Three-tire-base double-channel prefabricated occlusion lap joint waterproof coiled material
By setting a second polymer membrane base layer in the prefabricated overlapping waterproof membrane to separate the adhesive layer, the problem of adhesive layer adhesion is solved and the strength of the membrane and construction convenience are improved.
Patent Information
- Application Number
- CN202411237044.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-09-05
AI Technical Summary
When the prefabricated overlapping waterproof membrane is inserted into the gap, the adhesive layer easily sticks the third isolation film and the fourth isolation membrane together, which makes the construction difficult and the membrane strength is low.
A three-base double-channel prefabricated overlapping waterproof membrane is designed. By setting a second polymer membrane base layer between the second penetrating reaction adhesive layer and the third penetrating reaction adhesive layer, it is divided into four penetrating reaction adhesive layers. The adhesive layer is inserted into the adhesive layer, and one end of the second polymer film base layer is extended into the overlapping interface to clearly isolate the upper and lower layers of the overlapping interface, preventing the adhesive layer from adhering and increasing the strength of the membrane.
It achieves simple construction without adhesion at the overlap joint in actual production, improves the strength of the prefabricated overlapping waterproof membrane, and ensures that the third isolation film and the fourth isolation film are easy to tear off without excess glue remaining.
Smart Images

Figure CN118755399A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterproof coiled materials, and in particular to a three-base double-channel prefabricated bite-jointed overlapping waterproof coiled material. Background Art
[0002] Prefabricated waterproofing membrane refers to waterproofing membrane that is pre-laid before structural construction. It is a membrane with a polymer as the main body and a self-adhesive layer on the surface. After the construction of prefabricated waterproofing membrane, steel bars and concrete can be laid directly. It has low cost and fast construction speed. In addition, it has good puncture and tear resistance. It is an efficient, convenient building material with excellent physical and chemical properties.
[0003] With the in-depth research on prefabricated waterproof membranes, prefabricated interlocking overlapping waterproof membranes have emerged. For example, the invention patent application with publication number CN118109138A discloses an interlocking overlapping polymer waterproof material. Although its interlocking overlapping structure will not have wrinkles or warping after overlapping, in actual production, the adhesive layer inserted in the gap can easily stick the third isolation membrane and the fourth isolation membrane together, resulting in construction difficulties, and there is also a problem of low strength. Summary of the invention
[0004] The present invention proposes a three-base double-pass prefabricated interlocking lap waterproofing membrane, which solves the problem in the related art that the adhesive layer in the insertion gap of the prefabricated interlocking lap waterproofing membrane easily sticks the isolation membrane together, resulting in construction difficulties and low strength of the membrane itself.
[0005] The technical solution of the present invention is as follows: A three-base double-channel prefabricated bite overlap waterproof membrane, which includes, from bottom to top, a first isolation membrane, a first permeable reaction adhesive layer, a first polymer membrane base layer, a second permeable reaction adhesive layer, a second polymer membrane base layer, a third permeable reaction adhesive layer, a third polymer membrane base layer, a fourth permeable reaction adhesive layer and a surface layer. The surface layer is formed by connecting a second isolation membrane and an anti-adhesive layer. An overlap interface is arranged at the second permeable reaction adhesive layer and the third permeable reaction adhesive layer. One end of the second polymer membrane base layer extends into the overlap interface. The second isolation membrane and the overlap interface are respectively located on both sides of the anti-adhesive layer. The inner wall of the overlap interface is provided with a third isolation membrane and a fourth isolation membrane.
[0006] As a further technical solution, the thickness of the first isolation film, the second isolation film, the third isolation film and the fourth isolation film are independently 0.035-0.070 mm.
[0007] As a further technical solution, the thickness of the first polymer film base layer, the second polymer film base layer, and the third polymer film base layer are independently 0.1-0.15 mm.
[0008] As a further technical solution, the length of the overlapped joint is 60-100 mm, and the length of the extended joint is 2-100 mm.
