Zinc-rich coating containing modified mixed compound epoxy resin as well as preparation method and application of zinc-rich coating
By adding polyaniline and silane coupling agents to zinc-rich coatings to treat zinc powder, combined with a variety of fillers and curing agents, the problems of high coating costs and difficulty in construction caused by high zinc powder content are solved, and the adhesion of the coating is improved. and anti-corrosion properties, reducing the risk of zinc poisoning and the hazards of zinc oxide mist during welding, achieving more convenient construction and better coating performance.
Patent Information
- Application Number
- CN202410988842.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-11
AI Technical Summary
The high content of zinc powder in existing zinc-rich coatings results in high coating costs, difficult construction, and the coating is easily porous and has low adhesion, which affects the anti-corrosion performance, and also causes zinc poisoning in the human body and the hazards of zinc oxide mist during welding.
Polyaniline is added to the epoxy zinc-rich coating, and the epoxy resin is mixed and compounded through modification to reduce the zinc powder content. A silane coupling agent is used for surface treatment of zinc powder and polyaniline, and a variety of fillers and curing agents are used. Improve paint adhesion and anti-settling properties.
It effectively reduces the zinc powder content, improves the adhesion and anti-corrosion performance of the coating, reduces the risk of zinc poisoning and the hazards of zinc oxide mist during welding, and provides more convenient construction conditions and better coating performance.
Smart Images

Figure CN118755359A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to epoxy resin, in particular to a zinc-rich coating containing a modified mixed compound epoxy resin and a preparation method and application thereof. Background Art
[0002] Epoxy zinc-rich paint is a heavy-duty anti-corrosion paint with excellent corrosion resistance. It is currently the most widely used type of paint for steel structure anti-corrosion. It forms a zinc protective coating on the surface of the steel structure through the high adhesion of epoxy resin, and uses metal zinc as a sacrificial anode to protect the steel structure, preventing the steel structure from being eroded by the corrosive environment, thereby increasing the service life of the steel structure.
[0003] The anti-corrosion performance of zinc-rich coatings increases with the increase of zinc content. However, high content of zinc powder in the coating will increase the coating cost and zinc powder sedimentation and stratification, increase the difficulty and cost of coating construction. In addition, the coating obtained is prone to be porous and has low adhesion, which affects the bonding force between the upper coating and the zinc-rich coating, reduces the anti-corrosion performance of the coating, and affects its service life and safety.
[0004] Moreover, zinc-rich paints come into contact with large amounts of zinc powder during the preparation process, which increases the risk of zinc poisoning in the human body. In addition, zinc in zinc-rich paints is a sacrificial anode, and when welding on steel structures protected by zinc-rich paints, a large amount of zinc oxide mist will be generated, endangering the life and health of the workers. Summary of the invention
[0005] The present invention aims to provide a zinc-rich coating containing a modified mixed compound epoxy resin and a preparation method and application thereof. By adding polyaniline to the epoxy zinc-rich coating, the content of zinc powder in the coating is greatly reduced, the sedimentation and stratification phenomenon of the zinc powder coating is effectively improved, and performance indicators such as adhesion are also improved.
[0006] To achieve the above purpose, the present invention adopts the following technical methods:
[0007] The invention discloses a zinc-rich coating containing a modified mixed compound epoxy resin. The coating is composed of a main agent and a curing agent, wherein the main agent and the curing agent are in a mass ratio of 10:8-10:5. The main agent comprises, by weight percentage, 50%-60% of the modified mixed compound epoxy resin, 5%-8% of PANI, 5%-10% of zinc powder, 2%-7% of silicon dioxide (g), 1%-4% of barium sulfate, 2%-10% of zirconium dioxide, 3%-7% of mica powder, 1%-4% of titanium dioxide, 1%-4% of glass flakes, 0.5%-2% of mica iron oxide ash, 1%-4% of bentonite, and 10%-15% of a solvent.
