UV curing coating composition, preparation method thereof and blackboard
By using a UV curable coating composition in the blackboard coating, combined with polyurethane acrylate, modified nanosilica and hydrophobic antifouling additives, the problems of insufficient durability and poor cleaning effect of the blackboard coating are solved, achieving higher Excellent wear resistance, stain resistance and easy cleaning, extending the service life.
Patent Information
- Application Number
- CN202410994679.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-11
AI Technical Summary
The existing blackboard coating has insufficient durability and poor cleaning effect, and is prone to problems such as powder retention, scratches, oil and wax marks, and coating wear, resulting in a low service life.
Using a UV curing coating composition, including polyurethane acrylate, modified nanosilica and hydrophobic antifouling additives, the fluorine-containing carbon chain structure and acrylate group are introduced through grafting technology to form a stable inorganic-organic hybrid structure , improve the wear resistance, antifouling and easy cleaning of the coating.
It extends the service life of the blackboard coating, improves the coating's wear resistance, antifouling properties and ease of cleaning, and solves the problems of insufficient durability and poor cleaning effect.
Smart Images

Figure BDA0004960783640000141
Abstract
Description
Technical Field
[0001] The present application relates to blackboard coatings, and in particular to a UV curing coating composition and a preparation method thereof, and a blackboard. Background Art
[0002] As an important auxiliary tool, blackboard is widely used in daily study and work. Most of the existing blackboard coatings are prepared with acrylic resin as the base resin and cured by traditional curing methods (natural & thermal curing).
[0003] Although acrylic resin coating has excellent performance, its bonding strength is average, the cleaning effect is poor, and the long-term service life is low. There are some shortcomings in the actual wiping process that affect the writing on the blackboard. For example, when using traditional dust-free chalk to wipe, it is easy to leave powder and a small amount of scratches on the surface of the blackboard; the new water-soluble chalk can be wiped to a very low degree, most of which require wet wiping, and it is easy to leave oil and wax marks after wiping. In addition, after long-term use, the coating is prone to serious wear, paint loss, color fading, etc., and in severe cases, it may even cause the coating to peel off. Summary of the invention
[0004] The embodiments of the present application provide a UV curable coating composition and a preparation method thereof, and a blackboard, which can solve the problems of insufficient durability and poor cleaning effect of existing blackboard coatings.
[0005] In the first aspect, an embodiment of the present application provides a UV-curable coating composition, comprising optional additives and the following components in parts by weight: polyurethane acrylate, 25-40 parts; modified nano-silica, 8-12 parts; hydrophobic antifouling agent, 4-8 parts; reactive diluent, 5-15 parts; organic solvent, 25-35 parts; photoinitiator, 1-3 parts; wherein the modified nano-silica comprises a fluorine-containing carbon chain structure, an acrylate group and a polymethylhydrogensiloxane group grafted to the nano-silica; the hydrophobic antifouling agent comprises a modified cage-type polysilsesquioxane, and the modified cage-type polysilsesquioxane comprises a fluorine-containing carbon chain structure and an acrylate group grafted to the cage-type polysilsesquioxane.
[0006] According to an embodiment of the first aspect of the present application, modified nano-silica is obtained by grafting a composite coupling agent including a first coupling agent and a second coupling agent with nano-silica, the first coupling agent including a fluorine-containing carbon chain silane coupling agent, and the second coupling agent including a silane coupling agent containing an acrylate group.
[0007] According to an embodiment of the first aspect of the present application, the first coupling agent includes a perfluorocarbon chain silane coupling agent.
[0008] According to an embodiment of the first aspect of the present application, the first coupling agent includes one or more of perfluorododecyltrimethoxysilane, perfluorooctyltrimethoxysilane, perfluorooctyltriethoxysilane, and perfluorodecyltrimethoxysilane; the second coupling agent includes one or more of γ-aminopropyltriethoxysilane (KH550), γ-methacryloxypropyltrimethoxysilane, and 3-(trichlorosilyl)propyl acrylate.
[0009] According to an embodiment of the first aspect of the present application, the average particle size of nano-silicon dioxide is 20-200nm.
[0010] According to an embodiment of the first aspect of the present application, modified nano-silica is prepared by the following method: adding nano-silica to a mixed solution of ethanol, water and ammonia water to form a first solution; adding a fluorine-containing carbon chain silane coupling agent and a silane coupling agent containing an acrylate group to the first solution, reacting to obtain pre-grafted nano-silica; adding the pre-grafted nano-silica to toluene, and then adding polymethylhydrogensiloxane and tri(pentafluorophenyl)borane in sequence to react to obtain modified nano-silica.
