Thermal insulation coating for inner wall of tobacco curing barn and preparation method of thermal insulation coating

By using a modified thermal insulation coating made of nano-silica powder and other materials on the inner wall of the panel-type tobacco room, combined with a film-forming agent to form a waterproof film, the problem of reduced thermal insulation performance of the tobacco room is solved, achieving efficient insulation and waterproofing effects, and extending the service life longevity and reduced costs.

CN118755285AActive Publication Date: 2024-10-11HANZHONG CO OF SHAANXI TOBACCO CO
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410973441.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-11
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

Plate-type tobacco curing rooms are easily damaged during long-term use, and their thermal insulation performance is reduced, which affects the quality of tobacco leaf baking. The replacement cost is high, and the existing insulation materials are prone to aging in high-temperature and high-humidity environments, making it difficult to effectively maintain heat.

Method used

A thermal insulation coating composed of nano-silica powder, nano-silica sol, dispersant, thickener and film-forming agent is used to form a modified nano-silica sol by adjusting the viscosity and pH value. Combined with a high-speed stirring process, a thermal insulation coating with thermal insulation properties is prepared. A coating with waterproof properties, and a waterproof film is formed through a film-forming agent to improve the stability of the coating.

Benefits of technology

It achieves long-life insulation effect in high-temperature and high-humidity environments, improves the heat utilization rate of the tobacco room, extends the service life of insulation materials, and reduces energy consumption and replacement costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755285A_ABST
    Figure CN118755285A_ABST
Patent Text Reader

Abstract

The invention relates to a thermal insulation coating for the inner wall of a tobacco curing barn and a preparation method thereof, and the thermal insulation coating is prepared by taking nano silica powder and nano silica sol as main raw materials, hexadecyl trimethyl ammonium chloride, carboxyethyl silanetriol sodium salt and hexadecyl trimethyl ammonium bromide as dispersing agents, dimethyl cellulose and polyvinyl alcohol as thickening agents and sodium hydroxide as auxiliary agents. The modified dimethyl siloxane emulsion is used as a film-forming agent, the inner wall of the tobacco curing barn is coated with the nano SiO2 coating, the outer side of the coating is coated with the film-forming agent, a heat preservation coating with the good heat preservation effect and high hydrophobicity is formed, and therefore the heat preservation effect of the tobacco curing barn is improved. The method is easy to operate, the technological process is environmentally friendly, large-scale industrial production can be achieved, the heat preservation coating has the advantages of heat preservation and hydrophobicity, the method can serve in the tobacco curing barn environment with the high temperature and humidity for a long time, heat preservation materials on the inner wall of the tobacco curing barn can be protected, and the tobacco curing barn is not prone to aging and damage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of building thermal insulation coatings, and in particular to a thermal insulation coating for the inner wall of a tobacco flue-curing room and a preparation method thereof. Background Art

[0002] The plate-type flue-curing room is an energy-saving, environmentally friendly, and easy-to-assemble and disassemble tobacco leaf curing room. It is currently the most widely used type of flue-curing room. However, since the flue-curing room needs to be disassembled frequently, it is very easy to cause damage and aging during the long service process. The thermal insulation performance of the flue-curing room is greatly reduced, the utilization rate of curing energy is insufficient, and the quality of tobacco leaf curing is also affected, resulting in income loss for tobacco farmers.

[0003] At present, the plate-type flue-cured tobacco house is mainly composed of a single-layer color steel tile and a steel frame, with a layer of insulation cotton about 1 cm thick installed inside. During the long-term disassembly and service process, the color steel tile of the flue-cured tobacco house is prone to rust and damage, and the internal insulation cotton is also very easy to be scratched, or deformed and damaged in the high temperature and high humidity environment of flue-cured tobacco. This causes the thermal insulation performance of the flue-cured tobacco house to be greatly reduced, affecting the baking quality of tobacco leaves. However, there are economic cost pressures and land policy resistance in the replacement of old flue-cured tobacco houses with new flue-cured tobacco houses. Therefore, if a layer of insulation layer can be applied to the inner wall of a damaged or old flue-cured tobacco house, the thermal insulation performance of the flue-cured tobacco house can be improved, the baking quality of tobacco leaves can be improved, and the income and enthusiasm of tobacco farmers can be increased. However, since the baking process of the flue-cured tobacco house is a high temperature (40℃~80℃) and high humidity (>90%) environment, it is necessary to develop a long-life thermal insulation coating that can both keep warm and have a hydrophobic effect. Summary of the invention