[0008] The modified mixed compound epoxy resin is prepared by adding a xylene-n-butanol solvent system to the epoxy resin under stirring conditions in a dispersion plate to dilute and dissolve the epoxy resin to a solid content of 70-75%, then adding a bisphenol F epoxy resin to mix, and then cooling to room temperature for standby use; wherein the mass percentage of the epoxy resin to the bisphenol F epoxy resin is 7:3; and the volume ratio of xylene to n-butanol in the xylene-n-butanol solvent system is 2:1.
[0009] The bisphenol F epoxy resin is YDF-170; the epoxy resin is E51.
[0010] The zinc powder is prepared by soaking the zinc powder in xylene, filtering the zinc powder, adding a silane coupling agent to the zinc powder for surface treatment, and setting aside for use;
[0011] The PANI is prepared by soaking the PANI in a silane coupling agent, and then adding methyl isobutyl ketone to the centrifugal precipitate for surface treatment, and the precipitate is ready for use.
[0012] The silane coupling agent used in the above zinc powder treatment is KH560.
[0013] The silane coupling agent used in the above PANI treatment is KH560.
[0014] The curing agent is prepared by mixing two phenolic amine resins in a mass ratio of 3:2, and then diluting and dissolving the resins with a solvent until the solid content of the system is 80-85% for standby use; wherein the solvent is xylene and n-butanol mixed in a volume ratio of 2:1.
[0015] A method for preparing the zinc-rich coating containing a modified mixed compound epoxy resin,
[0016] 1) Surface treatment of zinc powder: fully immerse the zinc powder in xylene, filter it, add silane coupling agent to the zinc powder for surface treatment, and set aside;
[0017] 2) Surface treatment of polyaniline (PANI): fully immerse PANI in a silane coupling agent, filter and add methyl isobutyl ketone to PANI for dispersion treatment, and set aside;
[0018] 3) Mix fillers (silicon dioxide, barium sulfate, zirconium dioxide, mica powder, titanium dioxide, glass flakes, mica iron oxide ash, bentonite) and part of the modified epoxy resin (A), add a mixed solvent of xylene and n-butanol (volume ratio = 2:1), pre-disperse for 2 to 3 minutes at a speed of 3000 rpm, and then pour into a sand mill for grinding for 30 to 40 minutes. After grinding, discharge the material to obtain a color paste component;
[0019] The color paste component obtained as above is added to the remaining modified epoxy resin (A), pre-dispersed at a rotation speed of 1000-1200 rpm for 5-8 minutes, then PANI obtained in the above step 2) is added, dispersed at a rotation speed of 2000-2500 rpm for 10-13 minutes, and then zinc powder obtained in the above step 1) is added, and dispersed at a rotation speed of 3000-3500 rpm for 30-35 minutes to obtain a main agent;
[0020] 4) Mix two phenolic amine resins, NX5594 and NX5556M, in a mass ratio of 3:2, and dilute and dissolve the resins with a solvent to a solid content of 80-85% as a curing agent; wherein the solvent is a mixture of xylene and n-butanol in a volume ratio of 2:1;
[0021] 5) When using, mix the main agent and curing agent obtained above in a mass ratio of 10:8 to 10:5.
[0022] An application of the zinc-rich coating, wherein the zinc-rich coating is used as a carbon steel substrate in the field of corrosion protection.
[0023] The invention has the advantages that by introducing polyaniline into the coating, the content of zinc powder in the coating is greatly reduced, and the sedimentation and stratification phenomenon of the zinc powder coating is effectively improved. While providing convenience for on-site construction, it also reduces the potential danger to the life and health of operators caused by excessive zinc content in the zinc powder coating (zinc poisoning, toxic zinc oxide mist generated during welding operations, etc.) BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the mechanism by which filler glass flakes play an anti-corrosion role in coatings. DETAILED DESCRIPTION
[0025] The present invention is further described in detail below in conjunction with specific implementation modes.