[0009] In the present invention, the extending section of the second polymer film base layer is always within the overlapped interface.
[0010] As a further technical solution, the third isolation membrane is located on the upper surface of the inner wall, and the fourth isolation membrane is located on the lower surface of the inner wall.
[0011] As a further technical solution, the first isolation membrane, the second isolation membrane, the third isolation membrane and the fourth isolation membrane are each independently any flexible organic film, preferably one of PP film, PE film, PVC film, PI film, TPU film, PC film, TPO film, EPDM film, TPE film, TPEE film, PEEK film, PET film, PEN film, CNF film, and PHA film.
[0012] As a further technical solution, the raw materials of the first polymer film base layer, the second polymer film base layer, and the third polymer film base layer can each independently be any polymer film in the art, preferably one of PP film, PE film, PVC film, PI film, TPU film, PC film, TPO film, EPDM film, TPE film, TPEE film, PEEK film, PET film, PEN film, CNF film, and PHA film, more preferably PET film.
[0013] As a further technical solution, the raw material of the anti-sticking layer includes one of PE film, PP film, mineral sand, natural sand, and recycled concrete sand.
[0014] As a further technical solution, when the raw material of the anti-sticking layer includes natural sand, the natural sand includes one or more of river sand, lake sand, and desert sand.
[0015] As a further technical solution, when the raw material of the anti-sticking layer includes mineral sand, the mineral sand includes one or more of quartz sand, mullite sand, and sintered sand.
[0016] As a further technical solution, the raw materials of the first permeable reaction adhesive layer, the second permeable reaction adhesive layer, the third permeable reaction adhesive layer and the fourth permeable reaction adhesive layer independently include the following components in parts by mass: 30-40 parts of asphalt, 1-3 parts of carboxylated styrene-butadiene rubber, 5-15 parts of SBS, 2-5 parts of tackifier, 3-8 parts of plasticizer, 0.1-1 part of antioxidant, and 25-45 parts of modified filler, and the modified filler includes a polyurethane modified filler and a poly (N-isopropylacrylamide) modified filler.
[0017] In the present invention, SBS is a styrene-butadiene-styrene block copolymer.
[0018] In the present invention, polyurethane modified filler and poly-N-isopropylacrylamide modified filler are used in combination in the raw materials of the reactive adhesive layer, thereby further improving the strength of the waterproof coiled material.
[0019] As a further technical solution, the tackifier may be any one or more tackifiers in the art, preferably one or two of petroleum resin and rosin resin.
[0020] As a further technical solution, the plasticizer may be any one or more plasticizers in the art, preferably one or both of dibutyl phthalate and dioctyl phthalate.
[0021] As a further technical solution, the antioxidant may be any one or more antioxidants in the art, preferably one or two of antioxidant 1010 and antioxidant 168.
[0022] As a further technical solution, the mass of the polyurethane modified filler is ≥ the mass of the poly (N-isopropylacrylamide) modified filler.
[0023] The present invention limits the mass of the polyurethane modified filler to be greater than or equal to the mass of the poly-N-isopropylacrylamide modified filler, thereby further improving the strength of the waterproof coiled material.
[0024] As a further technical solution, the mass of the polyurethane modified filler is greater than the mass of the poly (N-isopropylacrylamide) modified filler.
[0025] The present invention limits the mass of the polyurethane modified filler to be greater than the mass of the poly-N-isopropylacrylamide modified filler, thereby further improving the strength of the waterproof coiled material.
[0026] As a further technical solution, the mass ratio of the polyurethane modified filler to the poly (N-isopropylacrylamide) modified filler is 4:1 to 5:2.
[0027] The present invention limits the mass ratio of the polyurethane modified filler to the poly (N-isopropylacrylamide) modified filler to 4:1-5:2, thereby further improving the strength of the waterproof coiled material.