[0004] The invention provides a thermal insulation coating for the inner wall of a flue-curing room and a preparation method thereof. The invention is simple to operate and the process is green and environmentally friendly, and large-scale industrial production can be realized. The thermal insulation coating has the characteristics of both thermal insulation and water repellency, can serve for a long time in a flue-curing room environment with high temperature and humidity, and is not prone to aging and damage.

[0005] To achieve the above object, the technical solution adopted by the present invention includes:

[0006] A thermal insulation coating for the inner wall of a flue-cured tobacco house, wherein the preparation material comprises nano silicon micropowder, nano silica sol, a dispersant, a thickener and a film-forming agent, the viscosity of the nano silica sol is adjusted to 1.5 mPa·s to 2.0 mPa·s, and the pH value of the nano silica sol is adjusted to 8.1 to 9.5 to obtain a modified nano silica sol; then the nano silicon micropowder is added to the modified nano silica sol, and then the dispersant and the thickener are sequentially added to the modified nano silica sol to obtain a thermal insulation coating;

[0007] The thermal insulation coating on the inner wall of the flue-curing tobacco room is composed of a thermal insulation coating layer and a film-forming agent layer.

[0008] Optionally, the particle size of the nano-silicon powder is 5 nm to 10 nm, and the mass ratio of the nano-silicon powder to the nano-silica sol is (0.5 to 1):1.

[0009] Optionally, the dispersant includes hexadecyltrimethylammonium chloride, carboxyethylsilanetriol sodium salt and hexadecyltrimethylammonium bromide, and the mass ratio of the three is 1:1:1.

[0010] Optionally, the total mass ratio of the dispersant to the total mass of the modified silica sol and the silica powder is 1 / (10-20).

[0011] Optionally, the thickener includes dimethyl cellulose and polyvinyl alcohol in a mass ratio of 1:1.

[0012] Optionally, the total mass ratio of the thickener to the total mass of the modified silica sol and the silica powder is 1 / (10-20).

[0013] Optionally, the viscosity of the film-forming agent is 1.9 mPa·s to 3.8 mPa·s, and the pH is 2.8 to 3.5.

[0014] Optionally, the preparation of the film-forming agent includes: firstly stirring polydimethylsiloxane in water evenly, and then adding an emulsifier to emulsify it into a polydimethylsiloxane emulsion.

[0015] Optionally, the thermal insulation coating and the film-forming agent both require high-speed stirring during the preparation process, the speed of the high-speed stirring is 2000r / min to 5000r / min, and the stirring time is 5 to 10min.

[0016] The preparation method of the thermal insulation coating for the inner wall of a flue-curing tobacco room described in any one of the present invention comprises: applying the thermal insulation coating to the inner wall surface of the room to be insulated to form a thermal insulation coating layer, then applying a film-forming agent to the outside of the thermal insulation coating layer to form a film-forming agent layer, and curing in a room temperature environment for 3 to 6 hours.