[0026] Example 1
[0027] Preparation method of modified mixed compound epoxy resin and zinc-rich and polyaniline coating:
[0028] (1) Add 13g of polyaniline (PANI) solid powder into a tin can containing 50ml of KH560 silane coupling agent, ensuring that the polyaniline is completely covered by the coupling agent. Soak and place at room temperature for 12 hours, then filter, and then use centrifugation (4000rmp, 30min) to remove excess KH560. Add about 20g of methyl isobutyl ketone to the obtained centrifugal precipitate, and shake and mix thoroughly to fully wet the surface of the polyaniline;
[0029] (2) Soak 13 g of metallic zinc powder (300 mesh) in 50 ml of xylene to ensure that the zinc powder is completely covered by xylene. After soaking for 2 h, filter out excess xylene, add about 25 g of KH560 silane coupling agent, shake and mix thoroughly to wet the surface of the zinc powder, let stand for 12 h, and centrifuge (4000 rpm, 30 min) to remove excess KH560.
[0030] (3) The modified epoxy resin is prepared by adding a xylene-n-butanol solvent system to epoxy E51 resin under stirring conditions on a dispersion plate to dilute and dissolve the epoxy resin to 70% solid content, then adding YDF-170 resin to mix, and then cooling to room temperature for standby use; wherein the mass percentage of epoxy resin to YDF-170 resin is 7:3; and the volume ratio of xylene to n-butanol in the xylene-n-butanol solvent system is 2:1.
[0031] (4) Add 30 g of a mixed solvent of xylene and n-butanol (volume ratio 2:1) to 100 g of the prepared modified epoxy resin (component A), pre-disperse for 2 to 3 minutes at a speed of 1000 rpm, and then add silicon dioxide (g): 3 g, barium sulfate: 1.5 g, zirconium dioxide: 5 g, mica powder: 5 g, titanium dioxide: 5 g, glass flakes: 5 g, mica iron oxide ash: 0.8 g, bentonite: 3 g in sequence. After all are added to the disperser, adjust the speed to 3500 rpm in stages, disperse for 35 minutes, and after the dispersion is completed, introduce the material into a grinder and grind for 2 hours. After the grinding is completed, discharge the material and connect it to the barrel;
[0032] (5) pre-dispersing the color paste prepared in the above step (4) at a rotation speed of 1200 rpm for 3 minutes, then adding 13 g of PANI obtained in the above step (1) and 13 g of zinc powder obtained in the above step (2), and further dispersing at a rotation speed of 3500 rpm for 30 minutes to obtain a main agent;
[0033] (6) Two phenolic amine resins, NX5594 and NX5556M, are mixed in a mass ratio of 3:2. After mixing, the resins are diluted and dissolved with a solvent until the solid content of the system is 80%, thereby obtaining a curing agent; wherein the solvent is a mixture of xylene and n-butanol in a volume ratio of 2:1.
[0034] The main agent obtained above and the curing agent (component B) are mixed in a ratio of 4:3 (mass ratio), stirred evenly to obtain a two-component coating, and then the obtained coating is sprayed / brushed on the surface of a carbon steel substrate.
[0035] The coating prepared by this formula takes 12 hours to dry, and the surface is flat, dense, and slightly glossy. Then refer to the following standards:
[0036] GB / T9286-1998 (paint film scratch test);
[0037] GB / T 6379-1996 (Determination of pencil hardness of paint film);
[0038] GB / T 1732—1993 (Determination of impact resistance of paint films);
[0039] GB / T 1731—1993 (Determination of paint film flexibility);
[0040] GB / T 1771-2007 (Determination of neutral salt spray resistance of paints and varnishes);
[0041] The coating performance was tested, with adhesion of level 0 using the cross-hatch method, pencil hardness of 3H, impact resistance greater than 50cm (500g), flexibility of 3mm, and after 2500h of the neutral salt spray test, rust spots appeared locally at the scratches on the coating surface, and the overall coating surface did not change much.