[0011] According to an embodiment of the first aspect of the present application, a modified cage-type polysilsesquioxane is prepared by the following method: perfluorooctyltrimethoxysilane is added to a mixed solution of tetrahydrofuran, deionized water and sodium hydroxide, and refluxed at a temperature of 100°C-105°C to obtain a fluorinated cage-type polysilsesquioxane; the fluorinated cage-type polysilsesquioxane and triethylamine are added to tetrahydrofuran, mixed at a temperature of 0°C-5°C to obtain a third solution, 3-(trichlorosilyl)propyl acrylate is added to the third solution within 1 hour, and reacted at a temperature of 0°C-5°C to obtain a modified cage-type polysilsesquioxane.
[0012] According to an embodiment of the first aspect of the present application, the polyurethane acrylate is an aliphatic polyurethane acrylate oligomer, and the functionality of the polyurethane acrylate is 4-15.
[0013] According to an embodiment of the first aspect of the present application, the reactive diluent is an acrylate reactive diluent, and the functionality of the reactive diluent is greater than 1.
[0014] According to an embodiment of the first aspect of the present application, the organic solvent includes one or more of n-butyl acetate, isopropanol, acetone, and ethylene glycol methyl ether; and / or,
[0015] The photoinitiator includes one or more of 1-hydroxycyclohexyl phenyl ketone and diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide; and / or,
[0016] The optional additives include one or more of a leveling agent, a pigment, and a defoaming agent, wherein the leveling agent includes one or more of a modified acrylic leveling agent and an organic silicon leveling agent.
[0017] In a second aspect, an embodiment of the present application provides a method for preparing a UV-curable coating composition, comprising: grafting a fluorine-containing carbon chain silane coupling agent and a silane coupling agent containing an acrylate group with nano-silica, and then adding polymethyl hydrogen siloxane for grafting to obtain modified nano-silica; reacting perfluorooctyltrimethoxysilane with tetrahydrofuran to obtain a fluorinated cage-type polysilsesquioxane, and then adding 3-(trichlorosilyl)propyl acrylate for grafting to obtain a modified cage-type polysilsesquioxane; adding 8-12 parts of modified nano-silica to 25-35 parts of an organic solvent, and then adding 25-40 parts of polyurethane acrylate, 5-15 parts of an active diluent and 4-8 parts of a modified cage-type polysilsesquioxane to obtain a first slurry; adding 1-3 parts of a photoinitiator and optional additives to the first slurry to obtain a UV-curable coating composition.
[0018] In a third aspect, an embodiment of the present application provides a blackboard, comprising a coating formed by the UV-curable coating composition of the embodiment of the first aspect, or a coating formed by the UV-curable coating composition prepared by the preparation method of the embodiment of the second aspect.
[0019] The prepared UV curing coating composition provided by the present application has good wear resistance, weather resistance and easy cleaning, and solves the problems of insufficient durability, difficult cleaning and poor effect of existing blackboard coatings. Among them, polyurethane acrylate is used as the matrix resin, which has good wear resistance and weather resistance, can resist frequent wiping and is not easy to wear, thereby extending the service life of the blackboard coating; modified nano-silicon dioxide grafted with fluorine-containing carbon chain structure, acrylate group and polymethyl hydrogen siloxane group is used, on the one hand, the fluorine-containing carbon chain structure is introduced into the nano-silicon dioxide, and the hydrophobicity and oleophobicity of the coating are improved, on the other hand, the acrylate group makes the nano-silicon dioxide form a cross-linked structure when the coating is cured, and the mechanical properties of the coating are enhanced, and on the other hand, the polymethyl hydrogen siloxane group forms a network structure that wraps the nano-particles, effectively preventing agglomeration.
[0020] The modified nano-silica enables the coating composition to form a stable inorganic-organic hybrid structure in the coating formed by curing, further improving the easy cleaning and wear resistance of the coating; the hydrophobic antifouling agent includes a modified cage-type polysilsesquioxane, whose structure includes an octahedral cage structure composed of siloxane, has a low surface energy, and the peripherally connected fluorinated carbon chain has hydrophobicity and oleophobicity, which can improve the antifouling and easy cleaning properties of the coating, and the grafted acrylate group forms a stable cross-linked structure when the coating is cured, thereby improving the durability of the coating. The coating prepared by the UV curing coating composition of the present application in the form of UV curing, each main component has an active acrylate group that can participate in the curing reaction, forming a stable chemical cross-linked structure, ensuring the uniformity and flatness of the coating, thereby extending the service life of the coating. DETAILED DESCRIPTION
[0021] In order to more clearly understand the above-mentioned purposes, features and advantages of the present application, the scheme of the present application will be further described below. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.
[0022] In the following description, many specific details are set forth to facilitate a full understanding of the present disclosure, but the present application may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present application, rather than all of the embodiments.
[0023] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0024] If not otherwise specified, all embodiments and optional embodiments of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.
[0025] Unless otherwise specified, all technical features and optional technical features of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.
[0026] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, a method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, a method may also include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0027] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0028] Unless otherwise specified, this application adopts conventional test methods or test methods recommended by the instrument.
[0029] The inventor of the present application has noticed that the acrylic resin coating has average bonding strength, poor cleaning effect and low long-term service life when used as a blackboard coating. Therefore, the inventor of the present application has provided a UV curable coating composition and a preparation method thereof through experiments to solve the problems of insufficient durability and poor cleaning effect of existing blackboard coatings.
