SiO2 / PVDF (Polyvinylidene Fluoride) hydrophobic self-cleaning coating solution as well as preparation method and application thereof
By combining nano-SiO2 with PVDF and modifying it by grafting, a hydrophobic self-cleaning coating with high durability and high light transmittance is formed, which solves the problems of poor durability and insufficient light transmittance of existing coating materials in industrial applications. problem, achieving efficient applications in fields such as protecting photovoltaic equipment.
Patent Information
- Application Number
- CN202410900211.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-11
AI Technical Summary
Existing coating materials have problems with poor durability and insufficient light transmittance in industrial applications, especially in the fields of protecting photovoltaic equipment, precision equipment, aerospace vehicles and automobiles, and are difficult to meet the requirements for high durability and self-cleaning performance.
By combining nano-SiO2 with PVDF, grafting method is used to modify nano-SiO2 and introduce PVDF to form a highly durable hydrophobic self-cleaning coating. The reaction of OTS-SiO2 solution and DMF is used to form a coating structure and improve the hydrophobic angle of the coating. and light transmittance.
A hydrophobic self-cleaning coating with high durability and high light transmittance is achieved. The hydrophobic angle reaches 103°-115.9°, the light transmittance is between 67%-81%, and the pencil hardness reaches 6H, which significantly improves the coating’s durability. Abrasion resistance and durability.
Smart Images

Figure CN118755322A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of coating materials and relates to the preparation of functional coatings, in particular to a SiO2 / PVDF hydrophobic self-cleaning coating solution and a preparation method and application thereof. Background Art
[0002] The development and progress of industry have rapidly increased human production capacity and made lifestyles more diverse. However, at the same time, the rapid development of industry has also led to environmental deterioration, such as sandstorms caused by soil erosion in the northwest region and fog and river pollution caused by various process waste gases, waste liquids and waste residues discharged from factories. These waste gases and waste liquids have caused huge losses in many fields such as the photovoltaic industry, precision equipment application industries such as electronic appliances, outdoor glass aesthetics, aerospace, and the automotive industry. In order to reduce the impact of pollution, people have adopted a variety of ways to mitigate pollution, such as manual cleaning, mechanical automatic cleaning, electric screen screening, and surface modification (super-hydrophobic and super-hydrophilic). Among them, super-hydrophobic and super-clear water surface modification with self-cleaning properties have received attention in many application fields and are regarded as effective methods to solve the impact of various pollution such as dust, sand, oil, and corrosion.
[0003] Researchers have discovered natural hydrophobic phenomena on plant branches and leaves in nature, such as lotus leaves with super-hydrophobic properties, which come from the special microscopic nanotexture structure on their surface. By observing and studying the hydrophobic phenomena and principles of natural plants, a large number of coating materials with relevant hydrophobic properties have been prepared and widely used in various fields. With the extensive research and application of relevant hydrophobic materials, more and more industries and fields have begun to use relevant hydrophobic materials or modify products through relevant principles, and have put forward higher requirements for hydrophobic coating materials. Different application industries have different performance requirements for super-hydrophobic coatings. The application value and prospects of super-hydrophobic materials have led to its continuous research in academia and industry. More and more super-hydrophobic materials have been developed and applied in production and life. The application with publication number CN110760224 A discloses a method for preparing a super hydrophobic film. The material uses PVDF and silica as raw materials, and mainly utilizes the unique chemical stability of these two raw materials to achieve anti-icing and anti-corrosion; the application with publication number CN115734991A discloses a composite coating prepared using fluorine-containing polymers, silica, hydrophilic polymers and modifiers, which has the effect of increasing atmospheric condensation on the surface of the substrate; it can be seen that even if the raw materials used are the same, but the preparation processes are different, the performance of the coatings obtained is very different; in order to obtain a coating material with high durability, self-cleaning properties and good light transmittance, this research group has conducted in-depth research. Summary of the invention
[0004] In order to solve the above technical problems, the present invention proposes a SiO2 / PVDF hydrophobic self-cleaning coating solution and a preparation method and application thereof.
[0005] The technical solution of the present invention is achieved in this way: A method for preparing a SiO2 / PVDF hydrophobic self-cleaning coating solution, comprising the following steps: (1) Dispersing nano-SiO2 in a mixed solution of ammonia water and anhydrous ethanol to obtain SiO2 dispersed ammonia solution; (2) After OTS and anhydrous ethanol are mixed, they are stirred evenly under the acidic conditions provided by glacial acetic acid to obtain an OTS modified solution; (3) mixing the SiO2 dispersed ammonia solution of step (1) and the OTS modified solution of step (2), and heating and stirring to perform reaction I to obtain an OTS-SiO2 solution; (4) DMF is added to the OTS-SiO2 solution of step (3), and after mixing, PVDF is added, and after heating and stirring, a PVDF@OTS-SiO2 coating suspension is obtained, i.e., a SiO2 / PVDF hydrophobic self-cleaning solution.