[0042] Comparative Example 1
[0043] A common epoxy zinc-rich primer on the market, its main ingredients include: epoxy E44 resin, zinc powder, ethyl silicate and corresponding fillers, auxiliary thickeners, etc. The mass ratio of the main agent to the curing agent is 3:1.
[0044] Comparative Example 2
[0045] (1) Add 10g of polyaniline (PANI) solid powder into a tin can containing 50ml of KH560 silane coupling agent, ensuring that the polyaniline is completely covered by the coupling agent. Soak and place at room temperature for 12 hours, then filter, and then use centrifugation (4000rmp, 30min) to remove excess KH560. Add about 15g of methyl isobutyl ketone to the obtained centrifugal precipitate, and shake and mix thoroughly to fully wet the surface of the polyaniline;
[0046] (2) Soak 20 g of metallic zinc powder (300 mesh) in 50 ml of xylene to ensure that the zinc powder is completely covered by xylene. After soaking for 2 h, filter out excess xylene, add about 20 g of KH560 silane coupling agent, shake and mix thoroughly to wet the surface of the zinc powder, let stand for 12 h, and centrifuge (4000 rpm, 30 min) to remove excess KH560.
[0047] (3) The modified epoxy resin is prepared by adding a xylene-n-butanol solvent system to epoxy E51 resin under stirring conditions on a dispersion plate to dilute and dissolve the epoxy resin to 70% solid content, then adding YDF-170 resin to mix, and then cooling to room temperature for standby use; wherein the mass percentage of epoxy resin to YDF-170 resin is 7:3; and the volume ratio of xylene to n-butanol in the xylene-n-butanol solvent system is 2:1.
[0048] (4) Add 20 g of a mixed solvent of xylene and n-butanol (volume ratio 2:1) to 100 g of the prepared modified epoxy resin (component A), pre-disperse for 3 minutes at a speed of 1000 rpm, and then add silicon dioxide (g): 3 g, barium sulfate: 1.5 g, zirconium dioxide: 3 g, mica powder: 5 g, titanium dioxide: 5 g, glass flakes: 3 g, mica iron oxide ash: 0.8 g, bentonite: 3 g in sequence. After all are added to the disperser, adjust the speed to 3500 rpm in stages, disperse for 35 minutes, and after the dispersion is completed, introduce the material into a grinder and grind for 2 hours. After the grinding is completed, discharge the material and connect it to the barrel;
[0049] (5) pre-dispersing the color paste prepared in the above step (4) at a rotation speed of 1200 rpm for 3 minutes, then adding 10 g of PANI obtained in the above step (1) and 20 g of zinc powder obtained in the above step (2), and further dispersing at a rotation speed of 3500 rpm for 30 minutes to obtain a main agent;
[0050] (6) Two phenolic amine resins, NX5594 and NX5556M, are mixed in a mass ratio of 3:2. After mixing, the resins are diluted and dissolved with a solvent until the solid content of the system is 80%, thereby obtaining a curing agent; wherein the solvent is a mixture of xylene and n-butanol in a volume ratio of 2:1.
[0051] The main agent obtained above and the curing agent (component B) are mixed at a mass ratio of 2:1, and stirred evenly to obtain a two-component coating, and then the obtained coating is sprayed / brushed on the surface of a carbon steel substrate.
[0052] Comparative Example 3
[0053] (1) Add 20g of polyaniline (PANI) solid powder into a tin can containing 50ml of KH560 silane coupling agent, ensuring that the polyaniline is completely covered by the coupling agent. Soak and place at room temperature for 12 hours, then filter, and then use centrifugation (4000rmp, 30min) to remove excess KH560. Add about 30g of methyl isobutyl ketone to the obtained centrifugal precipitate, and shake and mix thoroughly to make the surface of the polyaniline completely wet;
[0054] (2) Soak 10 g of metallic zinc powder (300 mesh) in 50 ml of xylene to ensure that the zinc powder is completely covered by xylene. After soaking for 2 h, filter out excess xylene, add about 15 g of KH560 silane coupling agent, shake and mix thoroughly to wet the surface of the zinc powder, let stand for 12 h, and centrifuge (4000 rpm, 30 min) to remove excess KH560.