[0030]
UV curing coating composition
[0031] In a first aspect, the present application provides a UV curable coating composition, comprising optional additives and the following components in parts by weight: polyurethane acrylate, 25-40 parts; modified nano-silica, 8-12 parts; hydrophobic antifouling agent, 4-8 parts; reactive diluent, 5-15 parts; organic solvent, 25-35 parts; photoinitiator, 1-3 parts; wherein the modified nano-silica comprises a fluorine-containing carbon chain structure, an acrylate group and a polymethylhydrogensiloxane group grafted to the nano-silica; the hydrophobic antifouling agent comprises a modified cage-type polysilsesquioxane, and the modified cage-type polysilsesquioxane comprises a fluorine-containing carbon chain structure and an acrylate group grafted to the cage-type polysilsesquioxane.
[0032] Without intending to be limited by any theory or explanation, the UV curable coating composition of the embodiment of the present application adopts polyurethane acrylate as the base resin, has good wear resistance and weather resistance, can resist frequent wiping and is not easy to wear, thereby extending the service life of the blackboard coating. The weight parts of polyurethane acrylate in the UV curable coating composition are 25-40 parts, and illustratively, the weight parts of polyurethane acrylate are 25 parts, 28 parts, 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, or the interval range composed of any two of the above values.
[0033] It is not intended to be limited to any theory or explanation. The UV curing coating composition of the embodiment of the present application adopts modified nano-silica grafted with fluorine-containing carbon chain structure, acrylate group and polymethyl hydrogen siloxane group. On the one hand, the fluorine-containing carbon chain structure is introduced into the nano-silica to improve the hydrophobicity and oleophobicity of the coating. On the other hand, the acrylate group makes the nano-silica form a cross-linked structure when the coating is cured, and the mechanical properties of the coating are enhanced. On the other hand, the polymethyl hydrogen siloxane group forms a network to wrap the structure of the nanoparticles, which effectively prevents agglomeration. Modified nano-silica enables the coating composition to form a stable inorganic-organic hybrid structure in the coating formed by curing, and further improves the easy cleaning and wear resistance of the coating. The weight parts of modified nano-silica in the UV curing coating composition are 8-12 parts. Exemplarily, the weight parts of modified nano-silica are 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, or the interval range composed of any two of the above numerical values.
[0034] Without intending to be limited by any theory or explanation, the UV-curable coating composition of the embodiment of the present application adopts a modified cage-type polysilsesquioxane as a hydrophobic antifouling agent to improve the ease of cleaning and durability. Specifically, the structure of the modified cage-type polysilsesquioxane includes an octahedral cage structure composed of siloxane, which has a low surface energy, and the peripherally connected fluorinated carbon chains have hydrophobic and oleophobic properties, which can improve the antifouling and easy cleaning properties of the coating, and the grafted acrylate groups form a stable cross-linked structure when the coating is cured, thereby improving the durability of the coating. The weight percentage of the hydrophobic antifouling agent in the UV-curable coating composition is 4-8 parts. Exemplarily, the weight percentage of the hydrophobic antifouling agent is 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, or an interval range composed of any two of the above values.
[0035] Without intending to be limited by any theory or explanation, the reactive diluent in the embodiments of the present application is mainly used to reduce the viscosity of the system, and the functional group carried by the reactive diluent enables it to participate in the curing reaction and improve the strength of the cured coating. For example, the functional group carried by the reactive diluent is an acrylate group. The weight proportion of the reactive diluent in the UV curable coating composition is 5-15 parts, and illustratively, the weight proportion of the reactive diluent is 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, or an interval range consisting of any two of the above values.
[0036] Without intending to be limited by any theory or explanation, the photoinitiator in the embodiments of the present application undergoes chemical changes after receiving or absorbing external energy, decomposing into free radicals or cations, thereby initiating a polymerization reaction. The weight percentage of the photoinitiator in the UV curable coating composition is 1-3 parts, and illustratively, the weight percentage of the photoinitiator is 1 part, 2 parts, 3 parts, or an interval range consisting of any two of the above values.
[0037] In summary, the UV curable coating composition of the embodiment of the present application adopts polyurethane acrylate as the base resin, and adds modified nano-silica and hydrophobic antifouling additives to solve the problems of insufficient durability and poor cleaning effect. The UV curable coating composition of the embodiment of the present application has active acrylate groups in each of its main components that can participate in the curing reaction. When cured by UV, a stable chemical cross-linking structure can be formed, which ensures the uniformity and flatness of the coating, thereby extending the service life of the coating.
[0038] In some embodiments, the modified nano-silica is obtained by grafting a composite coupling agent including a first coupling agent and a second coupling agent with nano-silica, the first coupling agent includes a fluorine-containing carbon chain silane coupling agent, and the second coupling agent includes a silane coupling agent containing an acrylate group.