[0028] As a further technical solution, the raw materials of the polyurethane modified filler include a first filler and polyurethane in a mass ratio of 1:0.05~0.3; the raw materials of the poly (N-isopropylacrylamide) modified filler include a second filler and poly (N-isopropylacrylamide) in a mass ratio of 1:0.05~0.3.
[0029] As a further technical solution, the preparation method of the polyurethane modified filler includes the following steps: uniformly mixing polyurethane, a first filler and a solvent, separating the solid and the liquid, and drying to obtain the polyurethane modified filler; the preparation method of the poly (N-isopropylacrylamide) modified filler includes the following steps: uniformly mixing poly (N-isopropylacrylamide), a second filler and a solvent, separating the solid and the liquid, and drying to obtain the poly (N-isopropylacrylamide) modified filler.
[0030] As a further technical solution, the first filler and the second filler independently include one or more of talcum powder, carbon black, and heavy calcium powder.
[0031] As a further technical solution, the preparation methods of the first permeable reaction adhesive layer, the second permeable reaction adhesive layer, the third permeable reaction adhesive layer and the fourth permeable reaction adhesive layer each independently include the following steps: heating the asphalt to 180-190°C, mixing it evenly with carboxylated styrene-butadiene rubber, SBS and modified filler, cooling it to 135-140°C, adding the remaining components and mixing.
[0032] As a further technical solution, the raw materials of the first permeable reaction adhesive layer, the second permeable reaction adhesive layer, the third permeable reaction adhesive layer and the fourth permeable reaction adhesive layer each independently further include 1 to 7 parts of styrene-acryl alcohol copolymer resin.
[0033] The present invention further adds 1 to 7 parts of styrene-acryl alcohol copolymer resin into the reactive adhesive layer, thereby further improving the strength of the waterproof coiled material.
[0034] As a further technical solution, the mass ratio of the styrene-acryl alcohol copolymer resin to the polyurethane modified filler is 3~5:25.
[0035] The invention limits the mass ratio of the styrene-acryl alcohol copolymer resin to the polyurethane modified filler to 3-5:25, thereby further improving the strength of the waterproof coiled material.
[0036] As a further technical solution, the preparation methods of the first permeable reaction adhesive layer, the second permeable reaction adhesive layer, the third permeable reaction adhesive layer and the fourth permeable reaction adhesive layer each independently include the following steps: heating the asphalt to 180-190°C, mixing it evenly with carboxylated styrene-butadiene rubber, SBS and polyurethane modified filler, then adding poly (N-isopropylacrylamide) modified filler and continuing to mix evenly, cooling it to 135-140°C, adding the remaining components and mixing.
[0037] In the present invention, the polyurethane modified filler and the poly (N-isopropylacrylamide) modified filler are added separately. The polyurethane modified filler is added first, and the dispersion of the polyurethane modified filler is improved through the interaction between the polyurethane modified filler and asphalt, and the compatibility with the base material is improved. Subsequently, the poly (N-isopropylacrylamide) modified filler is added, and the interaction between the poly (N-isopropylacrylamide) modified filler and the polyurethane modified filler not only improves the dispersion of the poly (N-isopropylacrylamide) modified filler and the compatibility with the base material, but also increases the crosslinking degree of the system, thereby further improving the strength of the waterproof membrane.
