Low-solid-phase mixed silver filled light-cured printing conductive ink and preparation method and printing method thereof
Through light-curing printing conductive ink with low solid filling mixed silver, combined with ultraviolet light and heat treatment, nano-silver particles are formed, which solves the problem of difficulty in balancing high precision and conductivity in light-curing technology, and achieves high-precision and excellent conductivity circuit printing. , suitable for multi-functional electronic components.
Patent Information
- Application Number
- CN202411064926.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-08-05
AI Technical Summary
Existing light-curing technology is difficult to achieve high-precision and excellent conductivity circuit printing at the same time. It is limited by the refractive index difference and large extinction coefficient of metal fillers and resin slurries, resulting in limited conductivity.
Using light-curing printing conductive ink with low solid filling mixed silver, through the combination of prepolymer, active monomer, photoinitiator, dispersant, silver powder and silver precursor, combined with ultraviolet light and heat treatment, nano silver particles are formed to achieve Conductive paths reduce the use of solid fillers, reduce light scattering effects, and improve mechanical strength and bonding strength.
It achieves high-precision and excellent conductivity circuit printing under low solid state conditions, reduces line width mis-curing, and improves the mechanical strength and conductive performance of the conductive film layer. It is suitable for multi-functional electronic components and does not require a high-temperature sintering process.
Smart Images

Figure CN118755312A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a photocurable printing conductive ink and a preparation method and a printing method thereof. Background Art
[0002] With the development and transformation of additive manufacturing technology, it has shown potential for application in the field of electronic component manufacturing because it can realize customization and the design and manufacture of complex structures. Photocuring technology is an emerging method of forming circuits. Compared with inkjet printing, direct writing or screen printing, it not only has higher printing accuracy, but also as a non-contact printing method, it can achieve complex forming on non-planar substrate surfaces. Therefore, this method can not only improve the performance and quality of electronic components, but also realize the multifunctionality of components and broaden the scope of application.
[0003] However, unlike ceramic materials, the refractive index difference between metal fillers and resin slurries is generally large, and the extinction coefficient is large, and the solid content of fillers is a prerequisite for preparing high conductivity. Therefore, the use of photocuring technology to print high-precision and excellent conductive circuits is greatly limited. Summary of the invention
[0004] The present invention aims to solve the problem that the existing photocuring technology printing cannot simultaneously print circuits with high precision and excellent conductivity, and further provides a photocuring printing conductive ink filled with low solid phase mixed silver and a preparation method and a printing method thereof.
[0005] A low-solid phase filled mixed silver light-curing printing conductive ink, which is prepared by weight from 10 to 30 parts of prepolymer, 20 to 30 parts of active monomer, 0.5 to 4 parts of photoinitiator, 1 to 5 parts of dispersant, 20 to 30 parts of silver powder and 5 to 20 parts of silver precursor;
[0006] The photoinitiator is ethyl 2,4,6-trimethylbenzoylphenylphosphonate;
[0007] The silver powder is flaky silver powder with a particle size of 0.1 μm to 10 μm;
[0008] The silver precursor is silver trifluoroacetate.
[0009] A method for preparing a low solid phase filled mixed silver light-curable printing conductive ink, which is carried out according to the following steps:
[0010] 1. Weigh 10 to 30 parts of prepolymer, 20 to 30 parts of active monomer, 0.5 to 4 parts of photoinitiator, 1 to 5 parts of dispersant, 20 to 30 parts of silver powder and 5 to 20 parts of silver precursor by mass;
[0011] 2. The weighed prepolymer, active monomer and silver precursor are mixed and dissolved to form a uniform solution, and then a dispersant and silver powder are added and mixed evenly, and finally a photoinitiator is added and vacuum degassed to obtain a light-curable printing conductive ink filled with low solid phase mixed silver.
