Moss-preventing finish paint, building coating and building surface renovation method
By combining the principle of photocatalysis and the high alkalinity of cement in the architectural coating, a long-lasting anti-moss effect is formed, and through the combination of the interface treatment agent and the anti-moss topcoat, the poor anti-moss performance and poor aging resistance in the existing technology are solved. It achieves long-lasting anti-moss and high adhesion, and is suitable for building surfaces in humid and rainy areas.
Patent Information
- Application Number
- CN202410916633.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-11
AI Technical Summary
Existing moss prevention coatings and building surface renovation methods have problems such as poor long-lasting moss prevention performance, poor aging resistance, and poor moss prevention effect. It is especially difficult to prevent moss growth on roofs in humid and rainy areas for a long time.
A moss-preventive topcoat is used, including component A and B. It combines the photocatalytic principle with the high alkalinity of cement to form a long-lasting anti-moss antibacterial effect, and through the combination of the interface treatment agent and the moss-preventive topcoat, Improve the adhesion and aging resistance of the coating to form a long-lasting anti-moss architectural coating.
It achieves a long-lasting anti-moss effect, improves the powder resistance and adhesion of the coating, and ensures that moss will not grow on the building surface again. It is simple and convenient to operate and is suitable for different types of building surfaces.
Smart Images

Figure FT_1 
Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building repair, and in particular to a moss prevention topcoat, a building coating and a building surface renovation method. Background Art
[0002] Moss plants grow in clusters in trees, on the ground, on roofs, and in any ditch or crack where there is sufficient water and not too bright light. They reproduce by spores at the top of their stems. They are very tenacious. Even in "barren land" like the roof, the joints or tiny cracks of the roof materials are enough for moss spores that drift with the wind or come with bird excrement to settle down and grow. Because southern China is humid and rainy, the moisture content of the roof is high. If the house is not exposed to the sun for too long, the entire roof will be covered with moss. Since moss is also a plant, it will erode the roof material and expand the gaps between the roof materials during the process of attaching to the roof. If left unattended, the roof will have material shedding, water leakage, and large-scale damage. At this time, it is too late to think of cleaning the culprit "little moss", and the homeowner will pay a heavy price for this inconspicuous problem.
[0003] The existing removal method is to spray chemical agents to kill the moss. After their roots have lost their vitality and cannot firmly grasp the roofing materials, they can use high-speed water jets from high-pressure water guns to hit the moss to make it fall off. Even if the tile roof with moss is removed, the appearance will appear relatively old. For roofs in humid climates, the moss may grow again a few months after it has just been cleaned. Therefore, after the moss is removed, the tile surface needs to be renovated with paint to prevent moss growth. There are two main technical means to prevent moss growth: One is the photocatalytic coating, which is applied on the wall to make the attached moss spores float up and then carried away by rainwater. The advantage is that it has self-cleaning function and high anti-fouling. The disadvantage is that photocatalysis is not effective in places with poor sunlight. Currently, nano titanium dioxide is the most commonly used. Under photocatalysis, Ti4+ in titanium dioxide is easily reduced to Ti3+, releasing nascent oxygen. Because nascent oxygen has extremely strong reactivity, it can oxidize organic matter and kill moss spores on the surface. However, the organic matter (emulsion, organic color paste) of the paint base will also be oxidized, and its polymer chain will be broken or degraded, destroying the continuity of the coating, forming soluble or volatile substances, and the aging resistance of the coating is not good.
[0004] Secondly, additives to prevent mold growth are added to the paint. Even if spores are attached to the surface, they cannot reproduce. The advantage is that it is not affected by sunlight and has a significant effect in inhibiting mold. The disadvantage is that different anti-mold agents correspond to different types of fungi. If the incompatible fungi fall on the coating surface, they will still reproduce. In addition, anti-mold agents have poor aging resistance and are ineffective over time. Summary of the invention
[0005] In view of the above problems, one of the objects of the present invention is to provide a moss-preventing topcoat to solve the problem of poor long-lasting moss-preventing performance of existing coatings for preventing moss growth; a second object of the present invention is to provide a building coating to solve the problem of poor aging resistance of existing anti-moss coatings; a third object of the present invention is to provide a building surface renovation method to solve the problem of poor moss-preventing effect of existing renovation methods.