[0039] In the embodiment of the present application, the above-mentioned fluorine-containing carbon chain silane coupling agent and the silane coupling agent containing acrylate groups are reacted and grafted with nano-silica, so that the fluorine-containing carbon chain and the acrylate group can be grafted onto the surface of the nano-silica, so that the obtained modified nano-silica can improve the hydrophobicity and oleophobicity of the formed coating, form a cross-linked structure, and enhance the mechanical properties of the coating.
[0040] In order to further improve the hydrophobicity and oleophobicity of the formed coating, in some embodiments, the first coupling agent includes a perfluorocarbon chain silane coupling agent. The embodiments of the present application further improve the hydrophobicity and oleophobicity by selecting a perfluorocarbon chain.
[0041] In some embodiments, the first coupling agent includes one or more of perfluorododecyltrimethoxysilane, perfluorooctyltrimethoxysilane, perfluorooctyltriethoxysilane, and perfluorodecyltrimethoxysilane; the second coupling agent includes one or more of γ-aminopropyltriethoxysilane (KH550), γ-methacryloxypropyltrimethoxysilane, and 3-(trichlorosilyl)propyl acrylate.
[0042] In some embodiments, the average particle size of nano silicon dioxide is 20-200 nm. The applicant has noticed that the particle size of nano silicon dioxide will affect the properties of the coating formed by the UV curing coating composition. When the average particle size of nano silicon dioxide is within the above range, its dispersibility is good, the flatness of the coating film is high, and the use cost is low.
[0043] The present application provides a method for preparing modified nano-silicon dioxide. In some embodiments, the modified nano-silicon dioxide is prepared by:
[0044] S10: adding nano-silica to a mixed solution of ethanol, water and ammonia to form a first solution; adding a fluorine-containing carbon chain silane coupling agent and an acrylate group-containing silane coupling agent to the first solution to react and obtain pre-grafted nano-silica;
[0045] S12: adding the pre-grafted nano-silica to toluene, and then sequentially adding polymethylhydrogensiloxane and tri(pentafluorophenyl)borane to react to obtain modified nano-silica.
[0046] In some embodiments, in step S10, each component is reacted according to the weight proportion: nano-silicon dioxide, 3-5 parts; ethanol, 600-1000 parts; water, 60-80 parts; ammonia water (concentration 18% wt), 50-65 parts; fluorine-containing carbon chain silane coupling agent, 2-3 parts; silane coupling agent containing acrylate group, 2-3 parts. Exemplarily, step S10 specifically includes: adding 3-5 parts of nano-silicon dioxide to a mixed solution of 600-1000 parts of anhydrous ethanol, 60-80 parts of water and 50-65 parts of ammonia water (concentration 18% wt), ultrasonically dispersing for 10 minutes (20-25kHz at 250-350W) to form a uniform solution. Add 2-3 parts of perfluorocarbon chain silane coupling agent and 2-3 parts of silane coupling agent containing acrylate group, stir and react at 1000r / min-1300r / min for 2h, wash with ethanol at 8000-10000rpm in a centrifuge for 3 times, dry at 60℃ for 1h to obtain pre-grafted nano-silica.
[0047] The preparation method of modified nano-silica in the embodiment of the present application is simple to operate and suitable for large-scale production.
[0048] In some embodiments, in step S12, each component is reacted according to the weight parts: pre-grafted nano-silica, 4-6 parts; toluene, 800-1200 parts; polymethylhydrogensiloxane (PMHS), 8-10 parts; tri(pentafluorophenyl)borane, 3-4 parts. Exemplarily, step S12 specifically includes: adding 4-6 parts of pre-grafted nano-silica to 800-1200 parts of toluene, ultrasonically dispersing for 10 minutes (250-350W at 20-25kHz), slowly adding 8-10 parts of PMHS, and then adding 3-4 parts of tri(pentafluorophenyl)borane, stirring and reacting at 1700r / min-2000r / min for 2 hours. Wash with ethanol and chloroform at 8000-10000rpm in a centrifuge for 3 times, and dry at 110°C for 1 hour to obtain modified nano-silica.
[0049] The present application provides a method for preparing a modified cage-type polysilsesquioxane. In some embodiments, the modified cage-type polysilsesquioxane is prepared by:
[0050] S11: adding perfluorooctyltrimethoxysilane to a mixed solution of tetrahydrofuran, deionized water and sodium hydroxide, and subjecting the mixture to a reflux reaction at a temperature of 100° C. to 105° C. to obtain a fluorinated cage-type polysilsesquioxane;
[0051] S13: Add fluorinated cage-type polysilsesquioxane and triethylamine to tetrahydrofuran, mix at a temperature of 0°C-5°C to obtain a third solution, add 3-(trichlorosilyl)propyl acrylate to the third solution within 1 hour, and react at a temperature of 0°C-5°C to obtain a modified cage-type polysilsesquioxane.