[0055] (3) The modified epoxy resin is prepared by adding a xylene-n-butanol solvent system to epoxy E51 resin under stirring conditions on a dispersion plate to dilute and dissolve the epoxy resin to 70% solid content, then adding YDF-170 resin to mix, and then cooling to room temperature for standby use; wherein the mass percentage of epoxy resin to YDF-170 resin is 7:3; and the volume ratio of xylene to n-butanol in the xylene-n-butanol solvent system is 2:1.
[0056] (4) Add 20 g of a mixed solvent of xylene and n-butanol (volume ratio 2:1) to 100 g of the prepared modified epoxy resin (component A), pre-disperse for 3 minutes at a speed of 1000 rpm, and then add silicon dioxide (g): 2 g, barium sulfate: 0.5 g, zirconium dioxide: 3 g, mica powder: 3 g, titanium dioxide: 5 g, glass flakes: 3 g, mica iron oxide ash: 2.8 g, bentonite: 3 g in sequence. After all are added to the disperser, adjust the speed to 3500 rpm in stages, disperse for 35 minutes, and after the dispersion is completed, introduce the material into a grinder and grind for 2 hours. After the grinding is completed, discharge the material and connect it to the barrel;
[0057] (5) pre-dispersing the color paste prepared in the above step (4) at a rotation speed of 1200 rpm for 3 minutes, then adding 20 g of PANI obtained in the above step (1) and 10 g of zinc powder obtained in the above step (2), and further dispersing at a rotation speed of 3500 rpm for 30 minutes to obtain a main agent;
[0058] (6) Two phenolic amine resins, NX5594 and NX5556M, are mixed in a mass ratio of 3:2. After mixing, the resins are diluted and dissolved with a solvent until the solid content of the system is 80%, thereby obtaining a curing agent; wherein the solvent is a mixture of xylene and n-butanol in a volume ratio of 2:1.
[0059] The main agent obtained above and the curing agent (component B) are mixed at a mass ratio of 2:1, and stirred evenly to obtain a two-component coating, and then the obtained coating is sprayed / brushed on the surface of a carbon steel substrate.
[0060] According to the above-mentioned coating preparation and coating application process, several coatings were obtained, and then the relevant performance evaluation of each coating obtained was listed in Table 1 below.
[0061]
[0062]
[0063] Comparative Example 1 is an epoxy zinc-rich coating circulated in the market. Referring to the above table, it can be concluded from the comparison with the example that the introduction of polyaniline in the present invention reduces the zinc powder content in the coating while improving the adhesion. The synergistic effect of zinc powder and polyaniline also greatly improves the salt spray resistance of the coating.
[0064] Comparative Examples 2 and 3 are coatings prepared by changing the content of zinc powder and polyaniline. It can be concluded from the comparative analysis that a unilateral increase in either the zinc powder content or the PANI content will have a negative impact on the coating performance.
[0065] The combination of the coating anti-settling agent in the present invention is fumed silica and bentonite; the glass flakes play a role in strengthening the hardness and wear resistance of the coating in the coating main agent system. Due to the low permeability of the glass flakes, the coating can be enhanced against the corrosion medium resistance (such as Figure 1 ) and because of its high adhesion to the resin matrix, the overall unity of the coating is enhanced, which can reduce the tendency of the coating to be damaged to a certain extent; the addition of zirconium dioxide improves the heat and salt water resistance of the epoxy resin coating and enhances its crack resistance; and the addition of mica powder, silica and other powders can improve the mechanical and anti-corrosion properties of the coating, greatly improving the adhesion and toughness of the coating.