[0006] One of the purposes of the present invention is achieved through the following technical solutions: A moss prevention topcoat comprises: component A and component B. Component A comprises, by weight, 100-300 parts of water, 50-100 parts of nano titanium dioxide, 400-600 parts of acrylic emulsion, and 18-41 parts of a first auxiliary agent; and component B comprises, by weight, 200-300 parts of cement, 500-800 parts of a first inorganic filler, and 8-19 parts of a second auxiliary agent.
[0007] Preferably, the first auxiliary agent comprises, by mass, 1 to 3 parts of preservative, 1 to 3 parts of cellulose, 1 to 3 parts of wetting agent, 1 to 3 parts of dispersant, 2 to 4 parts of defoaming agent, 5 to 10 parts of film-forming agent, 5 to 10 parts of ethylene glycol, 1 to 2 parts of pH regulator, and 1 to 3 parts of thickener.
[0008] Preferably, the first inorganic filler comprises, by mass, 400-600 parts of wollastonite powder and 100-200 parts of quartz powder.
[0009] Preferably, the second auxiliary agent comprises, by mass, 1 to 3 parts of retarder, 1 to 3 parts of water repellent, 1 to 3 parts of anti-efflorescence auxiliary agent, and 5 to 10 parts of anti-cracking microspheres.
[0010] Preferably, the component A also includes 50 to 100 parts of inorganic pigments.
[0011] Preferably, the ratio of component A to component B is 1:1-2, the inorganic pigment is rutile titanium dioxide, the quartz powder is silica powder, the retarder is sodium citrate, and the cement is aluminum sulfate cement.
[0012] Preferably, the preparation method of component A comprises: Add water, preservative, defoamer, wetting agent and dispersant into the disperser, and stir and disperse at a first speed; Keeping the first speed, adding cellulose, pH adjuster, nano titanium dioxide, and inorganic pigment in sequence and stirring and dispersing at the second speed; The speed of the disperser is set to the third speed, and acrylic emulsion, film-forming aid, ethylene glycol, and thickener are added in sequence for stirring and dispersing; Wherein, the first rotation speed is 400-500 rpm, the second rotation speed is 1200-1800 rpm, and the third rotation speed is 800-1000 rpm.
[0013] The second object of the present invention is achieved by the following technical solutions: A building coating comprises: an interface layer coated on a building surface and a topcoat layer coated on the interface layer. The topcoat layer is formed by coating the moss prevention topcoat of the present invention, and the interface layer is formed by coating an interface treatment agent.
[0014] Preferably, the interface treatment agent comprises: component A and component B. Component A comprises, by weight, 400-600 parts of cationic acrylic resin and 400-600 parts of water; and component B comprises, by weight, 700-1100 parts of a second inorganic filler and 3-9 parts of a third auxiliary agent.
[0015] Preferably, the second inorganic filler comprises, by weight, 400-600 parts of wollastonite powder, 200-300 parts of cement, and 100-200 parts of quartz powder. The third auxiliary agent comprises, by weight, 1-3 parts of retarder, 1-3 parts of rheological agent, and 1-3 parts of defoamer.
[0016] Preferably, in the interface treatment agent: the ratio of the component A to the component B is 1:1-2, the quartz powder is selected from silicon micropowder, the cement is selected from aluminum sulfate cement, and the retarder is selected from sodium tetraborate decahydrate.
[0017] The third object of the present invention is achieved by the following technical solutions: A method for renovating a building surface comprises the following steps: S1: Remove moss from building surfaces; S2: applying the architectural coating of the present invention on the architectural surface.
[0018] By adopting the above technical solution, the beneficial effects of the present invention are as follows: (1) The anti-moss topcoat of the present invention utilizes the principle of photocatalysis and the high alkalinity of cement itself, and the coating film has a long-lasting anti-moss and antibacterial effect. In addition, it adopts an organic and inorganic bonding combination to delay the degradation of organic matter by nano-titanium dioxide and improve the anti-powdering property of the coating.