[0052] In some embodiments, in step S11, each component is reacted according to the weight parts: perfluorooctyltrimethoxysilane, 4-6 parts; tetrahydrofuran, 22-30 parts; deionized water, 0.5-1 parts; sodium hydroxide, 0.4-0.8 parts. Exemplarily, step S11 specifically includes: in a fume hood, 4-6 parts of perfluorooctyltrimethoxysilane are added to a mixed solution of 22-30 parts of tetrahydrofuran, 0.5-1 parts of deionized water and 0.4-0.8 parts of sodium hydroxide, stirred at 200-300r / min at room temperature for 10min, and refluxed at 100-105°C for 1h. After the reaction is completed, the excess solvent is removed by rotary evaporation to obtain a fluorinated cage-type polysilsesquioxane.
[0053] In some embodiments, in step S13, each component is reacted according to the weight parts: fluorinated cage polysilsesquioxane, 6-9 parts; triethylamine, 0.6-1 parts; tetrahydrofuran, 100-120 parts; 3-(trichlorosilyl)propyl acrylate, 2-3 parts. Exemplarily, step S13 specifically includes: in a fume hood, 6-9 parts of fluorinated cage polysilsesquioxane and 0.6-1 parts of triethylamine are added to 100-120 parts of tetrahydrofuran, stirred at 200-300r / min for 10min in an ice-water bath (0-5°C), 2-3 parts of 3-(trichlorosilyl)propyl acrylate are slowly added to the above mixed solution within 1h, and the ice-water bath reaction is maintained for 1.5h. After the reaction is completed, the excess solvent is removed by rotary evaporation to obtain a modified cage polysilsesquioxane.
[0054] The preparation method of the modified cage-type polysilsesquioxane in the embodiment of the present application is simple to operate and suitable for large-scale production.
[0055] In some embodiments, the urethane acrylate is an aliphatic urethane acrylate oligomer, and the functionality of the urethane acrylate is 4-15.
[0056] In some embodiments, the reactive diluent is an acrylate reactive diluent, and the functionality of the reactive diluent is greater than 1.
[0057] In some embodiments, the aliphatic urethane acrylate oligomer has a number average molecular weight of 300-400.
[0058] The embodiments of the present application set the types and functionalities of polyurethane acrylate and reactive diluent so that the UV curable coating composition can easily form a cross-linked structure when curing to form a film, thereby improving stability.
[0059] In some embodiments, the reactive diluent includes at least one of methacrylic acid, butyl acrylate, isooctyl acrylate, glycidyl acrylate, hydroxyethyl methacrylate, ethyl acrylate, allyl methacrylate, hexanediol diacrylate, dipropylene glycol diacrylate, neopentyl glycol diacrylate, ethylene glycol dimethacrylate, and trimethylolpropane triacrylate.
[0060] In some embodiments, the organic solvent includes one or more of n-butyl acetate, isopropyl alcohol, acetone, and ethylene glycol methyl ether.
[0061] In some embodiments, the photoinitiator includes one or more of 1-hydroxycyclohexylphenyl ketone, diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide.
[0062] In some embodiments, the optional additives include one or more of a leveling agent, a pigment, and a defoaming agent, wherein the leveling agent includes one or more of a modified acrylic leveling agent and an organic silicon leveling agent. Appropriate pigments can make the coating color accurate, bright, and durable, and improve the aesthetics.
[0063] [Preparation method of UV curing coating composition]
[0064] In a second aspect, the present application provides a method for preparing a UV-curable coating composition, comprising: grafting a fluorine-containing carbon chain silane coupling agent and a silane coupling agent containing an acrylate group with nano-silica, and then adding polymethyl hydrogen siloxane for grafting to obtain modified nano-silica; reacting perfluorooctyltrimethoxysilane with tetrahydrofuran to obtain a fluorinated cage-type polysilsesquioxane, and then adding 3-(trichlorosilyl)propyl acrylate for grafting to obtain a modified cage-type polysilsesquioxane; adding 8-12 parts of modified nano-silica to 25-35 parts of an organic solvent, and then adding 25-40 parts of polyurethane acrylate, 5-15 parts of an active diluent and 4-8 parts of a modified cage-type polysilsesquioxane to obtain a first slurry; adding 1-3 parts of a photoinitiator and optional additives to the first slurry to obtain a UV-curable coating composition.
[0065] The present application prepares modified nano-silica grafted with a fluorine-containing carbon chain structure, an acrylate group and a polymethylhydrogensiloxane group and applies it to a UV-curing coating composition, thereby improving the cleanability and wear resistance of the coating; the present application prepares an octahedral cage structure composed of siloxane, which is grafted with a hydrophobic antifouling agent with a fluorine-containing carbon chain structure and an acrylate group, thereby further improving the antifouling, cleanability and durability of the coating.
[0066] In the above steps, the types and amounts of the components can be the same as those in the first aspect, and will not be described in detail herein. The reaction conditions are not specifically limited, and those skilled in the art can adjust them as needed.