[0038] The working principle and beneficial effects of the present invention are: The present invention provides a three-base double-pass prefabricated occlusal overlap waterproofing membrane, by setting a second polymer film base between the second permeable reaction adhesive layer and the third permeable reaction adhesive layer, using three polymer film bases to divide the permeable reaction adhesive layer into four regions as four permeable reaction adhesive layers, and at the same time, one end of the second polymer film base extends into the overlap interface, and the upper and lower layers of the overlap interface are clearly isolated. In the actual production process of the waterproofing membrane, the adhesive layer at the overlap interface will not stick the third isolation membrane and the fourth isolation membrane together, so that the third isolation membrane and the fourth isolation membrane are easy to tear off without excess glue remaining, and the construction is simple. In addition, the setting of the second polymer film base also improves the strength of the prefabricated occlusal overlap waterproofing membrane itself. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0040] Figure 1 This is a schematic diagram of the waterproof membrane structure of the present invention; In the figure: 1 is the first isolation membrane, 2 is the first permeable reaction adhesive layer, 3 is the first polymer film base layer, 4 is the second permeable reaction adhesive layer, 5 is the second polymer film base layer, 6 is the third permeable reaction adhesive layer, 7 is the third polymer film base layer, 8 is the fourth permeable reaction adhesive layer, 9 is the second isolation membrane, 10 is the anti-sticking layer, 11 is the third isolation membrane, and 12 is the fourth isolation membrane. DETAILED DESCRIPTION
[0041] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] The parameters of the raw materials in the following examples and comparative examples are as follows: Asphalt is 90# asphalt; The carboxylated styrene butadiene rubber is an ultrafine powder carboxylated styrene butadiene rubber, with the brand name Narpow VP201, purchased from Beijing Beihuayan Company affiliated to Beijing Chemical Research Institute of Sinopec Corporation; SBS is SBS F875; The petroleum resin is petroleum resin C9; The rosin resin is 424 rosin resin; The talc powder has a silicon dioxide content of 60wt%, a magnesium oxide content of 15wt%, and a particle size of 400 mesh; The carbon black is carbon black N330; Heavy calcium powder is heavy calcium carbonate powder with a particle size of 400 mesh; Polyurethane is TPU S90A from BASF, Germany; The weight average molecular weight of poly-N-isopropylacrylamide is 300,000; The styrene-acrylonitrile copolymer resin is SAA-100 styrene-acrylonitrile copolymer resin.
[0043] Example 1 A three-layer base double-course prefabricated bite-lap waterproof membrane, such as Figure 1 As shown, from bottom to top, it includes a first isolation film, a first permeable reaction adhesive layer, a first polymer film base layer, a second permeable reaction adhesive layer, a second polymer film base layer, a third permeable reaction adhesive layer, a third polymer film base layer, a fourth permeable reaction adhesive layer and a surface layer, the surface layer is formed by connecting the second isolation film and the anti-adhesive layer, an overlapping interface of 80 mm in length is arranged at the second permeable reaction adhesive layer and the third permeable reaction adhesive layer, one end of the second polymer film base layer extends into the overlapping interface by 30 mm, the second isolation film and the overlapping interface are respectively located on both sides of the anti-adhesive layer, the upper surface of the inner wall of the overlapping interface is provided with a third isolation film, and the lower surface of the inner wall of the overlapping interface is provided with a fourth isolation film; The first isolation film, the second isolation film, the third isolation film and the fourth isolation film are all PE films with a thickness of 0.05 mm; The first polymer film base layer, the second polymer film base layer, and the third polymer film base layer are all polyethylene terephthalate films with a thickness of 0.12 mm; The anti-sticking layer is a PE film with a thickness of 0.05 mm; The first permeable reaction adhesive layer, the second permeable reaction adhesive layer, the third permeable reaction adhesive layer and the fourth permeable reaction adhesive layer are all prepared by the following method: after heating 35 parts of asphalt to 185°C, 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS and 35 parts of talcum powder are added and mixed evenly, the temperature is lowered to 135°C, 3.5 parts of petroleum resin, 5 parts of dibutyl phthalate and 0.5 parts of antioxidant 1010 are added and mixed evenly to obtain the product.