[0019] (2) The architectural coating of the present invention comprises an interface layer formed by coating an interface treatment agent and a topcoat layer formed by coating an anti-moss topcoat. The interface treatment agent and the anti-moss topcoat are combined to give the architectural coating excellent adhesion, aging resistance and durability, thereby achieving long-term anti-moss effect.
[0020] (3) The building surface renovation method of the present invention is used to renovate the building surface, which is simple and convenient to operate and can prevent moss from growing on the building surface again, thereby achieving long-term moss prevention. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Schematic diagram illustrating the principle of the moss removal method.
[0022] Wherein: 1. Building surface; 2. Coating film formed by spraying moss treatment paint; 3. Moss. DETAILED DESCRIPTION
[0023] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation methods.
[0024] The test methods and detection methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials are commercially available unless otherwise specified.
[0025] An embodiment of the present invention provides a method for renovating a building surface, which comprises the following steps: S1: Remove moss from building surfaces.
[0026] S2: Apply architectural coatings to building surfaces.
[0027] For step S1, the existing moss removal method can be used: first spray chemical agents to kill the moss, so that their roots lose vitality and cannot firmly grasp the building materials, and then use the high-speed water flow sprayed from the high-pressure water gun to hit the moss to make it fall off. This method is indeed effective for flat buildings such as flat roofs that are not tile roofs, and the moss can be removed very cleanly. However, if it is a tile roof, the tiles are laid in a staggered manner, and the high-pressure water will inevitably cause the tiles to deviate or even fall off due to the strong pressure, and the water will pass through the gaps in the tiles, causing leakage. And when the tile roof is covered with moss, it will become extremely slippery, and cleaning the roof is a relatively dangerous job.
[0028] Therefore, an embodiment of the present invention provides a more convenient and safe moss removal method, which includes: applying a moss treatment paint on the moss on the surface of the building, waiting for the paint to penetrate into the moss and form a film to kill the moss, then peeling off the coating film and uprooting the moss adhered to the coating film.
[0029] The moss treatment coating of the embodiment of the present invention comprises: a strippable coating and fibers and algaecides dispersed in the strippable coating. The fibers can increase the mechanical properties of the moss treatment coating, achieve a certain tear resistance, and improve its stripping performance and the bonding strength between the moss and the coating, so that the moss can be peeled off in pieces along with the coating. The algaecide can improve the effectiveness and efficiency of killing mosses. The algaecide is pre-embedded in the coating, which reduces the volatilization rate of the algaecide, maintains a long-lasting killing effect, and also reduces harm to the human body.
[0030] Combination Figure 1 After the moss treatment paint is sprayed on the moss 3 on the building surface 1, the paint not only penetrates into the roots of the moss 3, but also covers the surface layer of the moss 3, and kills the moss 3 by algaecide and isolating water vapor. The coating film 2 is transparent after drying, and the color change of the moss 3 can be clearly observed: green→yellow→gray. The coating film 2 has a balanced adhesion and peeling. After the moss 3 is killed, the coating film 2 can be easily peeled off in pieces, and the moss 3 adhered to the coating film 2 can be pulled out by the roots, without the need for additional washing and cleaning of the building surface 1, which causes less damage to the building surface and is more environmentally friendly.
[0031] The peelable coating of the embodiment of the present invention can be a commercially available product. The peelable coating can be divided into two types: solvent-based and water-based according to the different solvents used. It is preferred to use a water-based peelable coating to reduce the damage to the human body and the environment during use, such as polyvinyl alcohol peelable coating, polyurethane peelable coating, acrylate peelable coating, and silicone peelable coating, etc. The selection can be based on the specific application environment and requirements.
[0032] The fiber of the embodiment of the present invention is a short fiber with a length of 1 to 15 mm, preferably 1 to 2 mm. The fiber can be selected according to actual needs, and generally needs to have a certain strength, rigidity and toughness so as to effectively enhance the mechanical properties of the moss-treated coating, such as: one or more of natural fiber, artificial fiber, polyester fiber, polyamide fiber, polyurethane fiber, polyolefin fiber, polyvinyl alcohol fiber, polychloroolefin fiber, polyacrylonitrile fiber, polylactic acid fiber, polyphenylene sulfide fiber, fluorine-containing fiber, polyimide fiber, polyhydroxyalkanoate fiber, carbon fiber, ceramic fiber, glass fiber, mineral fiber and metal fiber.