[0012] A method for printing a low solid phase filled mixed silver light-curable conductive ink, which is carried out according to the following steps:
[0013] 1. Apply or spray the low solid phase filled mixed silver light-curable printing conductive ink on a flat or curved substrate;
[0014] 2. Use modeling software to design the circuit, and perform UV light path scanning and curing according to the preset printing pattern under the conditions of UV light wavelength of 350nm to 420nm, power of 5mW to 10mW and scanning speed of 5mm / s to 30mm / s;
[0015] 3. Clean the ink outside the pattern with an isopropyl alcohol solution, and then perform light treatment or heat treatment to complete the printing method of the light-curing conductive ink filled with low solid phase mixed silver.
[0016] The beneficial effects of the present invention are:
[0017] The present invention uses a silver filler with a lower solid content (20 to 30 parts of silver powder) combined with a precursor silver that can be dissolved in a photosensitive material system. Not only can the use of solid fillers be reduced to reduce the scattering effect of light to cause serious line width miscuring, but also, since the selected precursor silver can be dissolved in photosensitive materials, the low solid filler is more conducive to rapid curing under low-dose ultraviolet exposure, so that the conductive film layer has excellent mechanical strength and bonding force. Secondly, the precursor silver can use light and heat to achieve the reduction of silver ions after curing, and nano silver particles are formed between the flaky elemental silver, so that the conductive path can still be achieved under low solid fillers, and the process of high-temperature sintering is not required, which is conducive to the application of conductive ink in more electronic components and devices, and has high precision and excellent conductive circuit printing. In addition, the present invention adjusts the ratio of prepolymer to active monomer and fills with low solid content, so that the prepared photocurable conductive ink has a lower viscosity (0.5Pa·s~1Pa·s), which is conducive to the slurry to achieve uniform coating thickness on a flat or curved substrate by coating or spraying. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a SEM image of the conductive pattern printed on the substrate in step three of the printing method in Example 1;
[0019] Figure 2The SEM images of the conductive pattern before and after the heat treatment in step 2 and step 3 in the printing method of Example 3, a is after the heat treatment, and b is before the heat treatment;
[0020] Figure 3 This is a physical picture of the conductive pattern printed on the curved substrate in step three of the printing method of Example 5. DETAILED DESCRIPTION
[0021] Specific implementation method 1: This implementation method is a low-solid phase filled mixed silver light-curable printing conductive ink, which is prepared by weight from 10 to 30 parts of prepolymer, 20 to 30 parts of active monomer, 0.5 to 4 parts of photoinitiator, 1 to 5 parts of dispersant, 20 to 30 parts of silver powder and 5 to 20 parts of silver precursor;
[0022] The photoinitiator is ethyl 2,4,6-trimethylbenzoylphenylphosphonate;
[0023] The silver powder is flaky silver powder with a particle size of 0.1 μm to 10 μm;
[0024] The silver precursor is silver trifluoroacetate.
[0025] The beneficial effects of this embodiment are:
[0026] This embodiment uses a silver filler with a lower solid content (20 to 30 parts of silver powder) combined with a precursor silver that can be dissolved in a photosensitive material system. It can not only reduce the use of solid fillers and reduce the scattering effect of light to cause serious line width miscuring, but also, because the selected precursor silver can be dissolved in photosensitive materials, low solid fillers are more conducive to rapid curing under low-dose ultraviolet exposure, so that the conductive film layer has excellent mechanical strength and bonding force. Secondly, the precursor silver can use light and heat to achieve silver ion reduction after curing, and nano silver particles are formed between the flaky elemental silver, so that the conductive path can still be achieved under low solid fillers. The process of high-temperature sintering is not required, which is conducive to the application of conductive ink in more electronic components and devices, and has high precision and excellent conductive circuit printing. In addition, this embodiment adjusts the ratio of prepolymer to active monomer and fills with low solid content, so that the prepared photocurable conductive ink has a lower viscosity (0.5Pa·s~1Pa·s), which is conducive to the slurry to achieve uniform coating thickness on a flat or curved substrate by coating or spraying.