[0006] In the above step (1), the concentration of SiO2 in the SiO2 dispersed ammonia solution is 0.01-0.1 g / mL, and the particle size of SiO2 is 12 nm; the volume ratio of ammonia water to anhydrous ethanol in the SiO2 dispersed ammonia solution is 1:2-10.
[0007] In the above step (2), the volume ratio of OTS to anhydrous ethanol is 1:10-100.
[0008] In the above step (3), the volume ratio of SiO2 dispersed ammonia solution to OTS modified solution is 1:0.5-10.
[0009] The reaction temperature of the above-mentioned heating and stirring reaction I is 40-45°C and the reaction time is 12-15h.
[0010] In the above step (4), the volume ratio of OTS-SiO2 solution to DMF is 1-4:7.5; the addition ratio of OTS-SiO2 solution to PVDF is 0.5-2 mL of OTS-SiO2 solution per g of PVDF.
[0011] The reaction temperature of the above-mentioned heating and stirring reaction II is 70-75°C and the reaction time is 2-2.5h.
[0012] The SiO2 / PVDF hydrophobic self-cleaning coating solution is prepared by the above method.
[0013] When the volume ratio of OTS-SiO2 solution to DMF is 1:2.5, the hydrophobic angle reaches a maximum value of 115.9° and the pencil hardness is 6H.
[0014] The SiO2 / PVDF hydrophobic self-cleaning coating prepared by using the above-mentioned SiO2 / PVDF hydrophobic self-cleaning coating solution has self-cleaning performance, a light transmittance of 67%-81%, and a hydrophobic angle of 103°-115.9°.
[0015] The above-mentioned SiO2 / PVDF hydrophobic self-cleaning coating solution is used in the preparation of coatings for protecting photovoltaic equipment, precision equipment, aerospace vehicles, automobile fields and electronic equipment.
[0016] The preparation mechanism of the coating of this application is: Figure 8 As shown in the figure, the -(CH2)7CH3 group obtained by hydrolysis of n-octyltriethoxysilane is grafted onto nano-SiO2 by the grafting method, so that the nano-SiO2 is modified and becomes hydrophobic. Since the viscosity of the solution is very high after PVDF is dissolved, a coating structure will be formed. When PVDF is not added, the scanning image of nano-SiO2 should be a regular agglomeration structure, as shown in the figure below. Fig. 9 As shown, the structure is irregular, and it can be seen that PVDF encapsulates nano-SiO2 to form an encapsulated structure. Therefore, when OTS-SiO2 is introduced into PVDF, the hydrophobic angle of the coating decreases compared to when OTS-SiO2 is directly sprayed, because PVDF encapsulates the agglomerated particles of SiO2. However, the introduction of PVDF greatly improves the durability of the coating, and finally a highly durable nano-SiO2 / PVDF hydrophobic self-cleaning coating is obtained.
[0017] The present invention has the following beneficial effects: (1) The present invention modifies nano-SiO2 by a grafting method, wherein n-octyltriethoxysilane (OTS) grafts -(CH2)7CH3 obtained by hydrolysis onto nano-SiO2, and the hydroxyl groups of the nano-silica side chains are modified into hydrophobic methyl groups, making the nano-SiO2 hydrophobic.
[0018] (2) The present invention introduces PVDF to improve the pencil hardness of the coating, i.e., durability (hardness 6H). Polyvinylidene fluoride (PVDF) has low surface energy, excellent inherent wear resistance and self-lubricating properties. Self-lubricating PVDF and rigid SiO2 can effectively improve wear resistance. When PVDF is not added, the pencil hardness of the OTS-SiO2 coating is only 2H. After the introduction of PVDF, the pencil hardness of the coating reaches 6H.
[0019] (3) The present invention can reduce the roughness of the coating surface through the spraying method, and improve the mechanical durability, so that a highly durable nano-SiO2 / PVDF hydrophobic self-cleaning coating can be produced.
[0020] (4) The present invention modifies nano-SiO2 by OTS. Currently, most modified SiO2 uses fluorine-containing modifiers, while OTS modifiers do not contain fluorine and are more environmentally friendly.
[0021] (5) The present invention breaks through the poor durability of most existing coatings and achieves high durability, providing a new direction for the design of highly durable hydrophobic self-cleaning coatings. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 The hydrophobic angle diagram of the coatings prepared in Examples 1-4 and Comparative Example 1.
[0024] Figure 2 The self-cleaning effect diagram of the coating prepared in Examples 1-4 and Comparative Example 1.
[0025] Figure 3 The light transmittance diagram of the coatings prepared in Examples 1-4 and Comparative Example 1.
[0026] Figure 4 The infrared spectra of the coatings prepared in Examples 1-4 and Comparative Example 1 are shown.
[0027] Figure 5 Surface morphology of the coatings prepared in Examples 1-4 and Comparative Example 1.
[0028] Figure 6 Graph showing the reflectivity of the coatings prepared in Examples 1-4 and Comparative Example 1.