[0033] Here, an embodiment of the present invention provides a preferred formula for a moss-treated coating, which includes, by mass: 400-600 parts of aliphatic polyurethane emulsion, 100-200 parts of water, 100-200 parts of algaecide, 10-20 parts of polypropylene fiber, 1-2 parts of defoamer, 1-2 parts of substrate wetting agent, and 3-10 parts of bentonite.
[0034] Sources of some of the above raw materials: Aliphatic polyurethane emulsion uses KB-525 from Youxinxin Material. It is water-based and environmentally friendly.
[0035] The algaecide used was LAMACIDE-TF / 037.ECO from La Marsa, Spain.
[0036] The preferred length of the polypropylene fiber is 1 to 2 mm and is purchased from Shandong Hongju Engineering Materials Co., Ltd.
[0037] The defoamer used is NXZ from Nopco.
[0038] The MW of the grid is selected for bentonite.
[0039] The substrate wetting agent used was Dow's BD405.
[0040] The preparation method of the moss-treated coating is as follows: water, substrate wetting agent and defoamer are added into a disperser, bentonite and polypropylene fiber are added under low-speed stirring, dispersed at high speed for 10 minutes, aliphatic polyurethane emulsion and algaecide are added after stopping the machine, and low-speed stirring is performed for 10 minutes to obtain the finished product.
[0041] Table 1 shows four specific experimental examples of moss-treated coatings according to the embodiments of the present invention.
[0042] Table 1
[0043] The performance indicators met by the above moss treatment coating are shown in Table 2: Table 2
[0044] Indicator Description: The tensile breaking strength is tested according to Method A of GB / T328.9-2007, the purpose of which is to examine the force required to break the paint film.
[0045] The peeling adhesion with the tile surface is carried out according to the method in Appendix A of JG / T375-2012. The lower the force value, the easier the paint film is to peel off.
[0046] The moss inactivation time was the time required to observe the moss color change from green to yellow or gray.
[0047] It is understandable that the moss removal method of the embodiment of the present invention is not only applicable to removing moss, but also applicable to removing algae attached to the surface of the building, such as lichens, etc. The moss removal method of the embodiment of the present invention is applicable to the building surfaces such as the ground, flat roof, wall, etc., and is particularly applicable to the tile surface.
[0048] For step S2, an embodiment of the present invention provides a building coating, which includes an interface layer coated on the building surface and a topcoat layer coated on the interface layer, wherein the topcoat layer is formed by coating a moss prevention topcoat, and the interface layer is formed by coating an interface treatment agent.
[0049] The interface treatment agent of the embodiment of the present invention comprises component A and component B, and the ratio of component A to component B is 1:1-2, preferably 1:1. Component A comprises the following components in parts by weight: 400-600 parts of cationic acrylic resin and 400-600 parts of water.
[0050] Sources of some raw materials of Component A: Cationic acrylic resin is selected from Taiwan Changwei CW-330 cationic acrylic resin.
[0051] Preparation method of component A: Stir the cationic acrylic resin and water evenly at a low speed in a disperser.
[0052] Component B includes the following components in mass parts: 700-1100 parts of the second inorganic filler and 3-9 parts of the third auxiliary agent. Among them, the second inorganic filler preferably includes the following components in mass parts: 400-600 parts of wollastonite powder, 200-300 parts of cement, and 100-200 parts of quartz powder. The third auxiliary agent preferably includes the following components in mass parts: 1-3 parts of retarder, 1-3 parts of rheological agent, and 1-3 parts of defoamer.
[0053] Sources of some raw materials of Component B: The wollastonite powder adopts 400 mesh wollastonite powder from Xinyu Shengrui.
[0054] The quartz powder uses 400 mesh silicon micropowder from Shenzhen Luyue Powder Technology Co., Ltd.
[0055] The retarder is sodium tetraborate decahydrate.
[0056] The cement used is 62.5# sulphoaluminate cement from Jiangxi Yinshan, which has low alkalinity and high bonding strength.
[0057] The rheological agent selected was STARVIS RS421 / 01F from Wacker.