[0017] The advantages and beneficial effects of the present invention are as follows:

[0018] (1) The main raw materials used in the present invention are widely available and inexpensive, and the raw materials are non-toxic, harmless, and non-flammable and explosive. The preparation and mixing process of the thermal insulation coating is simple, and no toxic or harmful substances are generated during use, which will not pollute the environment or endanger the health of personnel;

[0019] (2) The raw material of the present invention is nano-silica sol containing silicon micropowder. The silicon micropowder can be evenly dispersed in the silica sol by adding a dispersant and a thickener and mixing process, so that the thermal insulation coating can be more uniform;

[0020] (3) The thermal insulation coating of the present invention is mainly composed of nano-SiO2, which has low thermal conductivity and good thermal insulation effect, which is beneficial to improving the heat utilization rate in the tobacco flue-curing room, improving the quality of tobacco leaves after curing, and reducing the energy loss of coal, firewood, etc.;

[0021] (4) The film-forming agent described in the present invention is applied on the inner wall of the tobacco curing room after the silica sol is coated thereon. The purpose is to allow the film-forming agent to produce a cross-linking effect with the nano-SiO2 in the silica sol, so that the coating can be quickly cured and form a waterproof film, which can accelerate the formation of the thermal insulation coating and improve the hydrophobicity of the coating, thereby ensuring that the heat and moisture inside the tobacco curing room are not lost, and ensuring that the thermal insulation coating can serve stably in a high-humidity environment, thereby improving the service life of the thermal insulation material on the wall of the tobacco curing room. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:

[0023] Figure 1 It is a process flow chart of the method of the present invention;

[0024] Figure 2 After the thermal insulation coating prepared in Example 1 is coated on the inner wall of a flue-curing room, the temperature changes of the upper and lower three layers inside the flue-curing room;

[0025] Figure 3 This is a diagram showing the wetting results of the thermal insulation coating prepared in Example 1 with water after it is coated on the thermal insulation material;

[0026] Figure 4 After the thermal insulation coating prepared in Example 2 is coated on the inner wall of the flue-curing room, the temperature changes of the upper and lower three layers inside the flue-curing room;

[0027] Figure 5 This is a diagram showing the wetting results of the thermal insulation coating prepared in Example 2 with water after it is coated on the thermal insulation material;

[0028] Figure 6 This is a diagram showing the wetting results of the thermal insulation coating prepared in Example 3 with water after it is coated on the thermal insulation material. DETAILED DESCRIPTION

[0029] In accordance with the above technical solution, the following are specific embodiments of the present invention. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent changes made on the basis of the technical solution of this application fall within the protection scope of the present invention. The present invention is further described in detail below in conjunction with the embodiments.

[0030] The specific preparation and coating steps of the thermal insulation coating for the inner wall of a flue-cured tobacco house provided by the present invention are as follows:

[0031] (1) The raw materials of the thermal insulation coating mainly include: nano-silicon powder, nano-silicon sol, dispersant, thickener and film-forming agent. Among them, the nano-silicon powder is commercially available conventional nano-silicon powder, and the average particle size of the silicon powder is 5nm to 10nm; the nano-silicon sol is commercially available conventional nano-silicon sol, the concentration of SiO2 in the silica sol is 40%, and the average particle size of SiO2 is 30nm.

[0032] (2) adjusting the viscosity of the nano-silica sol to 1.5 mPa·s to 2.0 mPa·s and adjusting the pH of the nano-silica sol to 8.1 to 9.5 by adding water to obtain a modified nano-silica sol; and adding nano-silica powder to the modified nano-silica sol at a mass ratio of 0.5:1 to 1:1 to the silica sol, and stirring the mixture evenly;

[0033] The viscosity of the modified nano-silica sol is 1.5 mPa·s to 2.0 mPa·s, the pH value of the nano-silica sol is 8.1 to 9.5, the average particle size of the nano-silica powder is 5 nm to 10 nm, and the stirring speed is 2000 r / min to 5000 r / min.

[0034] (3) adding a dispersant to the modified nano-silica sol and continuously stirring; finally, adding a thickener to the nano-silica sol and stirring to prepare a thermal insulation coating;

[0035] Among them, the dispersants and the order of addition are: cetyltrimethylammonium chloride, carboxyethylsilanetriol sodium salt and cetyltrimethylammonium bromide are added in sequence; the mass ratio of each dispersant is 1:1:1; the total mass of the three dispersants is 1 / 10 to 1 / 20 of the total mass ratio of the modified silica sol and the silica micropowder, the stirring speed is 2000r / min to 5000r / min, and the stirring time is 5 to 10min.