[0029] Figure 7 The solar energy conversion efficiency diagram of the coatings prepared in Examples 1-4 and Comparative Example 1; IV curve diagram (a), PV curve diagram (b) and field test photos (c).
[0030] Figure 8 Diagram of the mechanism of OTS hydrolysis -(CH2)7CH3 group grafted onto nano-SiO2.
[0031] Fig. 9 This is the SEM test image of PVDF coated nano-SiO2. DETAILED DESCRIPTION
[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Unless otherwise specified, the experimental methods used in the following experimental examples are all conventional methods; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.
[0034] A method for preparing a SiO2 / PVDF hydrophobic self-cleaning coating solution, comprising the following steps: (1) Dispersing nano-SiO2 in a mixed solution of ammonia water and anhydrous ethanol to obtain SiO2 dispersed ammonia solution; (2) After OTS and anhydrous ethanol are mixed, they are stirred evenly under the acidic conditions provided by glacial acetic acid to obtain an OTS modified solution; (3) mixing the SiO2 dispersed ammonia solution of step (1) and the OTS modified solution of step (2), and heating and stirring to perform reaction I to obtain an OTS-SiO2 solution; (4) DMF is added to the OTS-SiO2 solution of step (3), and after mixing, PVDF is added, and after heating and stirring, a PVDF@OTS-SiO2 coating suspension is obtained, i.e., a SiO2 / PVDF hydrophobic self-cleaning solution.
[0035] The concentration of SiO2 in the SiO2 dispersed ammonia solution in the above step (1) is 0.01-0.1 g / mL, for example, 0.01-0.05 g / mL, 0.05-0.1 g / mL, 0.02 g / mL, 0.03 g / mL, 0.04 g / mL or 0.05 g / mL; 0.021 g / mL is taken as an example in the embodiment.
[0036] The particle size of SiO2 is 12nm.
[0037] The volume ratio of aqueous ammonia and anhydrous ethanol in the SiO2 dispersed ammonia solution is 1:2-10. For example, the ratio between the two can be 1:2-6, 1:6-10, 1:4-8, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10.
[0038] In the above step (2), the volume ratio of OTS to anhydrous ethanol is 1:10-100, for example, the ratio between the two can be 1:10-50, 1:50-80, 1:80-100, 1:10, 1:20, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90 or 1:100.
[0039] In the above step (3), the volume ratio of SiO2 dispersed ammonia solution to OTS modified solution is 1:0.5-10.
[0040] The reaction temperature of the above-mentioned heating and stirring reaction I is 40-45°C, for example, the reaction temperature is 40-43°C, 43-45°C, 40°C, 41°C, 42°C, 43°C, 44°C or 45°C; the reaction time is 12-15h, for example, the reaction time is 12-13h, 13-15h, 12h, 13h, 14h or 15h.
[0041] In the above step (4), the volume ratio of OTS-SiO2 solution to DMF is 1-4:7.5, for example, the volume ratio is 1-2:7.5, 2-4:7.5, 1:7.5, 2:7.5, 3:7.5, 4:7.5, and the addition ratio of OTS-SiO2 solution to PVDF is 0.5-2 mL of OTS-SiO2 solution per g PVDF, for example, 0.5-1 mL of OTS-SiO2 solution per g PVDF, 1-1.5 mL of OTS-SiO2 solution per g PVDF, 1.5-2 mL of OTS-SiO2 solution per g PVDF, 0.5 mL of OTS-SiO2 solution per g PVDF, 1 mL of OTS-SiO2 solution per g PVDF, 1.5 mL of OTS-SiO2 solution per g PVDF, or 2 mL of OTS-SiO2 solution per g PVDF.
[0042] The reaction temperature of the above-mentioned heating and stirring reaction II is 70-75°C and the reaction time is 2-2.5h.
[0043] Specifically, the following embodiments are used as examples for description: Example 1 The method for preparing a highly durable nano-SiO2 / PVDF hydrophobic self-cleaning coating solution of this embodiment comprises the following steps: Step 1: 1.0 g of nano-SiO2 was slowly dissolved in a mixture of 8 mL of ammonia water and 40 mL of anhydrous ethanol, and stirred for 10 min to mix.
[0044] Step 2: Add 2 mL of OTS and 100 mL of anhydrous ethanol, mix them evenly at room temperature, then add 10 mL of glacial acetic acid, and stir ultrasonically for 60 minutes.
[0045] Step 3: Add 10 mL of silica dispersed ammonia solution and 10 mL of OTS modified solution, mix well, and stir at 43 °C for 13 h to obtain OTS-SiO2 solution.
[0046] Step 4: Add 1 mL of OTS-SiO2 solution and 7.5 mL of DMF, mix them evenly, then add 2 g of PVDF, stir at 73 °C for 2 h to obtain PVDF@OTS-SiO2 coating suspension, i.e., SiO2 / PVDF hydrophobic self-cleaning solution.