[0058] The defoaming agent used is AGITAN from Mingling, Germany.
[0059] Preparation method of component B: put all components into powder mixing equipment and mix them evenly.
[0060] At present, most of the solutions involving tile renovation coatings in China only involve surface color change and protection, and there is little description of the interface adhesion between the coating and the tile surface. Usually, tiles that grow moss are mostly glazed clay tiles. The surface of the tiles is dense and smooth, and ordinary coatings are extremely difficult to adhere to, so interface treatment is required before applying the paint. Currently, the commonly used interface primers are acrylic emulsion primers and two-component epoxy primers. Among them, the adhesion of acrylic emulsion primers is limited, and there is a risk of falling off over time. The epoxy primer has too strong sealing properties, and the water vapor inside the tile cannot seep out. Over time, it will cause the surface coating to bulge and fall off.
[0061] The performance of the interface treatment agent of the embodiment of the present invention is tested according to the tensile bond strength test method of concrete interface agent in JC / T907-2018, and the strength is ≥3.0Mpa. Compared with the conventional anionic interface agent, the bonding strength of the interface treatment agent of this embodiment to new glazed tiles and old weathered tiles is 2 to 3 times that of the anionic interface agent, and it has good compatibility with the moss prevention topcoat, and can also have excellent adhesion on wet surfaces, greatly extending the tolerance of building surface construction.
[0062] The moss prevention topcoat of the embodiment of the present invention comprises component A and component B. The ratio of component A to component B is 1:1-2, preferably 1:1. Component A includes the following components in parts by mass: 100-300 parts of water, 50-100 parts of nano titanium dioxide, 400-600 parts of acrylic emulsion, 18-41 parts of the first auxiliary agent, and 50-100 parts of inorganic pigments can be added for coloring. Among them, the first auxiliary agent preferably includes the following components in parts by mass: 1-3 parts of preservatives, 1-3 parts of cellulose, 1-3 parts of wetting agents, 1-3 parts of dispersants, 2-4 parts of defoamers, 5-10 parts of film-forming aids, 5-10 parts of ethylene glycol, 1-2 parts of pH regulators, and 1-3 parts of thickeners. The inorganic pigment is preferably rutile titanium dioxide.
[0063] Sources of some raw materials for component A: The preservative used was Thor's EG-CLF.
[0064] As for the cellulose, PMC15US from Rakuten was used.
[0065] The wetting agent used was Dow's BD405.
[0066] The dispersant used was SN5040 from Nopco.
[0067] The defoamer used is NXZ from Nopco.
[0068] Nano titanium dioxide is KRONOClean 7000 from Omya.
[0069] The rutile titanium dioxide used is R996 from Longmanguoli.
[0070] The acrylic emulsion used was AC-8188 from Dow.
[0071] The film-forming aid is Runtai's dodecyl alcohol ester.
[0072] The pH regulator used was Dow's AMP-95.
[0073] The thickener used was Dow's TT-935.
[0074] Preparation method of component A: a. Add water, preservative, defoamer, wetting agent and dispersant into a disperser, and stir and disperse at a first speed; b. Maintaining the first speed, sequentially adding cellulose, pH regulator, nano titanium dioxide, and titanium dioxide, stirring and dispersing at the second speed; c. Set the speed of the disperser to the third speed, add acrylic emulsion, film-forming aid, ethylene glycol, and thickener in sequence, stir and disperse, and obtain component A.
[0075] Among them, the first rotation speed is 400-500 rpm, the second rotation speed is 1200-1800 rpm, and the third rotation speed is 800-1000 rpm.
[0076] Component B includes the following components in mass fractions: 200-300 parts of cement, 500-800 parts of the first inorganic filler, and 8-19 parts of the second additive. Among them, the first inorganic filler preferably includes the following components in mass fractions: 400-600 parts of wollastonite powder and 100-200 parts of quartz powder. The second additive preferably includes the following components in mass fractions: 1-3 parts of retarder, 1-3 parts of water repellent, 1-3 parts of anti-efflorescence additive, and 5-10 parts of anti-cracking microspheres.
[0077] Sources of some raw materials for component B: The wollastonite powder adopts 400 mesh wollastonite powder from Xinyu Shengrui.