[0067]
blackboard
[0068] In a third aspect, an embodiment of the present application provides a blackboard, comprising a coating formed by the UV-curable coating composition of the embodiment of the first aspect, or a coating formed by the UV-curable coating composition prepared by the preparation method of the embodiment of the second aspect.
[0069] The blackboard of the embodiment of the present application includes a coating made of the above-mentioned UV-curing coating composition. By applying modified nano-silica grafted with a fluorine-containing carbon chain structure, an acrylate group and a polymethylhydrogensiloxane group to the UV-curing coating composition, the cleanability and wear resistance of the blackboard are improved; by applying an octahedral cage structure composed of siloxane and a hydrophobic anti-fouling agent grafted with a fluorine-containing carbon chain structure and an acrylate group to the UV-curing coating composition, the anti-fouling, cleanability and durability of the blackboard are further improved.
[0070] Example
[0071] The following examples more specifically describe the disclosure of the present application, which are intended for illustrative purposes only, as it will be apparent to those skilled in the art that various modifications and variations are possible within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.
[0072] The preparation method of modified nano-silicon dioxide is as follows:
[0073] 4 parts of nano-silicon dioxide (particle size 100nm) were added to a mixed solution of 800 parts of anhydrous ethanol, 70 parts of water and 60 parts of ammonia water (concentration 18%wt), and ultrasonically dispersed for 10min (20-25kHz at 250-350W) to form a uniform solution. 2.5 parts of perfluorooctyl triethoxysilane and 2.5 parts of KH570 were added, and the mixture was stirred at 1200r / min for 2h, washed 3 times with ethanol at 8000-10000rpm in a centrifuge, and dried at 60℃ for 1h to obtain pre-grafted nano-silicon dioxide.
[0074] 5 parts of the above product were added to 1000 parts of toluene, ultrasonically dispersed for 10 minutes (20-25kHz at 250-350W), slowly added 9 parts of PMHS, and then added 3.5 parts of tris(pentafluorophenyl)borane, stirred at 1800r / min for 2 hours, washed with ethanol and chloroform at 9000rpm in a centrifuge for 3 times, and dried at 110°C for 1 hour to obtain modified nano-silica.
[0075] The preparation method of modified cage-type polysilsesquioxane is as follows:
[0076] In a fume hood, 5 parts of perfluorooctyltrimethoxysilane were added to a mixed solution of 26 parts of tetrahydrofuran, 0.8 parts of deionized water and 0.6 parts of sodium hydroxide, stirred at 250 r / min for 10 minutes at room temperature, and refluxed at 105°C for 1 hour. After the reaction was completed, the excess solvent was removed by rotary evaporation to obtain a fluorinated cage-type polysilsesquioxane.
[0077] In a fume hood, 8 parts of fluorinated cage-type polysilsesquioxane and 0.8 parts of triethylamine were added to 110 parts of tetrahydrofuran, stirred at 300 r / min for 10 minutes in an ice-water bath (0-5°C), 2.5 parts of 3-(trichlorosilyl)propyl acrylate were slowly added to the mixed solution within 1 hour, and the ice-water bath was kept to react for 1.5 hours. After the reaction was completed, the excess solvent was removed by rotary evaporation to obtain a modified cage-type polysilsesquioxane.
[0078] Example 1
[0079] A UV curing coating composition comprises the following components in parts by weight: 25 parts of polyurethane acrylate; 8 parts of modified nano-silicon dioxide; 5 parts of hydrophobic antifouling agent; 6 parts of active diluent (dipropylene glycol diacrylate); 25 parts of organic solvent (n-butyl acetate); and 1 part of photoinitiator (PI-184).
[0080] The preparation method is as follows:
[0081] After adding 8 parts of modified nano-silica to 25 parts of organic solvent, 25 parts of polyurethane acrylate, 6 parts of reactive diluent and 5 parts of modified cage-type polysilsesquioxane are added to obtain a first slurry; 1 part of photoinitiator and optional additives are added to the first slurry to obtain a UV-curable coating composition.
[0082] Example 2
[0083] A UV curing coating composition comprises the following components in parts by weight: 32 parts of polyurethane acrylate; 10 parts of modified nano-silicon dioxide; 6 parts of hydrophobic antifouling agent; 10 parts of active diluent (dipropylene glycol diacrylate); 30 parts of organic solvent (n-butyl acetate); and 2 parts of photoinitiator (PI-184).
[0084] The preparation method is as follows:
[0085] After adding 10 parts of modified nano-silica to 30 parts of organic solvent, 32 parts of polyurethane acrylate, 10 parts of active diluent and 6 parts of modified cage-type polysilsesquioxane are added to obtain a first slurry; 2 parts of photoinitiator and 0.5 parts of silicone leveling agent are added to the first slurry to obtain a UV-curable coating composition.