[0047] Coating performance test Add the prepared coating suspension into the liquid carrier barrel of the spray gun, adjust the spray gun position to keep it perpendicular to the surface of the glass substrate treated with piranha lotion, adjust the spray gun pressure to 10PSI, keep the distance between the spray gun mouth and the glass substrate at about 8-10cm, and the spray gun moving speed is about 3cm / s; spray the glass sheet, try to ensure that the above coating suspension covers the glass sheet evenly, dry it at room temperature, and then spray the next time. Repeat the above operation 3 times, and the drying time after each spraying is 1-2min. After the last spraying, place the glass sheet in a muffle furnace and bake it at 230℃ for 40min. A hydrophobic self-cleaning coating is obtained. Its hydrophobic angle reaches 103.2°, the transmittance reaches 79%, and the pencil hardness is 6H.
[0048] Example 2 The method for preparing a highly durable nano-SiO2 / PVDF hydrophobic self-cleaning coating solution of this embodiment comprises the following steps: Step 1: 1.0 g of nano-SiO2 was slowly dissolved in a mixture of 8 mL of ammonia water and 40 mL of anhydrous ethanol, and stirred for 10 min to mix.
[0049] Step 2: Add 2 mL of OTS and 100 mL of anhydrous ethanol, mix them evenly at room temperature, then add 10 mL of glacial acetic acid, and stir ultrasonically for 60 minutes.
[0050] Step 3: Add 10 mL of silica dispersed ammonia solution and 10 mL of OTS modified solution, mix well, and stir at 43 °C for 13 h to obtain OTS-SiO2 solution.
[0051] Step 4: Add 2 mL of OTS-SiO2 solution and 7.5 mL of DMF, mix them evenly, then add 2 g of PVDF, stir at 73 °C for 2 h to obtain PVDF@OTS-SiO2 coating suspension, i.e., SiO2 / PVDF hydrophobic self-cleaning solution.
[0052] Coating performance test Add the prepared coating suspension into the liquid carrier barrel of the spray gun, adjust the position of the spray gun to keep it perpendicular to the surface of the glass substrate treated with piranha lotion, adjust the spray gun pressure to 10PSI, keep the distance between the spray gun mouth and the glass substrate at about 8-10cm, and the spray gun moving speed is about 3cm / s; spray the glass sheet, try to ensure that the above coating suspension covers the glass sheet evenly, dry it at room temperature, and then spray the next time. Repeat the above operation 3 times, and the drying time after each spraying is 1-2min. After the last spraying, place the glass sheet in a muffle furnace and bake it at 230℃ for 40min. A hydrophobic self-cleaning coating is obtained. Its hydrophobic angle reaches 108.5°, the transmittance reaches 75%, and the pencil hardness is 6H.
[0053] Example 3 The method for preparing a highly durable nano-SiO2 / PVDF hydrophobic self-cleaning coating solution of this embodiment comprises the following steps: Step 1: 1.0 g of nano-SiO2 was slowly dissolved in a mixture of 8 mL of ammonia water and 40 mL of anhydrous ethanol, and stirred for 10 min to mix.
[0054] Step 2: Add 2 mL of OTS and 100 mL of anhydrous ethanol, mix them evenly at room temperature, then add 10 mL of glacial acetic acid, and stir ultrasonically for 60 minutes.
[0055] Step 3: Add 10 mL of silica dispersed ammonia solution and 10 mL of OTS modified solution, mix well, and stir at 43 °C for 13 h to obtain OTS-SiO2 solution.
[0056] Step 4: Add 3 mL of OTS-SiO2 solution and 7.5 mL of DMF, mix them evenly, then add 2 g of PVDF, stir at 73 °C for 2 h to obtain PVDF@OTS-SiO2 coating suspension, i.e., SiO2 / PVDF hydrophobic self-cleaning solution.
[0057] Coating performance test Add the prepared coating suspension into the liquid carrier barrel of the spray gun, adjust the position of the spray gun to keep it perpendicular to the surface of the glass substrate treated with piranha lotion, adjust the spray gun pressure to 10PSI, keep the distance between the spray gun mouth and the glass substrate at about 8-10cm, and the spray gun moving speed is about 3cm / s; spray the glass sheet, try to ensure that the above coating suspension covers the glass sheet evenly, dry it at room temperature, and then spray the next time. Repeat the above operation 3 times, and the drying time after each spraying is 1-2min. After the last spraying, place the glass sheet in a muffle furnace and bake it at 230℃ for 40min. A hydrophobic self-cleaning coating is obtained. Its hydrophobic angle reaches 115.9°, the transmittance reaches 68%, and the pencil hardness is 6H.
[0058] Example 4 The method for preparing a highly durable nano-SiO2 / PVDF hydrophobic self-cleaning coating solution of this embodiment comprises the following steps: Step 1: 1.0 g of nano-SiO2 was slowly dissolved in a mixture of 8 mL of ammonia water and 40 mL of anhydrous ethanol, and stirred for 10 min to mix.