[0078] The quartz powder uses 400 mesh silicon micropowder from Shenzhen Luyue Powder Technology Co., Ltd.
[0079] Sodium citrate is used as retarder.
[0080] The cement used is 62.5# sulphoaluminate cement from Jiangxi Yinshan, which has low alkalinity and high bonding strength.
[0081] The water repellent used is NT10 from German BYK.
[0082] The anti-efflorescence additive is Longhu’s KL-30.
[0083] The anti-cracking microspheres are Omyasphere 213T-FQ, which can reduce the shrinkage of cement to achieve the anti-cracking purpose.
[0084] Preparation method of component B: put all components into powder mixing equipment and mix them evenly.
[0085] The anti-moss topcoat of the embodiment of the present invention utilizes the principle of photocatalysis and the high alkalinity of cement itself, and the coating film has a lasting anti-moss and antibacterial effect.
[0086] The principle of photocatalysis is: using the energy of a specific wavelength of the light source to produce a photocatalytic effect, so that the oxygen and water molecules attached to the surface of the material are excited to generate super-active OH and O2 free ion radicals. These highly oxidizing free radicals can decompose almost all organic substances that are harmful to the human body or the environment, and ultimately decompose organic matter, bacteria, etc. on the surface of the coating into carbon dioxide and water. At the same time, they will also oxidize the organic matter (emulsion, organic color paste) in the coating, so that its polymer chain breaks or degrades, destroying the continuity of the coating and forming soluble or volatile substances. In order to reduce the damage of nano-titanium dioxide photocatalysis to organic matter, the bonding material of the moss prevention topcoat in the embodiment of the present invention is mainly inorganic, supplemented by organic, which delays the degradation of organic matter by nano-titanium dioxide and improves the anti-powdering property of the coating.
[0087] It is understandable that the architectural coating of the embodiment of the present invention can be used for renovation of old tiles. After removing the moss on the tile surface, an interface treatment agent and a moss prevention topcoat are applied to form an architectural coating to prevent moss from growing on the building surface again. It can also be used for protection of new tiles. An interface treatment agent and a moss prevention topcoat are directly applied to form an architectural coating to prevent moss from growing and damaging the tile structure and reduce subsequent maintenance. Of course, the architectural coating of this embodiment can be applied to other building surfaces besides the tile surface, especially a building surface that is as dense and smooth as the tile surface.
[0088] The performance of the building coating of this embodiment was tested with reference to GB / T9755-2014 "Synthetic Resin Emulsion Exterior Wall Paint" superior product and JC / T2090-2011 "Polymer Cement Waterproof Slurry" Type II. The specific proportions of each experimental example are shown in Table 3, and the test results of each experimental example are shown in Table 4. It can be seen that various properties of the building coating have passed the standard requirements, and the bonding strength is much greater than the standard requirements.
[0089] Table 3
[0090] Table 4
[0091] The building surface renovation method of this embodiment is further described below in conjunction with tile surface renovation. The tile surface is renovated according to Table 5: Table 5
[0092] The experimental data after relevant tests on the above embodiments and comparative examples are shown in Table 6: Table 6
[0093] The cross-cut adhesion method shall be in accordance with GB / T9286-2021 "Scratching Test for Paints and Varnishes".
[0094] The tensile bond strength with the tile surface is carried out according to the method of JC / T907-2018 "Concrete Interface Treatment Agent".
[0095] The aging resistance is carried out according to cycle A in GB / T9765-2009. The result evaluation is in accordance with GB / T1766.
[0096] Through the comparison of the above embodiments and the comparative examples, it can be seen that compared with the existing moss removal method, the moss removal method of the embodiment of the present invention is more convenient, safe and reliable, the adhesion between the building coating of this embodiment and the tile surface can reach level 0, the tensile bonding strength is significantly higher than that of the comparative example, the adhesion strength is high, the compatibility is good, the anti-aging performance and weather resistance are excellent, and it is more durable.
[0097] Although the present invention has been specifically shown and described in conjunction with the preferred embodiments, it should be understood by those skilled in the art that various changes in form and details may be made to the present invention without departing from the spirit and scope of the invention as defined in the appended claims, all of which are within the scope of protection of the present invention.
