Formaldehyde-removing coating with sound insulation effect and preparation method of formaldehyde-removing coating
By adding sound-insulating fillers and formaldehyde-absorbing fillers, especially modified diatomite, to the styrene-acrylic emulsion, the problem of the lack of formaldehyde removal and sound-insulating capabilities in the existing styrene-acrylic emulsion coatings is solved, and the formaldehyde adsorption and sound-insulating properties of the coating are achieved. significant improvement.
Patent Information
- Application Number
- CN202410966558.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-18
AI Technical Summary
Existing styrene-acrylic emulsion insulation coatings lack formaldehyde removal and sound insulation capabilities.
Adding sound-insulating fillers and formaldehyde-absorbing fillers to the styrene-acrylic emulsion, especially through the preparation method of modified diatomite, can improve the formaldehyde adsorption and sound-insulating properties of the coating.
Significantly improves the formaldehyde adsorption and sound insulation effect of the coating. Compared with unmodified diatomite, the addition of modified diatomite can significantly improve the formaldehyde adsorption capacity.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coating preparation, and in particular to a formaldehyde-removing coating with sound insulation effect and a preparation method thereof. Background Art
[0002] Styrene acrylic emulsion is a polymer material obtained by emulsion copolymerization of styrene and acrylate monomers. It is widely used in the production of architectural coatings, metal surface latex coatings, floor coatings, paper adhesives, adhesives, etc. due to its excellent properties such as good adhesion, transparent film, water resistance, oil resistance, heat resistance, and aging resistance.
[0003] For example, Chinese invention patent CN201010269978.X discloses a styrene acrylic emulsion thermal insulation coating, which contains 70 parts of styrene acrylic emulsion, 35 parts of closed-cell perlite, 36 parts of ethylenediamine, 10 parts of polypropylene fiber, 45 parts of acrylic resin, 12 parts of potassium sodium silicate, 5 parts of triethanolamine, 10 parts of phenol, 6 parts of binder, 10 parts of turpentine, 65 parts of water, 2 parts of preservative, 15 parts of kaolin, 3 parts of thickener, and 1 part of film-forming aid. Although the styrene acrylic emulsion thermal insulation coating has good thermal insulation, water resistance and alkali resistance, it does not have the function of removing formaldehyde, and the sound insulation ability needs to be further improved. Summary of the invention
[0004] In order to overcome at least one of the technical problems existing in the prior art, the present invention provides a formaldehyde-removing paint with sound insulation effect and a preparation method thereof.
[0005] The above technical problems to be solved by the present invention are achieved through the following technical solutions:
[0006] The invention provides a formaldehyde-removing paint with sound insulation effect, comprising styrene acrylic emulsion, defoamer, leveling agent, film-forming agent, dispersant and water; in addition, it also comprises sound insulation filler and formaldehyde adsorption filler.
[0007] The invention adds sound insulation filler and formaldehyde adsorption filler so that the prepared coating has sound insulation effect and formaldehyde adsorption effect.
[0008] Preferably, the sound insulation filler is selected from hollow glass microspheres.
[0009] Preferably, the formaldehyde adsorption filler is diatomaceous earth.
[0010] Preferably, the diatomaceous earth is modified diatomaceous earth;
[0011] The modified diatomaceous earth is prepared by the following method:
[0012] (1) taking diatomaceous earth, adding it to water, and stirring evenly to obtain a diatomaceous earth dispersion;
[0013] (2) Add cobalt chloride and titanium chloride to the diatomite dispersion and stir evenly, then add sodium hydroxide, heat to 50-70° C., continue stirring for 3-6 hours, and then filter and separate to obtain a solid mixture.
[0014] (3) calcining the solid mixture at 800-1200° C. for 3-6 hours; after the calcination, taking the calcined solid to obtain the modified diatomite.