[0036] The thickeners and the order of adding are: dimethyl cellulose and polyvinyl alcohol are added in sequence; the mass ratio of each thickener is 1:1; the total mass of the two thickeners is 1 / 10 to 1 / 20 of the total mass ratio of the modified silica sol and the silica powder, the stirring speed is 2000 r / min to 5000 r / min, and the stirring time is 5 to 10 minutes.

[0037] (4) Preparation of a film-forming agent, specifically, first adding polydimethylsiloxane to deionized water and stirring evenly, then adding an emulsifier and stirring at high speed to emulsify the polydimethylsiloxane emulsion;

[0038] The viscosity of the emulsified polydimethylsiloxane emulsion is 1.9 mPa·s to 3.8 mPa·s, and the pH is 2.8 to 3.5.

[0039] (5) Apply the thermal insulation coating described in step 3 to the inner wall surface of the flue-curing room, and then apply the film-forming agent described in step 4 to the inner wall surface of the flue-curing room. After curing at room temperature for 3 to 6 hours, the thermal insulation layer can be cured on the wall surface of the flue-curing room to form a thermal insulation layer.

[0040] Embodiment 1:

[0041] In this embodiment, nano-silicon powder and nano-silica sol are used as main raw materials, hexadecyltrimethylammonium chloride, carboxyethylsilanetriol sodium salt and hexadecyltrimethylammonium bromide are used as dispersants, dimethyl cellulose and polyvinyl alcohol are used as thickeners, and modified dimethylsiloxane is used as film-forming agent. Figure 1 The process shown is for the preparation and coating of thermal insulation coating:

[0042] (1) by adding deionized water, the viscosity of the nano-silica sol is adjusted to 1.5 mPa·s, and the pH value of the nano-silica sol is adjusted to 8.1 to form a modified nano-silica sol; and nano-silica powder with an average diameter of 5 nm is added to the modified nano-silica sol at a mass ratio of 0.5:1, and stirred at a stirring speed of 2000 r / min to be uniform;

[0043] (2) According to the mass ratio of each dispersant being 1:1:1, dispersants hexadecyltrimethylammonium chloride, carboxyethylsilanetriol sodium salt and hexadecyltrimethylammonium bromide are added to the silica sol in sequence, and the total mass of the three dispersants is 1 / 10 of the total mass ratio of the modified silica sol and the silica powder. The silica sol is stirred at a stirring speed of 2000 r / min for 5 min.

[0044] (3) According to the mass ratio of each dispersant being 1:1, the thickeners dimethyl cellulose and polyvinyl alcohol are added to the silica sol in sequence, and the total mass of the two thickeners is 1 / 10 of the total mass ratio of the modified silica sol and the silica powder. The silica sol is stirred at a stirring speed of 2000 r / min for 5 min to prepare a nano-SiO2 thermal insulation coating.

[0045] (4) Polydimethylsiloxane is first added to deionized water and stirred evenly, and then an emulsifier is added and emulsified by high-speed stirring to prepare a polydimethylsiloxane emulsion with a viscosity of 1.9 mPa·s and a pH of 2.8 as a film-forming agent.

[0046] (5) Apply the thermal insulation coating described in step 3 to the inner wall surface of the flue-curing room, and then apply the film-forming agent described in step 4 to the inner wall surface of the flue-curing room. After curing at room temperature for 3 hours, the thermal insulation layer can be cured on the wall surface of the flue-curing room to form a thermal insulation layer.