[0027] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the prepolymer is epoxy acrylate or polyurethane acrylate. Other aspects are the same as specific implementation method 1.
[0028] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the active monomer is isobornyl acrylate, 1,6-hexanediol diacrylate or polyethylene glycol diacrylate. Other aspects are the same as specific implementation method 1 or 2.
[0029] Specific embodiment 4: This embodiment is different from specific embodiments 1 to 3 in that the dispersant is BYK110 or polyethylene glycol 200. Other aspects are the same as specific embodiments 1 to 3.
[0030] Specific implementation method 5: This implementation method is a method for preparing a low solid phase filled mixed silver light-curable printing conductive ink, which is carried out according to the following steps:
[0031] 1. Weigh 10 to 30 parts of prepolymer, 20 to 30 parts of active monomer, 0.5 to 4 parts of photoinitiator, 1 to 5 parts of dispersant, 20 to 30 parts of silver powder and 5 to 20 parts of silver precursor by mass;
[0032] 2. The weighed prepolymer, active monomer and silver precursor are mixed and dissolved to form a uniform solution, and then a dispersant and silver powder are added and mixed evenly, and finally a photoinitiator is added and vacuum degassed to obtain a light-curable printing conductive ink filled with low solid phase mixed silver.
[0033] Specific implementation method 6: This implementation method is a method for printing a low solid phase filled mixed silver light-curable printing conductive ink, which is carried out according to the following steps:
[0034] 1. Apply or spray the low solid phase filled mixed silver light-curable printing conductive ink on a flat or curved substrate;
[0035] 2. Use modeling software to design the circuit, and perform UV light path scanning and curing according to the preset printing pattern under the conditions of UV light wavelength of 350nm to 420nm, power of 5mW to 10mW and scanning speed of 5mm / s to 30mm / s;
[0036] 3. Clean the ink outside the pattern with an isopropyl alcohol solution, and then perform light treatment or heat treatment to complete the printing method of the light-curing conductive ink filled with low solid phase mixed silver.
[0037] Specific implementation example 7: This implementation example is different from specific implementation example 6 in that the substrate described in step 1 is a glass substrate, a ceramic substrate or a plastic substrate. The rest is the same as specific implementation example 6.
[0038] Specific embodiment eight: This embodiment differs from specific embodiment six or seven in that: in step one, the light-curable printing conductive ink filled with low solid phase mixed silver is coated or sprayed on a flat or curved substrate at a coating thickness of 20 μm to 100 μm. The rest is the same as specific embodiment six or seven.
[0039] Specific embodiment 9: This embodiment is different from any one of specific embodiments 6 to 8 in that the mass percentage of the isopropanol solution in step 3 is 30% to 60%. The rest is the same as specific embodiments 6 to 8.
[0040] Specific embodiment 10: This embodiment differs from any one of specific embodiments 6 to 9 in that the light treatment described in step 3 is specifically performed at a wavelength of 350nm to 420nm and a power density of 20mW / cm 2 ~80mW / cm 2 The heat treatment in step 3 is specifically performed at a temperature of 100° C. to 200° C. for 30 min to 60 min. The rest is the same as the sixth to ninth embodiments.
[0041] The following examples are used to verify the beneficial effects of the present invention:
[0042] Embodiment 1:
[0043] A low solid phase filled mixed silver light-curable printing conductive ink, which is prepared by weight from 22 parts of prepolymer, 24 parts of active monomer, 2 parts of photoinitiator, 2 parts of dispersant, 20 parts of silver powder and 20 parts of silver precursor;
[0044] The photoinitiator is ethyl 2,4,6-trimethylbenzoylphenylphosphonate;
[0045] The silver powder is flaky silver powder with an average particle size of 1 μm;
[0046] The silver precursor is silver trifluoroacetate.
[0047] The prepolymer is polyurethane acrylate.
[0048] The active monomer is polyethylene glycol diacrylate.
[0049] The dispersant is BYK110.
