution and NaAc-HAc buffer solution is 1:1:280, and the rest of the parts not involved are the same as those in Example 8.

[0200] Embodiment 26

[0201] In this embodiment, the volume ratio of TMB solution, hydrogen peroxide solution and NaAc-HAc buffer solution is 10:10:300, and the remaining parts not involved are the same as those in Example 8.

[0202] Embodiment 27

[0203] In this embodiment, the volume ratio of TMB solution, hydrogen peroxide solution and NaAc-HAc buffer solution is 8:3:300, and the remaining parts not involved are the same as those in Example 8.

[0204] Embodiment 28

[0205] In this embodiment, the volume ratio of ABTS solution, hydrogen peroxide solution and NaAc-HAc buffer solution is 1:1:280, and the remaining parts are the same as those in Embodiment 9.

[0206] Embodiment 29

[0207] In this embodiment, the volume ratio of ABTS solution, hydrogen peroxide solution and NaAc-HAc buffer solution is 10:10:300, and the remaining parts not involved are the same as those in Example 9.

[0208] Embodiment 30

[0209] In this embodiment, the volume ratio of ABTS solution, hydrogen peroxide solution and NaAc-HAc buffer solution is 5:5:300, and the remaining parts are the same as those in Example 9.

[0210] Embodiment 31

[0211] In this embodiment, the volume ratio of ABTS solution, hydrogen peroxide solution and NaAc-HAc buffer solution is 1:1:280, and the remaining parts not involved are the same as those in Example 10.

[0212] Embodiment 32

[0213] In this embodiment, the volume ratio of ABTS solution, hydrogen peroxide solution and NaAc-HAc buffer solution is 10:10:300, and the remaining parts not involved are the same as those in Example 10.

[0214] Embodiment 33

[0215] In this embodiment, the volume ratio of ABTS solution, hydrogen peroxide solution and NaAc-HAc buffer solution is 6:2:290, and the remaining parts are the same as those in Embodiment 10.

[0216] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A shape memory nanozyme sponge, It is characterized in that The main body is composed of chitosan, poly N,N'-methylenebisacrylamide and polyacrylic acid, and precious metal nanozymes are distributed in the main body.

2. A method for preparing a shape memory nanozyme sponge, It is characterized in that The following steps are involved: Step 1, adding a protective agent solution and a noble metal solution into water, and then adding a reducing agent solution, and obtaining a noble metal nanozyme solution after reaction; The noble metal solution is a noble metal salt solution or a noble metal acid solution; Step 2, the acrylic acid aqueous solution of N,N'-methylenebisacrylamide, the chitosan solution and the noble metal nanozyme solution are mixed and precooled, and then ammonium persulfate solution and potassium pyrosulfite solution are added dropwise after precooling, and the mixture is thawed after freeze polymerization, and dried to obtain a shape memory nanozyme sponge.

3. A method for preparing a shape memory nanozyme sponge according to claim 2, It is characterized in that In step 1, the mixing volume ratio of the protective agent solution, the noble metal solution, the reducing agent solution and water is (4-7): (1-10): (3-5): (28-42).

4. A method for preparing a shape memory nanozyme sponge according to claim 2, It is characterized in that In step 1, the noble metal acid solution is chloroplatinic acid or chloroauric acid, and the noble metal salt solution is ruthenium trichloride.

5. A method for preparing a shape memory nanozyme sponge according to claim 2, It is characterized in that In step 2, the volume ratio of the aqueous solution of N,N'-methylenebisacrylamide in acrylic acid, the chitosan solution and the noble metal nanozyme solution is (120-180): (60-100): (1-50).

6. An application of the shape memory nanozyme sponge according to claim 1, It is characterized in that The shape memory nanozyme sponge is used to adsorb positively charged dye molecules or negatively charged dye molecules; The positively charged dye is toluidine blue O, crystal violet, methylene blue or 3,3',5,5'-tetramethylbenzidine oxidation product; The negatively charged dye includes bromophenol blue, thymol blue, litmus or 2,2'-azinobis-(3-ethylbenzothiazoline-6-sulfonic acid) oxidation product.

7. The use according to claim 6, It is characterized in that The shape memory nanozyme sponge is enriched with positively charged dye molecules on the sponge body by repeatedly performing a "drip-squeeze" operation.

8. The use according to claim 7, It is characterized in that The noble metal nanozyme in the shape memory nanozyme sponge can catalyze the reaction between 3,3',5,5'-tetramethylbenzidine and hydrogen peroxide to generate blue oxTMB, and the blue oxTMB is used to reflect the concentration of hydrogen peroxide.

9. The use according to claim 8, It is characterized in that The reaction of TMB and hydrogen peroxide is as follows: TMB solution, hydrogen peroxide solution and NaAc-HAc buffer solution are mixed evenly and then dripped onto the nanozyme sponge, and the "drip-squeeze" operation is repeated until all the reaction solutions are dripped, and the concentration of hydrogen peroxide is judged by the color on the nanozyme sponge; The volume ratio of TMB, hydrogen peroxide solution, and NaAc-HAc buffer solution is (1-10):(1-10):(280-300).

10. The use according to claim 6, It is characterized in that The shape memory nanozyme sponge is operated by "drip-squeeze-wash" to separate the negatively charged dye molecules originally contained in the sponge body from the sponge body.

11. The use according to claim 10, It is characterized in that The noble metal nanozyme in the shape memory nanozyme sponge can catalyze the reaction between 2,2'-azinobis-(3-ethylbenzothiazoline-6-sulfonic acid) and hydrogen peroxide to generate oxATBS, and the oxATBS is used to reflect the concentration of hydrogen peroxide.

12. The use according to claim 11, It is characterized in that The steps of the reaction of ABTS and hydrogen peroxide are: mixing ABTS solution, hydrogen peroxide solution and NaAc-HAc buffer solution in proportion and then dripping them onto the nanozyme sponge; after the reaction is complete, judging the concentration of hydrogen hydroxide by the color on the nanozyme sponge; squeezing and washing the nanozyme sponge; The steps of dripping, squeezing and washing are repeated, and the nanozyme sponge is used repeatedly; The mixing volume ratio of ABTS solution, hydrogen peroxide solution and NaAc-HAc buffer solution is (1-10):(1-10):(280-300).

Citation Information

Patent Citations

  • Nanometer enzyme-aerogel composite material, detection method of alcohol content in saliva and detection method of glucose content in blood

    CN111334559A

  • Self-adhesive hydrogel based on four-enzyme active nano-enzyme as well as preparation method and application of self-adhesive hydrogel

    CN114470310A

  • Platinum-modified mesoporous gold nano-enzyme as well as preparation method and application thereof

    CN117696050A

Cited By

  • Centrifugal micro-fluidic chip for automatic detection of nano-enzyme test strip and application of centrifugal micro-fluidic chip

    CN120586948A