[0086] Example 3
[0087] A UV curing coating composition comprises the following components in parts by weight: 40 parts of polyurethane acrylate; 12 parts of modified nano-silicon dioxide; 8 parts of hydrophobic antifouling agent; 15 parts of active diluent (dipropylene glycol diacrylate); 35 parts of organic solvent (n-butyl acetate); and 3 parts of photoinitiator (PI-184).
[0088] The preparation method is as follows:
[0089] After adding 12 parts of modified nano-silica to 35 parts of organic solvent, 40 parts of polyurethane acrylate, 15 parts of reactive diluent and 8 parts of modified cage-type polysilsesquioxane are added to obtain a first slurry; 3 parts of photoinitiator and optional additives are added to the first slurry to obtain a UV-curable coating composition.
[0090] Comparative Example 1
[0091] The only difference between Comparative Example 1 and Example 2 is that the modified nano-silica used in the preparation process is replaced by unmodified nano-silica.
[0092] Comparative Example 2
[0093] The only difference between Comparative Example 2 and Example 2 is that the hydrophobic antifouling agent used in the preparation process is not added.
[0094] Comparative Example 3
[0095] The only difference between Comparative Example 3 and Example 2 is that the polyurethane acrylate used in the preparation process is replaced by UV epoxy resin.
[0096] Comparative Example 4
[0097] The only difference between Comparative Example 1 and Example 2 is that the weight proportion of the modified nano-silicon dioxide used in the preparation process is 20 parts.
[0098] Comparative Example 5
[0099] The only difference between Comparative Example 1 and Example 2 is that the average particle size of the nano-silicon dioxide used in the preparation process is 500 nm.
[0100] Data analysis
[0101] The UV curable coating composition prepared above was evenly sprayed on the surface of the substrate, semi-dried at 80°C for 5-8 minutes, and UV cured for 1 minute (ultraviolet radiation illumination 25-50 mW / cm 2 ), and placed at room temperature for 24 hours to obtain an easy-to-clean UV-cured blackboard coating. The coatings in Examples 1-3 and Comparative Examples 1-5 were tested for performance, and the test method was as follows:
[0102] Water contact angle: An optical contact angle meter was used to quantitatively test the hydrophobicity of the coating. The contact angle (CA) was measured using 5 μL of test liquid. At least three different locations of the same sample were tested and the average value was taken.
[0103] Surface hardness: Tested in accordance with standard GB / T 6739-2022.
[0104] Wear resistance: Tested in accordance with standard ASTDM D4060.
[0105] Acid and alkali resistance: tested in accordance with standard GB / T 9274-1988.
[0106] Wiping effect: Write 20*40cm text on the blackboard coating of the above sample, and use a blackboard eraser to wipe it after 50 minutes (simulating the time of a class). The blackboard eraser must ensure that no water can be squeezed out after being soaked in water. Testers are required to score the wiping effect, with 1 point indicating the worst cleanliness and 5 points indicating the best cleanliness. There are 10 testers, remove the highest and lowest scores, and then take the average to get the test result.
[0107] The test results are shown in Table 1:
[0108] Table 1 Performance data test of embodiments and comparative examples
[0109]
[0110] As can be seen from the above table, Examples 1 to 3 illustrate that the present application improves the cleanability and wear resistance of the coating by preparing modified nano-silica grafted with a fluorine-containing carbon chain structure, an acrylate group and a polymethylhydrogensiloxane group and applying it to a UV-curing coating composition; the present application prepares an octahedral cage structure composed of siloxane, which is grafted with a hydrophobic antifouling agent having a fluorine-containing carbon chain structure and an acrylate group, thereby further improving the antifouling, cleanability and durability of the coating.
[0111] The performance of Comparative Example 1 is reduced because the nano-silica has not been modified, resulting in reduced performance; the absence of a hydrophobic agent in Comparative Example 2 has the greatest impact on the hydrophobic properties of the coating; the resin in Comparative Example 3 will also affect the effective combination of the components, resulting in reduced performance; the excessive amount of silica in Comparative Example 4 will lead to reduced performance, especially the greatest impact on mass loss due to wear; the particle size in Comparative Example 5 is too large, the specific surface area is reduced, and various performances will also be affected.
[0112] The above are only specific implementation methods of the present application. Those skilled in the art can clearly understand that for the convenience and simplicity of description, the specific working processes of the systems, modules and units described above can refer to the corresponding processes in the aforementioned method embodiments, and will not be repeated here. It should be understood that the protection scope of the present application is not limited to this. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in this application, and these modifications or replacements should be included in the protection scope of this application.
Claims
1. A UV curable coating composition, characterized in that: Including optional additives and the following components in parts by weight: Polyurethane acrylate, 25-40 parts; Modified nano-silicon dioxide, 8-12 parts; Hydrophobic antifouling agent, 4-8 parts; Active diluent, 5-15 parts; Organic solvent, 25-35 parts; Photoinitiator, 1-3 parts; Wherein, the modified nano-silica includes a fluorine-containing carbon chain structure, an acrylate group and a polymethylhydrogensiloxane group grafted to the nano-silica; The hydrophobic antifouling auxiliary agent comprises a modified cage-type polysilsesquioxane, and the modified cage-type polysilsesquioxane comprises a fluorine-containing carbon chain structure and an acrylate group grafted to the cage-type polysilsesquioxane.