[0059] Step 2: Add 2 mL of OTS and 100 mL of anhydrous ethanol, mix them evenly at room temperature, then add 10 mL of glacial acetic acid, and stir ultrasonically for 60 minutes.
[0060] Step 3: Add 10 mL of silica dispersed ammonia solution and 10 mL of OTS modified solution, mix well, and stir at 43 °C for 13 h to obtain OTS-SiO2 solution.
[0061] Step 4: Add 4 mL of OTS-SiO2 solution and 7.5 mL of DMF, mix them evenly, then add 2 g of PVDF, stir at 73 °C for 2 h to obtain PVDF@OTS-SiO2 coating suspension, i.e., SiO2 / PVDF hydrophobic self-cleaning solution.
[0062] Coating performance test Add the prepared coating suspension to the liquid carrier barrel of the spray gun, adjust the position of the spray gun to keep it perpendicular to the surface of the glass substrate treated with piranha lotion, adjust the spray gun pressure to 10PSI, keep the distance between the spray gun mouth and the glass substrate at about 8-10cm, and the spray gun moves at a speed of about 3cm / s; spray the glass sheet, try to ensure that the above coating suspension covers the glass sheet evenly, dry it at room temperature, and then spray the next time. Repeat the above operation 3 times, and the drying time after each spraying is 1-2min. After the last spraying, place the glass sheet in a muffle furnace and bake it at 230℃ for 40min. A hydrophobic self-cleaning coating is obtained. Its hydrophobic angle reaches 111.1°, the transmittance reaches 65%, and the pencil hardness is 6H.
[0063] Example 5 The method for preparing a highly durable nano-SiO2 / PVDF hydrophobic self-cleaning coating solution of this embodiment comprises the following steps: Step 1: 4.5 g of nano-SiO2 was slowly dissolved in a mixture of 15 mL of ammonia water and 30 mL of anhydrous ethanol, and stirred for 10 min to mix.
[0064] Step 2: Add 10 mL of OTS and 100 mL of anhydrous ethanol, mix them evenly at room temperature, then add 10 mL of glacial acetic acid, and stir ultrasonically for 60 minutes.
[0065] Step 3: Add 10 mL of silica-dispersed ammonia solution and 5 mL of OTS-modified solution, mix well, and stir at 40 °C for 15 h to obtain OTS-SiO2 solution.
[0066] Step 4: Add 3 mL of OTS-SiO2 solution and 7.5 mL of DMF, mix them evenly, then add 2 g of PVDF, stir at 70 °C for 2.5 h to obtain PVDF@OTS-SiO2 coating suspension, i.e., SiO2 / PVDF hydrophobic self-cleaning solution.
[0067] Coating performance test Add the prepared coating suspension into the liquid carrier barrel of the spray gun, adjust the position of the spray gun so that it is perpendicular to the surface of the glass substrate treated with piranha lotion, adjust the spray gun pressure to 10PSI, keep the distance between the spray gun nozzle and the glass substrate at about 8-10cm, and move the spray gun at a speed of about 3cm / s; spray the glass sheet, try to ensure that the above coating suspension covers the glass sheet evenly, dry it at room temperature, and then spray the next time. Repeat the above operation 3 times, and the drying time after each spraying is 1-2min. After the last spraying, place the glass sheet in a muffle furnace and bake it at 230℃ for 40min to obtain a hydrophobic self-cleaning coating.
[0068] Example 6 The method for preparing a highly durable nano-SiO2 / PVDF hydrophobic self-cleaning coating solution of this embodiment comprises the following steps: Step 1: 1.1 g of nano-SiO2 was slowly dissolved in a mixture of 10 mL of ammonia water and 100 mL of anhydrous ethanol, and stirred for 10 min to mix.
[0069] Step 2: Add 2 mL of LOTs and 200 mL of anhydrous ethanol, mix them evenly at room temperature, then add 50 mL of glacial acetic acid, and stir ultrasonically for 60 minutes.
[0070] Step 3: Add 1 mL of silica-dispersed ammonia solution and 10 mL of OTS-modified solution, mix well, and stir at 45 °C for 12 h to obtain OTS-SiO2 solution.
[0071] Step 4: Add 3 mL of OTS-SiO2 solution and 7.5 mL of DMF, mix them evenly, then add 2 g of PVDF, stir at 75 °C for 2 h to obtain PVDF@OTS-SiO2 coating suspension, i.e., SiO2 / PVDF hydrophobic self-cleaning solution.
[0072] Coating performance test Add the prepared coating suspension into the liquid carrier barrel of the spray gun, adjust the position of the spray gun so that it is perpendicular to the surface of the glass substrate treated with piranha lotion, adjust the spray gun pressure to 10PSI, keep the distance between the spray gun nozzle and the glass substrate at about 8-10cm, and move the spray gun at a speed of about 3cm / s; spray the glass sheet, try to ensure that the above coating suspension covers the glass sheet evenly, dry it at room temperature, and then spray the next time. Repeat the above operation 3 times, and the drying time after each spraying is 1-2min. After the last spraying, place the glass sheet in a muffle furnace and bake it at 230℃ for 40min to obtain a hydrophobic self-cleaning coating.