[0044] Example 2 A three-base double-channel prefabricated bite overlap waterproof membrane, which comprises, from bottom to top, a first isolation membrane, a first permeable reaction adhesive layer, a first polymer membrane base layer, a second permeable reaction adhesive layer, a second polymer membrane base layer, a third permeable reaction adhesive layer, a third polymer membrane base layer, a fourth permeable reaction adhesive layer and a surface layer, wherein the surface layer is formed by connecting the second isolation membrane and the anti-adhesion layer, a 100 mm long overlap joint is arranged at the second permeable reaction adhesive layer and the third permeable reaction adhesive layer, one end of the second polymer membrane base layer extends into the overlap joint by 100 mm, the second isolation membrane and the overlap joint are respectively located on both sides of the anti-adhesion layer, the third isolation membrane is arranged on the upper surface of the inner wall of the overlap joint, and the fourth isolation membrane is arranged on the lower surface of the inner wall of the overlap joint; The first isolation film, the second isolation film, the third isolation film and the fourth isolation film are all PP films with a thickness of 0.07 mm; The first polymer film base layer, the second polymer film base layer, and the third polymer film base layer are all polyethylene terephthalate films with a thickness of 0.1 mm; The anti-sticking layer is quartz sand with a thickness of 0.07 mm; The first permeable reaction adhesive layer, the second permeable reaction adhesive layer, the third permeable reaction adhesive layer and the fourth permeable reaction adhesive layer are all prepared by the following method: after heating 30 parts of asphalt to 180°C, 1 part of carboxylated styrene-butadiene rubber, 5 parts of SBS and 25 parts of carbon black are added and mixed evenly, the temperature is lowered to 135°C, 2 parts of rosin resin, 3 parts of dioctyl phthalate and 0.1 part of antioxidant 168 are added and mixed evenly to obtain the product.
[0045] Example 3 A three-base double-channel prefabricated bite overlap waterproof membrane, which comprises, from bottom to top, a first isolation membrane, a first permeable reaction adhesive layer, a first polymer membrane base layer, a second permeable reaction adhesive layer, a second polymer membrane base layer, a third permeable reaction adhesive layer, a third polymer membrane base layer, a fourth permeable reaction adhesive layer and a surface layer, wherein the surface layer is formed by connecting the second isolation membrane and the anti-adhesion layer, a 60mm long overlap joint is arranged at the second permeable reaction adhesive layer and the third permeable reaction adhesive layer, one end of the second polymer membrane base layer extends into the overlap joint by 2mm, the second isolation membrane and the overlap joint are respectively located on both sides of the anti-adhesion layer, the third isolation membrane is arranged on the upper surface of the inner wall of the overlap joint, and the fourth isolation membrane is arranged on the lower surface of the inner wall of the overlap joint; The first isolation film, the second isolation film, the third isolation film and the fourth isolation film are all PE films with a thickness of 0.035 mm; The first polymer film base layer, the second polymer film base layer, and the third polymer film base layer are all polyethylene terephthalate films with a thickness of 0.15 mm; The anti-adhesive layer is a PP film with a thickness of 0.035 mm; The first permeable reaction adhesive layer, the second permeable reaction adhesive layer, the third permeable reaction adhesive layer and the fourth permeable reaction adhesive layer are all prepared by the following method: after heating 40 parts of asphalt to 190°C, 3 parts of carboxylated styrene-butadiene rubber, 15 parts of SBS and 45 parts of heavy calcium powder are added and mixed evenly, the temperature is lowered to 140°C, 5 parts of rosin resin, 8 parts of dioctyl phthalate and 1 part of antioxidant 168 are added and mixed evenly to obtain the product.
[0046] Example 4 The only difference from Example 1 is: The first permeation reaction adhesive layer, the second permeation reaction adhesive layer, the third permeation reaction adhesive layer and the fourth permeation reaction adhesive layer are all prepared by the following method: S1, dissolving 7.5 g of polyurethane in 500 mL of a mixed solution of xylene and butyrolactone in a volume ratio of 33:67, adding 50 g of talcum powder and mixing evenly, filtering, and drying to obtain a polyurethane modified filler; S2. Heat 35 parts of asphalt to 185°C, add 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS and 35 parts of polyurethane modified filler and mix well, then cool to 135°C, add 3.5 parts of petroleum resin, 5 parts of dibutyl phthalate and 0.5 parts of antioxidant 1010 and mix well to obtain.