[0047] After the thermal insulation coating is applied to the tobacco flue-curing room, the actual tobacco leaf curing process is carried out, and a temperature recorder is used to record the complete curing temperature changes of the tobacco, including the temperature of the upper layer (near the roof) and the lower layer (near the ground) inside the tobacco flue-curing room. The results are as follows: Figure 2 As shown in the figure, after the start of baking, the temperature in the flue-curing room gradually rises until 15,000 minutes later, the temperature reaches the high temperature area required for baking. The temperature in this area is mainly distributed between 60℃ and 70℃, and the temperature can last for about 2,000 minutes before the baking ends. In addition, the temperature changes in the upper and lower areas of the flue-curing room show similar change patterns, and the temperature distribution is also similar. The temperature changes inside the flue-curing room are stable, and the flue-curing room has a good thermal insulation effect. This shows that the flue-curing room has a good thermal insulation effect after being coated with thermal insulation paint.

[0048] The water wettability test method is used to measure the hydrophobic effect of the coated insulation board material. The process is: drop water onto the surface of the coated insulation material and measure the contact angle of water using a contact angle meter (model: JC2000DM). The results are as follows: Figure 3 As shown in the figure, it can be seen that the water droplets do not spread on the surface of the insulation material, and form a relatively obvious arc shape with an angle of 118°, which shows that the insulation board material with coating has a strong hydrophobic effect, which helps to extend the service life of the insulation material in a high humidity environment.

[0049] Embodiment 2:

[0050] In this embodiment, nano-silicon powder and nano-silica sol are used as main raw materials, hexadecyltrimethylammonium chloride, carboxyethylsilanetriol sodium salt and hexadecyltrimethylammonium bromide are used as dispersants, dimethyl cellulose and polyvinyl alcohol are used as thickeners, and modified dimethylsiloxane is used as film-forming agent. Figure 1 The process shown is for the preparation and coating of thermal insulation coating:

[0051] (1) adjusting the viscosity of the nano-silica sol to 2.0 mPa·s and the pH of the nano-silica sol to 9.5 by adding deionized water to obtain a modified nano-silica sol; adding nano-silica powder with an average diameter of 5 nm to the modified nano-silica sol in a mass ratio of 1:1, and stirring at a stirring speed of 5000 r / min to obtain a uniform mixture;

[0052] (2) According to the mass ratio of each dispersant being 1:1:1, dispersants hexadecyltrimethylammonium chloride, carboxyethylsilanetriol sodium salt and hexadecyltrimethylammonium bromide are added to the silica sol in sequence, and the total mass of the three dispersants is 1 / 20 of the total mass ratio of the modified silica sol and the silica powder. The silica sol is stirred at a stirring speed of 5000 r / min for 10 min.

[0053] (3) According to the mass ratio of each dispersant being 1:1, the thickeners dimethyl cellulose and polyvinyl alcohol are added to the silica sol in sequence, and the total mass of the two thickeners is 1 / 20 of the total mass ratio of the modified silica sol and the silica powder. The silica sol is stirred at a stirring speed of 5000 r / min for 10 min to prepare a nano-SiO2 thermal insulation coating.

[0054] (4) Polydimethylsiloxane is first added to deionized water and stirred evenly, and then an emulsifier is added and emulsified by high-speed stirring to prepare a polydimethylsiloxane emulsion with a viscosity of 3.8 mPa·s and a pH of 3.5 as a film-forming agent.

[0055] (5) Apply the thermal insulation coating described in step 3 to the inner wall surface of the flue-curing room, and then apply the film-forming agent described in step 4 to the inner wall surface of the flue-curing room. After curing at room temperature for 6 hours, the thermal insulation layer can be cured on the wall surface of the flue-curing room to form a thermal insulation layer.