[0073] Comparative Example 1 A coating solution preparation method of this embodiment includes the following steps: 7.5 mL of DMF and 2 g of PVDF were stirred at 70-75° C. for 2-2.5 h to prepare a PVDF coating suspension.
[0074] Coating performance test Add the prepared coating suspension into the liquid carrier barrel of the spray gun, adjust the position of the spray gun so that it is perpendicular to the surface of the glass substrate treated with piranha lotion, adjust the spray gun pressure to 10PSI, keep the distance between the spray gun mouth and the glass substrate at about 8-10cm, and the spray gun moves at a speed of about 3cm / s; spray the glass sheet, try to ensure that the above coating suspension covers the glass sheet evenly, dry it at room temperature, and then spray the next time. Repeat the above operation 3 times, and the drying time after each spraying is 1-2min. After the last spraying, place the glass sheet in a muffle furnace and bake it at 230℃ for 40min. A hydrophobic self-cleaning coating is obtained. Its hydrophobic angle reaches 92.7°, the transmittance reaches 81%, and the pencil hardness is 6H.
[0075] Implementation effect example The hydrophobic angles of the hydrophobic self-cleaning coatings prepared in Examples 1-4 and Comparative Example 1 were tested respectively: a contact angle meter was used to measure the contact angles of water droplets on composite hydrophobic coatings with different ratios, and deionized water was dripped on the sample surface with a syringe to characterize the size of the water contact angle of the hydrophobic coating on the sample surface.
[0076] result Figure 1As shown, the contact angles of the coatings obtained by adding (0mL, 1mL, 2mL, 3mL, 4mL) of OTS-SiO2 solution to Comparative Example 1 and Examples 1-4 are 92.7°, 103.2°, 108.5°, 115.9°, and 111.1°, respectively. It can be seen from the figure that as the content of OTS-SiO2 solution increases, the water contact angle increases in ad, and decreases again in e. Due to the micro-nano rough structure on the surface of the PVDF@OTS-SiO2 coating, water droplets have a water contact angle on the coating, and within a certain range, the increase in the content of SiO2 particles increases the roughness of the coating, which increases the contact angle of water droplets on the coating, but excessive content of SiO2 particles will reduce the roughness, thereby reducing the contact angle.
[0077] Self-cleaning performance test analysis The self-cleaning and dust-removing performance of the composite coating was tested by coating dust on the surface of a glass slide, placing the coated side of the glass slide upward at an inclination angle of 35°, and then dropping water drops from one end at a high point.
[0078] like Figure 2 As shown, a is an uncoated bare glass slide, and bf are glass slides sprayed with PVDF@OTS-SiO2 coatings with OTS-SiO2 solution added in amounts of 0mL, 1mL, 2mL, 3mL, and 4mL, respectively. As can be seen from the figure, compared with the uncoated bare glass slide, the water droplets on the glass slide sprayed with PVDF@OTS-SiO2 coatings carry away the dust and present a clear water mark on it, and the glass slide presents a clean surface where the water droplets flow. The reason is that when water droplets roll on the inclined surface, small vortices will be generated on the hydrophobic coating, and the debris on the coating surface will be carried to the front of the water droplets by the vortices and carried away by the water droplets, thus presenting a self-cleaning effect.
[0079] Transmittance test analysis The transmittance of hydrophobic coatings with different ratios was measured at room temperature using a UV-visible spectrophotometer with a wavelength range of 300-1100nm, and the instrument was calibrated by running empty. The transmittance of PVDF@OTS-SiO2 hydrophobic coatings prepared with different OTS-SiO2 solution addition amounts (0mL, 1L, 2mL, 3mL, 4mL) was measured.
[0080] like Figure 3 The figure shows the transmittance of a bare glass slide and the transmittance of a glass slide sprayed with a PVDF@OTS-SiO2 composite coating with 0mL, 1mL, 2mL, 3mL, and 4mL of OTS-SiO2 solution added. Figure 3It can be seen that the transmittance of the bare glass slide without spraying the hydrophobic coating is about 91%, and the ae transmittance is about 81%, 79%, 75%, 68%, and 67%, respectively. With the increase of the amount of OTS-SiO2 added, the transmittance of the coating tends to decrease. This is because the increase in the amount of OTS-SiO2 added will increase the roughness of the coating, but its dispersion density on the glass slide will also increase, resulting in some loss of transmittance. When the amount of OTS-SiO2 solution added is 2mL, the prepared composite coating takes into account both hydrophobicity and transmittance, and has the best comprehensive performance.