[0050] The method for preparing the above-mentioned low solid phase filled mixed silver light-curable printing conductive ink is carried out according to the following steps:
[0051] 1. Weigh 22 parts of prepolymer, 24 parts of active monomer, 2 parts of photoinitiator, 2 parts of dispersant, 20 parts of silver powder and 20 parts of silver precursor according to mass proportion;
[0052] 2. The weighed prepolymer, active monomer and silver precursor are mixed and dissolved to form a uniform solution, and then a dispersant and silver powder are added and mixed evenly, and finally a photoinitiator is added and vacuum degassed to obtain a light-curable printing conductive ink filled with low solid phase mixed silver.
[0053] The above-mentioned method for printing a light-curable conductive ink filled with mixed silver with low solid phase is carried out according to the following steps:
[0054] 1. Coating a low solid phase filled mixed silver light-curable printing conductive ink on a flat substrate at a coating speed of 10 mm / s and a coating thickness of 20 μm;
[0055] 2. Use modeling software to design the circuit, and perform UV light path scanning and curing according to the preset printing pattern under the conditions of UV light wavelength of 405nm, power of 10mW and scanning speed of 20mm / s;
[0056] 3. Use 50% isopropyl alcohol solution to clean the ink outside the pattern, and then use a wavelength of 405nm and a power density of 40mW / cm 2 Under the conditions of , the substrate was treated with light for 10 minutes to obtain a conductive pattern printed on the substrate.
[0057] The substrate described in step 1 is an alumina ceramic substrate.
[0058] Embodiment 2: This embodiment is different from Embodiment 1 in that: printing method: the scanning speed in step 2 is 10 mm / s; in step 3, the light treatment is replaced by heat treatment, and the heat treatment is specifically performed at a temperature of 120° C. for 30 minutes. The rest is the same as Embodiment 1.
[0059] Embodiment 3: This embodiment is different from Embodiment 1 in that: printing method: in step 1, the coating thickness is 40 μm; in step 2, the scanning speed is 10 mm / s; in step 3, the light treatment is replaced by heat treatment, and the heat treatment is specifically performed at a temperature of 120° C. for 30 minutes. The rest is the same as in Embodiment 1.
[0060] Example 4: This example is different from Example 1 in that: a low solid phase filled mixed silver light-curable printing conductive ink is prepared by weight from 24 parts of prepolymer, 30 parts of active monomer, 3 parts of photoinitiator, 3 parts of dispersant, 30 parts of silver powder and 10 parts of silver precursor;
[0061] The silver powder is flaky silver powder with an average particle size of 0.5 μm;
[0062] The active monomer is 1,6-hexanediol diacrylate;
[0063] Printing method: the power in step 2 is 20 mW; in step 3, the light treatment is replaced by heat treatment, and the heat treatment is specifically performed at a temperature of 120° C. for 60 minutes. The rest is the same as in Example 1.
[0064] Embodiment 5: This embodiment is different from Embodiment 1 in that: in step 1, the flat substrate is replaced by a curved substrate; the substrate is an acrylic plastic substrate with a curvature radius of 2.5 cm. Others are the same as Embodiment 1.
[0065] Comparative Experiment 1: The difference between this embodiment and the first embodiment is: Printing method: the light treatment in step 3 is eliminated. The rest is the same as the first embodiment.
[0066] Comparative Experiment 2: The difference between this embodiment and the third embodiment is that the silver precursor is not used in the low solid phase filled mixed silver light curing printing conductive ink, the silver powder is 29.8 parts, and the heat treatment in step 3 is omitted. The rest is the same as the third embodiment.
[0067] After calculation: m(C2F2O2Ag) / m(Ag)=221 / 108, 20 parts of silver trifluoroacetate can theoretically be reduced to 9.8 parts of elemental silver, so the silver content in comparative experiment 2 is the same as that in embodiment 3.
[0068] Test method:
[0069] 1. Viscosity test: The light-curable printed conductive ink filled with low solid phase mixed silver was tested at room temperature using the HAAKE rheometer parallel plate method, with a plate diameter of 30 mm and a plate gap of 0.45 mm.