[0066] In summary, the present invention increases the flexibility and strength of the resin by compounding two modified epoxy resins, improves the tolerance of the resin to zinc powder, reduces the content ratio of zinc powder in the coating system by adding and using PANI, solves the unfavorable factors such as easy sedimentation of the coating system after adding zinc powder, reduced adhesion of the prepared coating, and brittle coating; at the same time, the surface of the zinc powder is pretreated by a silane coupling agent to further improve the compatibility of the zinc powder with the modified epoxy resin; multiple stabilizers are selected for combined use to solve the dispersion and stability problem of zinc powder and polyaniline in the modified epoxy resin; the compounded epoxy resin and the zinc-rich and polyaniline coating of the present invention are applied to the protection of carbon steel substrates, and have better chemical corrosion protection and physical protection and more convenient construction conditions compared with ordinary zinc-rich primers.
Claims
1. A zinc-rich coating containing a modified mixed compounded epoxy resin, characterized in that: The coating is composed of a main agent and a curing agent, and the mass ratio of the main agent to the curing agent is 10:8-10:5; wherein, the main agent, by weight percentage, is a modified mixed compound epoxy resin: 50%-60%, PANI: 5%-8%, zinc powder: 5%-10%, silicon dioxide (g): 2%-7%, barium sulfate: 1%-4%, zirconium dioxide: 2%-10%, mica powder: 3%-7%, titanium dioxide: 1%-4%, glass flakes: 1%-4%, mica iron oxide ash: 0.5%-2%, bentonite: 1%-4%, and solvent: 10%-15%.
2. The zinc-rich coating containing modified mixed compounded epoxy resin according to claim 1, characterized in that: The modified mixed compound epoxy resin is prepared by adding a xylene-n-butanol solvent system to the epoxy resin (E51) to dilute and dissolve the epoxy resin to 70-75% solid content under stirring conditions on a dispersion plate, then adding a bisphenol F epoxy resin (YDF-170) to mix, and then cooling to room temperature for standby use; wherein the mass percentage of the epoxy resin to the bisphenol F epoxy resin is 7:3; and the volume ratio of xylene to n-butanol in the xylene-n-butanol solvent system is 2:
1.
3. The zinc-rich coating containing modified mixed compounded epoxy resin according to claim 2, characterized in that: The bisphenol F epoxy resin is YDF-170; the epoxy resin is E51.
4. The zinc-rich coating containing modified mixed compounded epoxy resin according to claim 1, characterized in that: The zinc powder is prepared by soaking the zinc powder in xylene, filtering the zinc powder, adding a silane coupling agent to the zinc powder for surface treatment, and setting aside for use; The PANI is prepared by soaking the PANI in a silane coupling agent, and then adding methyl isobutyl ketone to the centrifugal precipitate for surface treatment, and the precipitate is ready for use.
5. The zinc-rich coating containing modified mixed compounded epoxy resin according to claim 1, characterized in that: The curing agent is prepared by mixing two phenolic amine resins in a mass ratio of 3:2, and then diluting and dissolving the resins with a solvent until the solid content of the system is 80-85% for standby use; wherein the solvent is xylene and n-butanol mixed in a volume ratio of 2:
1.
6. A method for preparing a zinc-rich coating containing a modified mixed compounded epoxy resin according to claim 1, characterized in that: The main agent and the curing agent are mixed according to the ratio described in claim 1.
7. An application of the zinc-rich coating according to claim 1, characterized in that: The zinc-rich coating is used in the field of corrosion protection for carbon steel substrates.
Citation Information
Patent Citations
Epoxy zinc-rich primer containing mica iron oxide and preparation method of epoxy zinc-rich primer
CN104830201A
Polyaniline-modified epoxy-zinc powder composite paint and preparation method
CN107099219A
Solvent-free epoxy zinc-rich anticorrosive paint and preparation method thereof
CN112500764A
Single-component scale type epoxy zinc-rich anti-corrosive primer and preparation method thereof
CN112920687A
Primer-topcoat type epoxy zinc powder coating and preparation method thereof
CN114045090A