[0081] Pencil Hardness Test Analysis The hardness of the hydrophobic coating was evaluated by the standard test method of coating performance, and the maximum hardness of the pencil lead that the coating could withstand was tested (from soft to hard, it was divided into 6B-6H). The pencil hardness of the PVDF@OTS-SiO2 coating on the glass slide with different OTS-SiO2 addition amounts measured reached 6H. Polyvinylidene fluoride (PVDF) has low surface energy, excellent inherent wear resistance and self-lubricating properties. Therefore, by adding polyvinylidene fluoride (PVDF) to improve the durability and friction resistance of the coating, the highly durable nano-SiO2 / PVDF hydrophobic self-cleaning coating required by the present invention was obtained.
[0082] Infrared spectroscopy The chemical composition of the surface of each sample was analyzed by FT-IR spectroscopy, such as Figure 4 This is the ATR-FTIR spectrum of the hydrophobic silica film. The infrared spectra of the composite coatings with different OTS-SiO2 additions have the same trend of change. Different peaks represent different vibration particles. Due to the stretching vibration of the Si-O-Si bond, the spectrum at 1050cm -1 There is an absorption band near 3100cm -1 The -OH absorption peak is near the surface, indicating the generated network structure of nano-silica at a wave number of 2850 cm -1 and 2923cm -1 The -CH2 and -CH3 stretching vibrations of OTS are nearby, indicating that the hydrophobic methyl group is grafted onto the mesh nano-silica, successfully modifying the silica and achieving the purpose of hydrophobic coating. It can be seen from the figure that the infrared spectrum is at 1460-1400cm -1There is a CF bond stretching vibration peak nearby, which shows that PVDF and nano-SiO2 are successfully combined. The binding force between PVDF and OTS-SiO2 is mainly the result of the combined action of chemical bonds and intermolecular forces. Chemical bond: Since the chemical structure of PVDF contains F-C bonds, this bond has the nature of a short bond and can form the most stable and firm bond. The formation of this chemical bond may react with the chemical groups on the surface of SiO2, thereby enhancing the binding force between the two. Intermolecular force: In addition to chemical bonds, the binding between PVDF and SiO2 may also rely on intermolecular forces, such as van der Waals forces, hydrogen bonds, etc. It helps to construct a micro-nano structure on the surface of the coating and form a stable coating structure, thereby enhancing the wear resistance of the coating. It can be seen from the figure that the infrared spectrum is at 1460-1400cm -1 There is a CF bond stretching vibration peak nearby, which shows that PVDF and nano-SiO2 are successfully combined.
[0083] Surface morphology analysis This method uses the Michelson interference principle, uses white light as the light source, and uses a white light interferometer to test the roughness of the coating. Figure 5 As shown in the figure, ae are white light interference patterns of glass slides sprayed with PVDF@OTS-SiO2 composite coatings with OTS-SiO2 solution addition amounts of 0mL, 1mL, 2mL, 3mL, and 4mL, respectively. As can be seen from the figure, micro-nano-scale bulges of different sizes and heights appear closely in the ae figure, indicating that the coatings have a certain rough structure, making the composite coating hydrophobic. It can be seen from the figure that the RA of ae is 781nm, 787nm, 844nm, 1615nm, and 1309nm, respectively. The RA increases first and then decreases, and the maximum is 1615nm at d, indicating that the roughness of the coating increases with the increase of SiO2, and begins to decrease after reaching a certain level. The reason is that SiO2 nanoparticles can improve the surface roughness of the PVDF coating. The enhancement of the surface roughness is mainly attributed to the agglomeration of SiO2 nanoparticles. Therefore, the hydrophobicity of the PVDF@OTS-SiO2 composite coating is the best when the OTS-SiO2 solution addition amount is 3mL.
[0084] Coating reflectivity analysis like Figure 6As shown in the figure, the reflectivity of the coating under different OTS-SiO2 solution addition amounts in the visible light range was tested, where a is blank glass, and bf are PVDF@OTS-SiO2 coated glasses with 0mL, 1mL, 2mL, 3mL, and 4mL of OTS-SiO2 solution added, respectively. From the data analysis, it can be seen that the SiO2 content will affect the reflectivity of the hydrophobic coating, and the reflectivity is lowest when OTS-SiO2 is not added. In the PVDF@OTS-SiO2 coating coated with different contents of OTS-SiO2 solution, with the increase of OTS-SiO2 addition, the reflectivity of the coating shows an upward trend, and the reflectivity in e reaches a maximum of 7.4%, so its transmittance is also affected. This is because the main function of PVDF is to enhance the adhesion ability of the coating and provide low surface energy, and the relationship between adhesion and transmittance is contradictory, so it will affect the transmittance of the coating, thereby increasing the reflectivity.
[0085] Analysis of solar energy conversion efficiency In this experiment, a glass slide coated with PVDF@OTS-SiO2 was placed on a photovoltaic panel and its photovoltaic performance was analyzed using a solar cell analyzer. Figure 7 As shown, they are bare glass slides without spraying, and S1-S5 are the photovoltaic performance of glass slides sprayed with PVDF@OTS-SiO2 coatings with OTS-SiO2 solution addition amounts of 0mL, 1mL, 2mL, 3mL, and 4mL, respectively.