[0047] Example 5 The only difference from Example 1 is: The first permeation reaction adhesive layer, the second permeation reaction adhesive layer, the third permeation reaction adhesive layer and the fourth permeation reaction adhesive layer are all prepared by the following method: S1, dissolving 7.5 g of poly (N-isopropylacrylamide) in 500 mL of water, adding 50 g of talcum powder and mixing evenly, filtering, and drying to obtain a poly (N-isopropylacrylamide) modified filler; S2. Heat 35 parts of asphalt to 185°C, add 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS, and 35 parts of poly (N-isopropylacrylamide) modified filler, mix well, cool to 135°C, add 3.5 parts of petroleum resin, 5 parts of dibutyl phthalate, and 0.5 parts of antioxidant 1010, mix well, and obtain.
[0048] Example 6 The only difference from Example 1 is: The first permeation reaction adhesive layer, the second permeation reaction adhesive layer, the third permeation reaction adhesive layer and the fourth permeation reaction adhesive layer are all prepared by the following method: S1, dissolving 7.5 g of polyurethane in 500 mL of a mixed solution of xylene and butyrolactone in a volume ratio of 33:67, adding 50 g of talcum powder and mixing evenly, filtering, and drying to obtain a polyurethane modified filler; S2, dissolving 7.5 g of poly (N-isopropylacrylamide) in 500 mL of water, adding 50 g of talcum powder and mixing evenly, filtering, and drying to obtain a poly (N-isopropylacrylamide) modified filler; S3. Heat 35 parts of asphalt to 185°C, add 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS and 10 parts of polyurethane modified filler and mix evenly, then add 25 parts of poly (N-isopropylacrylamide) modified filler and continue to mix evenly, cool to 135°C, add 3.5 parts of petroleum resin, 5 parts of dibutyl phthalate and 0.5 parts of antioxidant 1010 and mix evenly to obtain.
[0049] Example 7 The only difference from Example 6 is that: S3. Heat 35 parts of asphalt to 185°C, add 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS and 17.5 parts of polyurethane modified filler and mix well, then add 17.5 parts of poly (N-isopropylacrylamide) modified filler and continue to mix well, cool to 135°C, add 3.5 parts of petroleum resin, 5 parts of dibutyl phthalate and 0.5 parts of antioxidant 1010 and mix well to obtain.
[0050] Example 8 The only difference from Example 6 is that: S3. Heat 35 parts of asphalt to 185°C, add 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS and 20 parts of polyurethane modified filler and mix evenly, then add 15 parts of poly (N-isopropylacrylamide) modified filler and continue to mix evenly, cool to 135°C, add 3.5 parts of petroleum resin, 5 parts of dibutyl phthalate and 0.5 parts of antioxidant 1010 and mix evenly to obtain.
[0051] Example 9 The only difference from Example 6 is that: S3. Heat 35 parts of asphalt to 185°C, add 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS and 25 parts of polyurethane modified filler and mix evenly, then add 10 parts of poly (N-isopropylacrylamide) modified filler and continue to mix evenly, cool to 135°C, add 3.5 parts of petroleum resin, 5 parts of dibutyl phthalate and 0.5 parts of antioxidant 1010 and mix evenly to obtain.
[0052] Example 10 The only difference from Example 6 is that: S3. Heat 35 parts of asphalt to 185°C, add 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS and 28 parts of polyurethane modified filler and mix evenly, then add 7 parts of poly (N-isopropylacrylamide) modified filler and continue to mix evenly, cool to 135°C, add 3.5 parts of petroleum resin, 5 parts of dibutyl phthalate and 0.5 parts of antioxidant 1010 and mix evenly to obtain the product.