[0070] 2. Polymerization speed: The modulus change of the light-cured conductive ink filled with low solid phase mixed silver is measured in real time under continuous UV irradiation. The maximum value of the differential of the modulus with respect to time is used to evaluate the polymerization rate. The wavelength of the UV curing unit is 405nm, and the irradiation intensity is 1% of the peak radiation intensity, which is 10300mW / cm 2 .
[0071] 3. Line width resolution test: Use a high-definition optical microscope to measure the conductive pattern printed on the substrate.
[0072] 4. Sample morphology test after photothermal treatment: The conductive pattern printed on the substrate was observed using a scanning electron microscope.
[0073] 5. Resistance: Connect the two ends of the conductive pattern printed on the substrate to the red and black test leads of the multimeter to test its resistance value.
[0074] 6. Conductivity: Print 6 square conductive films of 1 cm×1 cm according to the method in the embodiment, test with a four-probe resistance meter, and take the average value.
[0075] 7. Pencil hardness: Use pencils of different hardness to scratch the surface of the conductive pattern printed on the substrate, and evaluate its wear resistance by observing the scratches.
[0076] The test results are shown in Table 1:
[0077] Table 1
[0078]
[0079] In the table, “——” represents the establishment of no conductive path, that is, the non-conductive state; the specific meaning of the error curing width in the table is that the printing line width is designed to be 40μm, and the line width value of the actual curing test is the difference between the designed line width.
[0080] It can be seen from the test results in Table 1 that the low solid phase filled mixed silver light-curable printing conductive ink not only has high polymerization rate and printing line width accuracy, but also has excellent electrical conductivity and pencil hardness, and can realize the printing and molding of precision conductive layers on flat or curved substrates. Comparison of Examples 1 and 2 with Comparative Experiment 1 shows that the light-curable conductive ink can establish a conductive network after illumination or low-temperature heat treatment, so that the conductive film layer has good electrical properties, which can be applied to the circuit preparation and connection of various high-precision electronic components. Comparison of Example 3 with Comparative Experiment 2 shows that the use of micron- or submicron-level flaky silver powder and silver trifluoroacetate as mixed silver sources can generate nanosilver between flaky silver particles after low-temperature heat treatment to produce an effective conductive path and obtain excellent electrical properties, while pure flaky silver particles are non-conductive because they cannot achieve overlap between particles; in addition, by comparing Example 3 with Comparative Experiment 2, it can be seen that the filling of more flaky silver particles will reduce the polymerization rate of the conductive ink and the pencil hardness of the conductive film layer.
[0081] Figure 1 This is a SEM image of the conductive pattern printed on the substrate in step 3 of the printing method of Example 1. As can be seen from the figure, after light treatment, silver trifluoroacetate has been reduced to nanosilver particles and filled between the flaky silver particles, which enables the flaky particles to establish a conductive path connection through the nanosilver particles, greatly reducing the tunneling resistance.
[0082] Figure 2 The SEM images of the conductive pattern before and after the heat treatment in step 2 and step 3 of the printing method of Example 3 are shown in Figure 1. a is after the heat treatment, and b is before the heat treatment. It can be seen from the figure that after the heat treatment, the silver trifluoroacetate is thermally reduced to nano silver particles and filled between the micron silver flakes, while the conductive pattern layer that has not been heat treated does not produce nano silver, and the flaky silver particles are completely filled with polymer, which hinders the formation of the conductive path.
[0083] Figure 3This is a physical picture of the conductive pattern printed on the curved substrate in step 3 of the printing method of Example 5. As can be seen from the figure, the light-curing printing conductive ink filled with mixed silver in Example 5 can achieve good printing on the curved substrate under the scanning of ultraviolet light. After cleaning, the conductive pattern structure is clear and maintains good adhesion to the substrate without falling off.