[0015] The inventors found in their research that adding modified diatomaceous earth prepared by the above method of the present invention to the coating can greatly improve the formaldehyde adsorption effect of the coating compared to adding unmodified diatomaceous earth.
[0016] Preferably, the ratio of diatomaceous earth to water in step (1) is 1 kg: 10-20 L.
[0017] Most preferably, the ratio of diatomaceous earth to water in step (1) is 1 kg:15 L.
[0018] Preferably, in step (2), the usage ratio of diatomaceous earth dispersion to cobalt chloride, titanium chloride and sodium hydroxide is 10-20 L: 0.10-0.15 kg: 0.15-0.20 kg: 0.20-0.30 kg.
[0019] Most preferably, in step (2), the ratio of the diatomaceous earth dispersion to cobalt chloride, titanium chloride and sodium hydroxide is 15L:0.13kg:0.19kg:0.24kg.
[0020] Preferably, an auxiliary agent is also added in step (2).
[0021] Preferably, the dosage ratio of diatomaceous earth dispersion to auxiliary agent is 10-20 L: 0.1-0.2 kg.
[0022] Most preferably, the dosage ratio of diatomaceous earth dispersion to auxiliary agent is 15L:0.15kg.
[0023] Preferably, the auxiliary agent consists of sodium methylene dinaphthalene sulfonate and sodium octadecyl toluene sulfonate.
[0024] Preferably, the weight ratio of sodium methylene dinaphthalene sulfonate to sodium octadecyl toluene sulfonate is 1-3:1-3.
[0025] The inventors found in further research that the addition of additives is critical in the modification process of diatomite; the study shows that the modified diatomite prepared by adding additives composed of sodium methylene dinaphthalene sulfonate and sodium octadecyl toluene sulfonate can further significantly improve the formaldehyde adsorption effect of the coating compared to the modified diatomite prepared without adding additives composed of sodium methylene dinaphthalene sulfonate and sodium octadecyl toluene sulfonate.
[0026] Preferably, in step (3), the solid mixture is calcined at 1000° C. for 5 h; after the calcination, the calcined solid is taken to obtain the modified diatomite.
[0027] Preferably, the formaldehyde-removing paint with sound insulation effect comprises the following raw material components in parts by weight:
[0028] 80-120 parts of styrene-acrylic emulsion; 30-50 parts of sound insulation filler; 20-30 parts of formaldehyde adsorption filler; 1-3 parts of defoaming agent; 1-5 parts of leveling agent; 1-3 parts of dispersant; 4-8 parts of film-forming agent; 50-70 parts of water.
[0029] Preferably, the formaldehyde-removing paint with sound insulation effect comprises the following raw material components in parts by weight:
[0030] 90-110 parts of styrene-acrylic emulsion; 30-40 parts of sound insulation filler; 20-25 parts of formaldehyde adsorption filler; 1-2 parts of defoaming agent; 2-4 parts of leveling agent; 1-2 parts of dispersant; 4-6 parts of film-forming agent; 50-60 parts of water.
[0031] Most preferably, the formaldehyde-removing paint with sound insulation effect comprises the following raw material components in parts by weight:
[0032] 100 parts of styrene acrylic emulsion; 40 parts of sound insulation filler; 25 parts of formaldehyde adsorption filler; 1 part of defoamer; 2 parts of leveling agent; 2 parts of dispersant; 5 parts of film-forming agent; 60 parts of water.
[0033] The present invention also provides a method for preparing the above-mentioned formaldehyde-removing coating with sound insulation effect, which comprises the following steps:
[0034] The formaldehyde-removing paint with sound insulation effect can be obtained by uniformly dispersing styrene-acrylic emulsion, defoaming agent, leveling agent, film-forming agent, dispersant, sound insulation filler, formaldehyde adsorption filler and water.