[0056] After the thermal insulation coating is applied to the tobacco flue-curing room, the actual tobacco leaf curing process is carried out, and a temperature recorder is used to record the complete curing temperature changes of the tobacco, including the temperature of the upper layer (near the roof) and the lower layer (near the ground) inside the tobacco flue-curing room. The results are as follows: Figure 4 As shown in the figure, the time of tobacco curing is not fixed. Figure 2 and Figure 4 Compared with the above, their horizontal coordinates are not exactly the same. As can be seen from the figure, after the start of baking, the temperature in the flue-curing room gradually rises until 12000 minutes later, the temperature reaches the high temperature area required for baking. The temperature in this area is mainly distributed between 60℃ and 70℃, and the temperature can last for about 2000 minutes before the baking ends. In addition, the temperature changes in the upper and lower areas of the flue-curing room show similar change patterns, and the temperature distribution is also similar. The temperature changes inside the flue-curing room are stable, and the flue-curing room has a good thermal insulation effect. This shows that the flue-curing room has a good thermal insulation effect after being coated with thermal insulation paint.

[0057] The water wettability test method is used to measure the hydrophobic effect of the coated insulation board material. The process is: drop water onto the surface of the coated insulation material and measure the contact angle of water using a contact angle meter (model: JC2000DM). The results are as follows: Figure 5 As shown in the figure, it can be seen that the water droplets do not spread on the surface of the insulation material, and form a relatively obvious arc shape with an angle of 115°, which shows that the insulation board material with coating has a strong hydrophobic effect, which helps to extend the service life of the insulation material in a high humidity environment.

[0058] Embodiment 3:

[0059] In this embodiment, nano-silicon powder and nano-silica sol are used as main raw materials, hexadecyltrimethylammonium chloride, carboxyethylsilanetriol sodium salt and hexadecyltrimethylammonium bromide are used as dispersants, dimethyl cellulose and polyvinyl alcohol are used as thickeners, and modified dimethylsiloxane is used as film-forming agent. Figure 1 The process shown is for the preparation and coating of thermal insulation coating:

[0060] (1) adjusting the viscosity of the nano-silica sol to 2.5 mPa·s and the pH value of the nano-silica sol to 9.7 by adding deionized water to obtain a modified nano-silica sol; adding nano-silica powder with an average diameter of 5 nm to the modified nano-silica sol in a mass ratio of 1:1, and stirring at a stirring speed of 5000 r / min to obtain a uniform mixture;

[0061] (2) According to the mass ratio of each dispersant being 1:1:1, dispersants hexadecyltrimethylammonium chloride, carboxyethylsilanetriol sodium salt and hexadecyltrimethylammonium bromide are added to the silica sol in sequence, and the total mass of the three dispersants is 1 / 20 of the total mass ratio of the modified silica sol and the silica powder. The silica sol is stirred at a stirring speed of 5000 r / min for 10 min.

[0062] (3) According to the mass ratio of each dispersant being 1:1, the thickeners dimethyl cellulose and polyvinyl alcohol are added to the silica sol in sequence, and the total mass of the two thickeners is 1 / 20 of the total mass ratio of the modified silica sol and the silica powder. The silica sol is stirred at a stirring speed of 5000 r / min for 10 min to prepare a nano-SiO2 thermal insulation coating.

[0063] (4) Polydimethylsiloxane is first added to deionized water and stirred evenly, and then an emulsifier is added and emulsified by high-speed stirring to prepare a polydimethylsiloxane emulsion with a viscosity of 3.8 mPa·s and a pH of 3.5 as a film-forming agent.

[0064] (5) Apply the thermal insulation coating described in step 3 to the inner wall surface of the flue-curing room, and then apply the film-forming agent described in step 4 to the inner wall surface of the flue-curing room. After curing at room temperature for 6 hours, the thermal insulation layer can be cured on the wall surface of the flue-curing room to form a thermal insulation layer.

[0065] The water wettability test method is used to measure the hydrophobic effect of the coated insulation board material. The process is: drop water onto the surface of the coated insulation material and measure the contact angle of water using a contact angle meter (model: JC2000DM). The results are as follows: Figure 6As shown in the figure, it can be seen that the water droplets do not spread on the surface of the thermal insulation material, and form a relatively obvious arc shape with an angle of only 80°, indicating that the thermal insulation material has a poor hydrophobic effect after coating. In the actual high-humidity environment, the life of the thermal insulation material is easily reduced due to water intrusion. In addition, this also shows that changing the viscosity and pH of the modified nano-silica sol is not within the parameter range of the present invention, which will have an adverse effect on film formation, thereby affecting the hydrophobicity of the prepared coating.