Claims
1. A low solid phase filled mixed silver light-curable printing conductive ink, Features It is prepared from 10 to 30 parts of prepolymer, 20 to 30 parts of active monomer, 0.5 to 4 parts of photoinitiator, 1 to 5 parts of dispersant, 20 to 30 parts of silver powder and 5 to 20 parts of silver precursor in parts by mass. The photoinitiator is ethyl 2,4,6-trimethylbenzoylphenylphosphonate; The silver powder is flaky silver powder with a particle size of 0.1 μm to 10 μm; The silver precursor is silver trifluoroacetate.
2. A light-curable printing conductive ink filled with mixed silver with low solid phase according to claim 1, Features The prepolymer is epoxy acrylate or polyurethane acrylate.
3. A light-curable printing conductive ink filled with mixed silver with low solid phase according to claim 1, Features The active monomer is isobornyl acrylate, 1,6-hexanediol diacrylate or polyethylene glycol diacrylate.
4. A light-curable printing conductive ink filled with mixed silver with low solid phase according to claim 1, Features The dispersant is BYK110 or polyethylene glycol 200.
5. A method for preparing a light-curable printing conductive ink filled with mixed silver at low solid phase as claimed in claim 1, Features It is carried out in the following steps:
1. Weigh 10 to 30 parts of prepolymer, 20 to 30 parts of active monomer, 0.5 to 4 parts of photoinitiator, 1 to 5 parts of dispersant, 20 to 30 parts of silver powder and 5 to 20 parts of silver precursor by mass; 2. The weighed prepolymer, active monomer and silver precursor are mixed and dissolved to form a uniform solution, and then a dispersant and silver powder are added and mixed evenly, and finally a photoinitiator is added and vacuum degassed to obtain a light-curable printing conductive ink filled with low solid phase mixed silver.
6. A method for printing a light-curable conductive ink filled with mixed silver at low solid phase as claimed in claim 1, Features It is carried out in the following steps:
1. Apply or spray the low solid phase filled mixed silver light-curable printing conductive ink on a flat or curved substrate; 2. Use modeling software to design the circuit, and perform UV light path scanning and curing according to the preset printing pattern under the conditions of UV light wavelength of 350nm to 420nm, power of 5mW to 10mW and scanning speed of 5mm / s to 30mm / s; 3. Clean the ink outside the pattern with an isopropyl alcohol solution, and then perform light treatment or heat treatment to complete the printing method of the light-curing conductive ink filled with low solid phase mixed silver.
7. A method for printing a low solid phase filled mixed silver light-curable conductive ink according to claim 6, Features The substrate described in step 1 is a glass substrate, a ceramic substrate or a plastic substrate.
8. The method for printing a light-curable conductive ink filled with mixed silver at low solid phase according to claim 6, Features In step 1, the light-curable printing conductive ink filled with low solid phase mixed silver is coated or sprayed on a flat or curved substrate at a coating thickness of 20 μm to 100 μm.
9. The method for printing a light-curable conductive ink filled with mixed silver at low solid phase according to claim 6, Features The mass percentage of the isopropanol solution described in step 3 is 30% to 60%.
10. The method for printing a light-curable conductive ink filled with mixed silver at low solid phase according to claim 6, Features The light treatment described in step 3 is specifically performed at a wavelength of 350nm to 420nm and a power density of 20mW / cm 2 ~80mW / cm 2 Under the condition of , the light treatment is carried out for 10min to 30min; the heat treatment described in step 3 is specifically carried out at a temperature of 100°C to 200°C for 30min to 60min.
Citation Information
Patent Citations
Front silver paste for crystalline silicon solar battery plate and preparation method thereof
CN101986391A
Conductive material and process
CN104024351A
Conductive silver paste capable of being sintered at low temperature and preparation method therefor
CN105469849A
Preparation method of prepolymer containing nano-silver sheet and conductive adhesive thereof
CN110819290A
Conductive silver paste based on smooth ultrathin flake silver powder and preparation method of conductive silver paste
CN111599507A