[0035] Beneficial effects: The present invention provides a formaldehyde-removing paint with a new composition and sound insulation effect; the present invention adds sound insulation fillers and formaldehyde adsorption fillers, so that the prepared paint has sound insulation and formaldehyde adsorption effects; in particular, further adding modified diatomaceous earth prepared by the method of the present invention can greatly improve the formaldehyde adsorption effect of the paint compared with adding unmodified diatomaceous earth. DETAILED DESCRIPTION
[0036] The present invention is further explained below in conjunction with specific examples, but the examples do not limit the present invention in any form.
[0037] The raw materials in the following examples are all common raw materials that can be purchased by those skilled in the art through conventional channels.
[0038] Example 1 Formaldehyde-removing coating with sound insulation effect
[0039] Raw materials by weight: 100 parts of styrene acrylic emulsion; 40 parts of sound insulation filler; 25 parts of formaldehyde adsorption filler; 1 part of defoamer; 2 parts of leveling agent; 2 parts of dispersant; 5 parts of film-forming agent; 60 parts of water;
[0040] The sound insulation filler is hollow glass microspheres;
[0041] The formaldehyde adsorption filler is diatomaceous earth.
[0042] Preparation method: After styrene acrylic emulsion, defoaming agent, leveling agent, film-forming agent, dispersant, sound insulation filler, formaldehyde adsorption filler and water are evenly dispersed, the formaldehyde-removing paint with sound insulation effect is obtained.
[0043] Example 2 Formaldehyde-removing coating with sound insulation effect
[0044] Raw materials by weight: 100 parts of styrene acrylic emulsion; 40 parts of sound insulation filler; 25 parts of formaldehyde adsorption filler; 1 part of defoamer; 2 parts of leveling agent; 2 parts of dispersant; 5 parts of film-forming agent; 60 parts of water;
[0045] The sound insulation filler is hollow glass microspheres;
[0046] The formaldehyde adsorption filler is modified diatomaceous earth;
[0047] The modified diatomaceous earth is prepared by the following method:
[0048] (1) taking diatomaceous earth, adding it to water, and stirring it evenly to obtain a diatomaceous earth dispersion; wherein the ratio of diatomaceous earth to water is 1 kg:15 L;
[0049] (2) adding cobalt chloride and titanium chloride to the diatomite dispersion and stirring evenly, then adding sodium hydroxide, heating to 60° C., continuing stirring for 4 hours and filtering to separate a solid mixture; wherein the amount ratio of the diatomite dispersion to cobalt chloride, titanium chloride and sodium hydroxide is 15L:0.13kg:0.19kg:0.24kg;
[0050] (3) calcining the solid mixture at 1000° C. for 5 h; after the calcination, taking the calcined solid to obtain the modified diatomite.
[0051] Preparation method: After styrene acrylic emulsion, defoaming agent, leveling agent, film-forming agent, dispersant, sound insulation filler, formaldehyde adsorption filler and water are evenly dispersed, the formaldehyde-removing paint with sound insulation effect is obtained.
[0052] Example 3 Formaldehyde-removing coating with sound insulation effect
[0053] Raw materials by weight: 100 parts of styrene acrylic emulsion; 40 parts of sound insulation filler; 25 parts of formaldehyde adsorption filler; 1 part of defoamer; 2 parts of leveling agent; 2 parts of dispersant; 5 parts of film-forming agent; 60 parts of water;
[0054] The sound insulation filler is hollow glass microspheres;
[0055] The formaldehyde adsorption filler is modified diatomaceous earth;
[0056] The modified diatomaceous earth is prepared by the following method:
[0057] (1) taking diatomaceous earth, adding it to water, and stirring it evenly to obtain a diatomaceous earth dispersion; wherein the ratio of diatomaceous earth to water is 1 kg:15 L;
[0058] (2) adding an auxiliary agent to the diatomite dispersion, then adding cobalt chloride and titanium chloride and stirring evenly, then adding sodium hydroxide, heating to 60° C., continuing stirring for 4 hours, and filtering and separating to obtain a solid mixture; wherein the amount ratio of the diatomite dispersion to cobalt chloride, titanium chloride and sodium hydroxide is 15L:0.13kg:0.19kg:0.24kg; the amount ratio of the diatomite dispersion to the auxiliary agent is 15L:0.15kg; the auxiliary agent is composed of sodium methylene dinaphthalene sulfonate and sodium octadecyl toluene sulfonate in a weight ratio of 1:1;
[0059] (3) calcining the solid mixture at 1000° C. for 5 h; after the calcination, taking the calcined solid to obtain the modified diatomite.