[0086] Depend on Figure 7 -a shows that the photovoltaic current decreases slowly with the increase of voltage, and then decreases rapidly to 0 at 3-4.5V. Among them, the current of S2 is significantly larger than that of other contents when the voltage is relatively small. Figure 7 -b shows that the photovoltaic power increases with the increase of voltage, first slowly increases around 3-4.8V, and then rapidly decreases until it reaches 0. As can be seen from the figure, the photovoltaic performance of the coated glass slide does not change significantly compared with the bare glass slide, indicating that the coating will not affect the solar energy conversion efficiency of the glass slide too much.
[0087] Mechanism diagram analysis like Figure 8 As shown, the -(CH2)7CH3 group obtained by hydrolyzing n-octyltriethoxysilane is grafted onto nano-SiO2 by a grafting method, and the hydroxyl group of the nano-silica side chain is modified into a hydrophobic -(CH2)7CH3, making the nano-SiO2 modified and thus hydrophobic. It can be seen that the modification of nano-SiO2 is successful.
[0088] SEM analysis After PVDF is dissolved, the solution viscosity is very high and a coating structure will be formed. When PVDF is not added, the scanning image of nano-SiO2 should be a regular agglomeration structure, such as Fig. 9 As shown, the structure is irregular, and it can be seen that PVDF encapsulates nano-SiO2 to form a coating structure.
[0089] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a SiO2 / PVDF hydrophobic self-cleaning coating solution, characterized in that: Here are the steps: (1) Dispersing nano-SiO2 in a mixed solution of ammonia water and anhydrous ethanol to obtain SiO2 dispersed ammonia solution; (2) After OTS and anhydrous ethanol are mixed, they are stirred evenly under the acidic conditions provided by glacial acetic acid to obtain an OTS modified solution; (3) mixing the SiO2 dispersed ammonia solution of step (1) and the OTS modified solution of step (2), and heating and stirring to perform reaction I to obtain an OTS-SiO2 solution; (4) DMF is added to the OTS-SiO2 solution of step (3), and after mixing, PVDF is added, and after heating and stirring, a PVDF@OTS-SiO2 coating suspension is obtained, i.e., a SiO2 / PVDF hydrophobic self-cleaning solution.
2. The method for preparing the SiO2 / PVDF hydrophobic self-cleaning coating solution according to claim 1, characterized in that: In the step (1), the concentration of SiO2 in the SiO2 dispersed ammonia solution is 0.01-0.1 g / mL, and the particle size of SiO2 is 12 nm; the volume ratio of ammonia water to anhydrous ethanol in the SiO2 dispersed ammonia solution is 1:2-10.
3. The method for preparing the SiO2 / PVDF hydrophobic self-cleaning solution according to claim 2, characterized in that: In the step (2), the volume ratio of OTS to anhydrous ethanol is 1:10-100.
4. The method for preparing the SiO2 / PVDF hydrophobic self-cleaning coating solution according to claim 1, characterized in that: In the step (3), the volume ratio of the SiO2 dispersed ammonia solution to the OTS modified solution is 1:0.5-10.
5. The method for preparing the SiO2 / PVDF hydrophobic self-cleaning coating solution according to any one of claims 1 to 4, characterized in that: The reaction temperature of the heating and stirring reaction I is 40-45° C. and the reaction time is 12-15 h.
6. The method for preparing the SiO2 / PVDF hydrophobic self-cleaning coating solution according to claim 5, characterized in that: In the step (4), the volume ratio of the OTS-SiO2 solution to DMF is 1-4:7.5; the addition ratio of the OTS-SiO2 solution to PVDF is 0.5-2 mL of OTS-SiO2 solution per g of PVDF.
7. The method for preparing the SiO2 / PVDF hydrophobic self-cleaning coating solution according to claim 6, characterized in that: The reaction temperature of the heating and stirring reaction II is 70-75° C. and the reaction time is 2-2.5 h.
8. The SiO2 / PVDF hydrophobic self-cleaning coating solution prepared by the method of claim 5 or 6.
9. The SiO2 / PVDF hydrophobic self-cleaning coating prepared by using the SiO2 / PVDF hydrophobic self-cleaning coating solution according to claim 8, characterized in that: The SiO2 / PVDF hydrophobic self-cleaning coating has self-cleaning performance, a light transmittance of 67%-81%, and a hydrophobic angle of 103°-115.9°.
10. Use of the SiO2 / PVDF hydrophobic self-cleaning coating solution according to claim 9 in preparing coatings for protecting photovoltaic equipment, precision equipment, aerospace vehicles, automobile fields and electronic equipment.
Citation Information
Patent Citations
Wear-resistant super-hydrophobic coating compound
CN106634064A
An ultra-hydrophobic polymer microporous membrane and a preparing method thereof
CN107349803A
Wear-resisting super-hydrophobic coating composition as well as preparation method and application thereof
CN107987675A
Cited By
A fluorine-free transparent self-cleaning solid lubricating coating and a method for preparing the same
CN119823644B