[0066] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A thermal insulation coating for the inner wall of a tobacco flue-curing room, It is characterized in that The preparation material consists of nano silicon powder, nano silica sol, dispersant, thickener and film-forming agent. The viscosity of the nano-silica sol is adjusted to 1.5 mPa·s to 2.0 mPa·s, and the pH value of the nano-silica sol is adjusted to 8.1 to 9.5 to obtain a modified nano-silica sol; Then, nano silicon powder is added into the modified nano silica sol, and then a dispersant and a thickener are sequentially added into the modified nano silica sol to obtain a thermal insulation coating; The thermal insulation coating on the inner wall of the flue-curing tobacco room is composed of a thermal insulation coating layer and a film-forming agent layer.

2. The thermal insulation coating for the inner wall of a flue-cured tobacco room according to claim 1, It is characterized in that The particle size of the nano silicon powder is 5nm-10nm, and the mass ratio of the nano silicon powder to the nano silica sol is (0.5-1):

1.

3. The thermal insulation coating for the inner wall of a flue-cured tobacco room according to claim 1 or 2, It is characterized in that The dispersant comprises hexadecyltrimethylammonium chloride, carboxyethylsilanetriol sodium salt and hexadecyltrimethylammonium bromide, and the mass ratio of the three is 1:1:

1.

4. The thermal insulation coating for the inner wall of a flue-cured tobacco room according to claim 3, It is characterized in that The total mass ratio of the dispersant to the modified silica sol and the silica powder is 1 / (10-20).

5. The thermal insulation coating for the inner wall of a flue-cured tobacco room according to claim 1 or 2, It is characterized in that The thickener comprises dimethyl cellulose and polyvinyl alcohol, and the mass ratio of the two is 1:

1.

6. The thermal insulation coating for the inner wall of a flue-cured tobacco room according to claim 5, It is characterized in that The total mass ratio of the thickener to the total mass of the modified silica sol and the silica powder is 1 / (10-20).

7. The thermal insulation coating for the inner wall of a flue-cured tobacco room according to claim 1 or 2, It is characterized in that The viscosity of the film-forming agent is 1.9 mPa·s to 3.8 mPa·s, and the pH value is 2.8 to 3.

5.

8. The thermal insulation coating for the inner wall of a flue-cured tobacco room according to claim 7, It is characterized in that The preparation of the film-forming agent comprises: firstly stirring polydimethylsiloxane in water evenly, and then adding an emulsifier to emulsify the polydimethylsiloxane emulsion.

9. The thermal insulation coating for the inner wall of a flue-cured tobacco room according to claim 1 or 2, It is characterized in that The thermal insulation coating and the film-forming agent both require high-speed stirring during the preparation process, the speed of the high-speed stirring is 2000r / min to 5000r / min, and the stirring time is 5 to 10min.

10. The method for preparing the thermal insulation coating for the inner wall of a flue-cured tobacco house according to any one of claims 1 to 9, It is characterized in that include: The thermal insulation coating is applied to the inner wall surface of the room to be insulated to form a thermal insulation coating layer, and then a film-forming agent is applied to the outside of the thermal insulation coating layer to form a film-forming agent layer, and then the room temperature environment is maintained for 3 to 6 hours.

Citation Information

Patent Citations

  • Hydrophobic hydrocarbon coatings

    CN103596701A

  • Preparation method of moisture-proof heat-resistant toughened automotive hemming glue

    CN108707438A

  • Oil-dirt-resistance smokeless odorless water-based inorganic nano-ceramic kitchenware coating and preparation method thereof

    CN109401370A

  • Waterborne high-temperature-resistant non-sticking paint and preparation method thereof

    CN109749622A

  • Inner container easy to clean, production method thereof and cooking utensil

    CN113384154A