[0060] Preparation method: After styrene acrylic emulsion, defoaming agent, leveling agent, film-forming agent, dispersant, sound insulation filler, formaldehyde adsorption filler and water are evenly dispersed, the formaldehyde-removing paint with sound insulation effect is obtained.
[0061] Example 4 Formaldehyde-removing coating with sound insulation effect
[0062] Raw materials by weight: 100 parts of styrene acrylic emulsion; 40 parts of sound insulation filler; 25 parts of formaldehyde adsorption filler; 1 part of defoamer; 2 parts of leveling agent; 2 parts of dispersant; 5 parts of film-forming agent; 60 parts of water;
[0063] The sound insulation filler is hollow glass microspheres;
[0064] The formaldehyde adsorption filler is modified diatomaceous earth;
[0065] The modified diatomaceous earth is prepared by the following method:
[0066] (1) taking diatomaceous earth, adding it to water, and stirring it evenly to obtain a diatomaceous earth dispersion; wherein the ratio of diatomaceous earth to water is 1 kg:15 L;
[0067] (2) adding an auxiliary agent to the diatomite dispersion, then adding cobalt chloride and titanium chloride and stirring evenly, then adding sodium hydroxide, heating to 60° C., continuing stirring for 4 hours, and filtering and separating to obtain a solid mixture; wherein the amount ratio of the diatomite dispersion to cobalt chloride, titanium chloride and sodium hydroxide is 15L:0.13kg:0.19kg:0.24kg; the amount ratio of the diatomite dispersion to the auxiliary agent is 15L:0.15kg; the auxiliary agent is sodium methylene dinaphthalene sulfonate;
[0068] (3) calcining the solid mixture at 1000° C. for 5 h; after the calcination, taking the calcined solid to obtain the modified diatomite.
[0069] Preparation method: After styrene acrylic emulsion, defoaming agent, leveling agent, film-forming agent, dispersant, sound insulation filler, formaldehyde adsorption filler and water are evenly dispersed, the formaldehyde-removing paint with sound insulation effect is obtained.
[0070] Example 5 Formaldehyde-removing coating with sound insulation effect
[0071] Raw materials by weight: 100 parts of styrene acrylic emulsion; 40 parts of sound insulation filler; 25 parts of formaldehyde adsorption filler; 1 part of defoamer; 2 parts of leveling agent; 2 parts of dispersant; 5 parts of film-forming agent; 60 parts of water;
[0072] The sound insulation filler is hollow glass microspheres;
[0073] The formaldehyde adsorption filler is modified diatomaceous earth;
[0074] The modified diatomaceous earth is prepared by the following method:
[0075] (1) taking diatomaceous earth, adding it to water, and stirring it evenly to obtain a diatomaceous earth dispersion; wherein the ratio of diatomaceous earth to water is 1 kg:15 L;
[0076] (2) adding an auxiliary agent to the diatomite dispersion, then adding cobalt chloride and titanium chloride and stirring evenly, then adding sodium hydroxide, heating to 60° C., continuing stirring for 4 hours, and filtering and separating to obtain a solid mixture; wherein the amount ratio of the diatomite dispersion to cobalt chloride, titanium chloride and sodium hydroxide is 15L:0.13kg:0.19kg:0.24kg; the amount ratio of the diatomite dispersion to the auxiliary agent is 15L:0.15kg; the auxiliary agent is sodium octadecyl toluene sulfonate;
[0077] (3) calcining the solid mixture at 1000° C. for 5 h; after the calcination, taking the calcined solid to obtain the modified diatomite.