2. The UV curable coating composition according to claim 1, characterized in that The modified nano-silica is obtained by grafting a composite coupling agent including a first coupling agent and a second coupling agent with the nano-silica. The first coupling agent includes a fluorine-containing carbon chain silane coupling agent, and the second coupling agent includes a silane coupling agent containing an acrylate group.
3. The UV curable coating composition according to claim 2, characterized in that: The first coupling agent includes one or more of perfluorododecyltrimethoxysilane, perfluorooctyltrimethoxysilane, perfluorooctyltriethoxysilane, and perfluorodecyltrimethoxysilane; The second coupling agent includes one or more of γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, and 3-(trichlorosilyl)propyl acrylate.
4. The UV curable coating composition according to claim 2, characterized in that The average particle size of the nano silicon dioxide is 20-200 nm.
5. The UV curable coating composition according to any one of claims 1 to 4, characterized in that: The modified nano silicon dioxide is prepared by the following method: Adding the nano-silica to a mixed solution of ethanol, water and ammonia to form a first solution; adding the fluorine-containing carbon chain silane coupling agent and the silane coupling agent containing an acrylate group to the first solution to react and obtain pre-grafted nano-silica; The pre-grafted nano-silica is added into toluene, and then polymethyl hydrogen siloxane and tri(pentafluorophenyl)borane are added in sequence to react to obtain the modified nano-silica.
6. The UV curable coating composition according to any one of claims 1 to 4, characterized in that: The modified cage-type polysilsesquioxane is prepared by the following method: Adding perfluorooctyltrimethoxysilane to a mixed solution of tetrahydrofuran, deionized water and sodium hydroxide, and subjecting the mixture to a reflux reaction at a temperature of 100° C. to 105° C., to obtain a fluorinated cage-type polysilsesquioxane; The fluorinated cage-type polysilsesquioxane and triethylamine are added to tetrahydrofuran, and mixed at a temperature of 0°C-5°C to obtain a third solution. 3-(trichlorosilyl)propyl acrylate is added to the third solution within 1 hour, and reacted at a temperature of 0°C-5°C to obtain the modified cage-type polysilsesquioxane.
7. The UV curable coating composition according to claim 1, characterized in that: The polyurethane acrylate is an aliphatic polyurethane acrylate oligomer, and the functionality of the polyurethane acrylate is 4-15; and / or, The reactive diluent is an acrylate reactive diluent, and the functionality of the reactive diluent is greater than 1.
8. The UV curable coating composition according to claim 1, characterized in that: The organic solvent comprises one or more of n-butyl acetate, isopropanol, acetone, and ethylene glycol methyl ether; and / or, The photoinitiator includes one or more of 1-hydroxycyclohexyl phenyl ketone and diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide; and / or, The optional additives include one or more of a leveling agent, a pigment, and a defoaming agent, wherein the leveling agent includes one or more of a modified acrylic leveling agent and an organic silicon leveling agent.
9. A method for preparing a UV curable coating composition, characterized in that: include: After a silane coupling agent containing a fluorine carbon chain and a silane coupling agent containing an acrylate group are grafted onto nano-silica, polymethyl hydrogen siloxane is added for grafting to obtain modified nano-silica; After perfluorooctyltrimethoxysilane and tetrahydrofuran are reacted to obtain a fluorinated cage-type polysilsesquioxane, 3-(trichlorosilyl)propyl acrylate is added for grafting to obtain a modified cage-type polysilsesquioxane; After adding 8-12 parts of the modified nano-silica to 25-35 parts of an organic solvent, 25-40 parts of polyurethane acrylate, 5-15 parts of a reactive diluent and 4-8 parts of the modified cage-type polysilsesquioxane are added to obtain a first slurry; 1-3 parts of a photoinitiator and optional additives are added to the first slurry to obtain a UV-curable coating composition.
10. A blackboard, characterized in that: A coating formed by the UV curing coating composition according to any one of claims 1 to 8, or a coating formed by the UV curing coating composition prepared by the preparation method according to claim 9.
Citation Information
Patent Citations
UV photo-curing hydrophobic antifouling paint and preparation thereof
CN101372562A
High-hydrophilicity high-wear-resistance organic / inorganic hybrid photocuring paint composition
CN105153924A
Antifouling and anti-glare paint and preparation method thereof
CN111826061A
Modified silicon dioxide aerogel reinforced styrene-butadiene rubber and preparation method thereof
CN116239829A
Super-hydrophobic coating based on polyhedral oligomeric silsesquioxane
CN116285671A
Cited By
Artistic paint with anti-graffiti stain-resistant coating and preparation method of artistic paint
CN122587581A
An artistic paint having an anti-graffiti stain resistant coating and a method of making the same