Claims
1. A moss prevention paint, It is characterized in that include: A component and B component; The component A comprises, by weight, 100 to 300 parts of water, 50 to 100 parts of nano titanium dioxide, 400 to 600 parts of acrylic emulsion, and 18 to 41 parts of the first auxiliary agent; The B component comprises, by weight, 200 to 300 parts of cement, 500 to 800 parts of a first inorganic filler, and 8 to 19 parts of a second auxiliary agent.
2. The moss prevention topcoat according to claim 1, It is characterized in that The first auxiliary agent comprises, by weight, 1 to 3 parts of preservative, 1 to 3 parts of cellulose, 1 to 3 parts of wetting agent, 1 to 3 parts of dispersant, 2 to 4 parts of defoaming agent, 5 to 10 parts of film-forming aid, 5 to 10 parts of ethylene glycol, 1 to 2 parts of pH regulator, and 1 to 3 parts of thickener; The first inorganic filler comprises, by mass, 400 to 600 parts of wollastonite powder and 100 to 200 parts of quartz powder; The second auxiliary agent comprises, by weight, 1 to 3 parts of retarder, 1 to 3 parts of water repellent, 1 to 3 parts of anti-efflorescence auxiliary agent, and 5 to 10 parts of anti-cracking microspheres.
3. The moss prevention topcoat according to claim 2, It is characterized in that The component A also includes: 50 to 100 parts of inorganic pigment.
4. The moss prevention topcoat according to claim 3, It is characterized in that The ratio of component A to component B is 1:1-2; the inorganic pigment is rutile titanium dioxide; the quartz powder is silica powder; the retarder is sodium citrate; and the cement is aluminum sulfate cement.
5. The moss prevention topcoat according to claim 3 or 4, It is characterized in that The preparation method of component A comprises: Add water, preservative, defoamer, wetting agent and dispersant into the disperser, and stir and disperse at a first speed; Keeping the first speed, adding cellulose, pH adjuster, nano titanium dioxide, and inorganic pigment in sequence and stirring and dispersing at the second speed; The speed of the disperser is set to the third speed, and acrylic emulsion, film-forming aid, ethylene glycol, and thickener are added in sequence for stirring and dispersing; Wherein, the first rotation speed is 400-500 rpm, the second rotation speed is 1200-1800 rpm, and the third rotation speed is 800-1000 rpm.
6. A building coating, It is characterized in that include: An interface layer coated on a building surface and a topcoat layer coated on the interface layer; the topcoat layer is formed by coating the moss prevention topcoat according to any one of claims 1 to 5; and the interface layer is formed by coating an interface treatment agent.
7. The architectural coating according to claim 6, It is characterized in that The interface treatment agent comprises: component A and component B; The component A comprises, by mass, 400 to 600 parts of cationic acrylic resin and 400 to 600 parts of water; The component B comprises, by mass, 700 to 1100 parts of the second inorganic filler and 3 to 9 parts of the third auxiliary agent.
8. The architectural coating according to claim 7, It is characterized in that The second inorganic filler comprises, by mass, 400 to 600 parts of wollastonite powder, 200 to 300 parts of cement, and 100 to 200 parts of quartz powder; The third auxiliary agent comprises, by weight, 1 to 3 parts of a retarder, 1 to 3 parts of a rheological agent, and 1 to 3 parts of a defoaming agent.
9. The architectural coating according to claim 8, It is characterized in that In the interface treatment agent, the ratio of component A to component B is 1:1-2; the quartz powder is selected from silicon micropowder, the cement is selected from aluminum sulfate cement, and the retarder is selected from sodium tetraborate decahydrate.
10. A method for renovating a building surface, It is characterized in that The steps include: S1: Remove moss from building surfaces; S2: Applying the architectural coating according to any one of claims 6 to 9 on the building surface.
Citation Information
Patent Citations
High-wear-resistance interior wall cement paint and preparation method thereof
CN115322604A
Brick-smashing-free interface material for repairing and preparation method of brick-smashing-free interface material
CN115584152A
Cited By
High-weather-resistance inorganic waterproof stone-like paint and preparation method thereof