[0078] Preparation method: After styrene acrylic emulsion, defoaming agent, leveling agent, film-forming agent, dispersant, sound insulation filler, formaldehyde adsorption filler and water are evenly dispersed, the formaldehyde-removing paint with sound insulation effect is obtained.
[0079] Experimental example: Formaldehyde adsorption capacity test
[0080] The formaldehyde detector is fixed on the side wall of a 10L glass bottle; then it is sealed with a sealing plug with an injection tube; 1L of the paint to be tested is injected through the injection tube; then formaldehyde is injected through the injection tube so that the formaldehyde concentration in the glass bottle is 10mg / m 3 ; After sealing and storing for 1 day, record the formaldehyde concentration of the formaldehyde detector;
[0081] According to the above method, the formaldehyde adsorption effect of the formaldehyde-removing paint with sound insulation effect prepared in Examples 1 to 5 was tested; each group of paints was tested 5 times and the average value was taken; the test results are shown in Table 1.
[0082] Table 1. Formaldehyde adsorption test results
[0083] Test coating types Formaldehyde concentration Experimental Group 1 The formaldehyde-removing coating with sound insulation effect prepared by experimental group 1 <![CDATA[8.5mg / m 3 <!-- 4 -->]]> Experimental Group 2 The formaldehyde-removing coating with sound insulation effect prepared by experimental group 1 <![CDATA[5.7mg / m 3 ]]> Experimental Group 3 The formaldehyde-removing coating with sound insulation effect prepared by experimental group 1 <![CDATA[3.1mg / m 3 ]]> Experimental Group 4 The formaldehyde-removing coating with sound insulation effect prepared by experimental group 1 <![CDATA[4.9mg / m 3 ]]> Experimental Group 5 The formaldehyde-removing coating with sound insulation effect prepared by experimental group 1 <![CDATA[4.5mg / m 3 ]]>
[0084] From the experimental results in Table 1, it can be seen that the formaldehyde concentration in experimental group 1 is 8.5 mg / m 3 , compared with the original formaldehyde concentration of 10mg / m 3 , which is significantly reduced; this shows that: the present invention makes the prepared coating have formaldehyde adsorption effect by adding formaldehyde adsorption filler diatomaceous earth.
[0085] It can be seen from the experimental results in Table 1 that the formaldehyde concentration of Experimental Group 2 is further significantly reduced compared with that of Experimental Group 1; this indicates that adding the modified diatomaceous earth prepared by the method of the present invention to the coating can significantly improve the formaldehyde adsorption effect of the coating compared with adding unmodified diatomaceous earth.
[0086] It can be seen from the experimental results in Table 1 that the formaldehyde concentration of experimental group 3 is also further significantly reduced compared with that of experimental group 2; this shows that: in the modification process of diatomite, the addition of additives is very critical; the above experiment shows that the modified diatomite prepared by adding additives composed of sodium methylene dinaphthalene sulfonate and sodium octadecyl toluene sulfonate can further significantly improve the formaldehyde adsorption effect of the coating compared with the modified diatomite prepared without adding additives composed of sodium methylene dinaphthalene sulfonate and sodium octadecyl toluene sulfonate.
[0087] It can be seen from the experimental results in Table 1 that the formaldehyde concentrations of experimental groups 4 and 5 are lower than those of experimental group 2, but the reduction is not large; the reduction is much smaller than that of experimental group 3; this shows that in the modification process of diatomaceous earth, the modified diatomaceous earth prepared by the auxiliary agent composed of sodium methylene dinaphthalene sulfonate and sodium octadecyl toluene sulfonate must be added, which can further significantly improve the formaldehyde adsorption effect of the coating compared with the modified diatomaceous earth prepared without the auxiliary agent composed of sodium methylene dinaphthalene sulfonate and sodium octadecyl toluene sulfonate; however, the modified diatomaceous earth prepared by adding only a single sodium methylene dinaphthalene sulfonate or a single sodium octadecyl toluene sulfonate cannot further significantly improve the formaldehyde adsorption effect of the coating.
Claims
1. A formaldehyde-removing paint with sound insulation effect, comprising styrene acrylic emulsion, defoamer, leveling agent, film-forming agent, dispersant and water, characterized in that: It also contains sound insulation fillers and formaldehyde absorbing fillers.
2. The formaldehyde-removing paint with sound insulation effect according to claim 1, characterized in that: The sound insulation filler is selected from hollow glass microspheres.
3. The formaldehyde-removing paint with sound insulation effect according to claim 1, characterized in that: The formaldehyde adsorption filler is diatomaceous earth.
4. The formaldehyde-removing paint with sound insulation effect according to claim 3, characterized in that: The diatomaceous earth is modified diatomaceous earth; The modified diatomaceous earth is prepared by the following method: (1) taking diatomaceous earth, adding it to water, and stirring evenly to obtain a diatomaceous earth dispersion; (2) Add cobalt chloride and titanium chloride to the diatomite dispersion and stir evenly, then add sodium hydroxide, heat to 50-70° C., continue stirring for 3-6 hours, and then filter and separate to obtain a solid mixture. (3) calcining the solid mixture at 800-1200° C. for 3-6 hours; after the calcination, taking the calcined solid to obtain the modified diatomite.
5. The formaldehyde-removing paint with sound insulation effect according to claim 4, characterized in that: In step (1), the usage ratio of diatomaceous earth to water is 1kg:10-20L.
6. The formaldehyde-removing paint with sound insulation effect according to claim 4, characterized in that: In step (2), the usage ratio of diatomaceous earth dispersion to cobalt chloride, titanium chloride and sodium hydroxide is 10-20 L: 0.10-0.15 kg: 0.15-0.20 kg: 0.20-0.30 kg.
7. The formaldehyde-removing paint with sound insulation effect according to claim 4, characterized in that: In step (3), the solid mixture is calcined at 1000° C. for 5 hours; after the calcination, the calcined solid is taken to obtain the modified diatomite.
8. The formaldehyde-removing paint with sound insulation effect according to claim 1, characterized in that: The raw material components include the following parts by weight: 80-120 parts of styrene-acrylic emulsion; 30-50 parts of sound insulation filler; 20-30 parts of formaldehyde adsorption filler; 1-3 parts of defoaming agent; 1-5 parts of leveling agent; 1-3 parts of dispersant; 4-8 parts of film-forming agent; 50-70 parts of water.
9. The formaldehyde-removing paint with sound insulation effect according to claim 1, characterized in that: The raw material components include the following parts by weight: 90-110 parts of styrene-acrylic emulsion; 30-40 parts of sound insulation filler; 20-25 parts of formaldehyde adsorption filler; 1-2 parts of defoaming agent; 2-4 parts of leveling agent; 1-2 parts of dispersant; 4-6 parts of film-forming agent; 50-60 parts of water.
10. The method for preparing the formaldehyde-removing paint with sound insulation effect according to any one of claims 1 to 9, characterized in that: The following steps are included: The formaldehyde-removing paint with sound insulation effect can be obtained by uniformly dispersing styrene-acrylic emulsion, defoaming agent, leveling agent, film-forming agent, dispersant, sound insulation filler, formaldehyde adsorption filler and water.
Citation Information
Patent Citations
Multifunctional internal wall thermal-insulation paint
CN104530844A
Formaldehyde-removing environment-friendly water-based paint and preparation method thereof
CN105062242A
Diatom mud efficient in absorbing formaldehyde and construction method thereof
CN108069674A
Preparation method for odor-less all-effect latex paint
CN109266137A
Odorless environment-friendly coating material
CN111187544A