[0053] Embodiment 11 The only difference from Example 6 is that: S3. Heat 35 parts of asphalt to 185°C, add 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS and 31 parts of polyurethane modified filler and mix well, then add 4 parts of poly (N-isopropylacrylamide) modified filler and continue to mix well, cool to 135°C, add 3.5 parts of petroleum resin, 5 parts of dibutyl phthalate and 0.5 parts of antioxidant 1010 and mix well to obtain.
[0054] Example 12 The only difference from Example 9 is: S3. Heat 35 parts of asphalt to 185°C, add 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS, and 25 parts of polyurethane modified filler, mix well, then add 10 parts of poly (N-isopropylacrylamide) modified filler and continue to mix well, cool to 135°C, add 1 part of styrene-acryl alcohol copolymer resin, 3.5 parts of petroleum resin, 5 parts of dibutyl phthalate, and 0.5 parts of antioxidant 1010, mix well to obtain.
[0055] Example 13 The only difference from Example 12 is: S3. Heat 35 parts of asphalt to 185°C, add 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS and 25 parts of polyurethane modified filler and mix evenly, then add 10 parts of poly (N-isopropylacrylamide) modified filler and continue to mix evenly, cool to 135°C, add 3 parts of styrene-acryl alcohol copolymer resin, 3.5 parts of petroleum resin, 5 parts of dibutyl phthalate and 0.5 parts of antioxidant 1010 and mix evenly to obtain the product.
[0056] Embodiment 14 The only difference from Example 12 is: S3. Heat 35 parts of asphalt to 185°C, add 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS and 25 parts of polyurethane modified filler and mix well, then add 10 parts of poly (N-isopropylacrylamide) modified filler and continue to mix well, cool to 135°C, add 5 parts of styrene-propylene alcohol copolymer resin, 3.5 parts of petroleum resin, 5 parts of dibutyl phthalate and 0.5 parts of antioxidant 1010 and mix well to obtain.
[0057] Embodiment 15 The only difference from Example 12 is: S3. Heat 35 parts of asphalt to 185°C, add 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS and 25 parts of polyurethane modified filler and mix well, then add 10 parts of poly (N-isopropylacrylamide) modified filler and continue to mix well, cool to 135°C, add 7 parts of styrene-acryl alcohol copolymer resin, 3.5 parts of petroleum resin, 5 parts of dibutyl phthalate and 0.5 parts of antioxidant 1010 and mix well to obtain.
[0058] Example 16 The only difference from Example 14 is that: S3. Heat 35 parts of asphalt to 185°C, add 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS, 25 parts of polyurethane modified filler, and 10 parts of poly (N-isopropylacrylamide) modified filler, mix well, then cool to 135°C, add 5 parts of styrene-acryl alcohol copolymer resin, 3.5 parts of petroleum resin, 5 parts of dibutyl phthalate, and 0.5 parts of antioxidant 1010, mix well, and obtain.
[0059] Embodiment 17 The only difference from Example 14 is that: S3. Heat 35 parts of asphalt to 185°C, add 2 parts of carboxylated styrene-butadiene rubber, 10 parts of SBS, and 10 parts of poly (N-isopropylacrylamide) modified filler, mix well, then add 25 parts of polyurethane modified filler and continue to mix well. Cool down to 135°C, add 5 parts of styrene-acryl alcohol copolymer resin, 3.5 parts of petroleum resin, 5 parts of dibutyl phthalate, and 0.5 parts of antioxidant 1010, mix well to obtain the product.
[0060] Comparative Example 1 The only difference from Example 1 is: A prefabricated bite-jointed overlapping waterproof membrane comprises, from bottom to top, a first insulating membrane, a first permeable reactive adhesive layer, a first polymer membrane base layer, a second permeable reactive adhesive layer, a second polymer membrane base layer, a third permeable reactive adhesive layer and a surface layer. The surface layer is formed by connecting a second insulating membrane and an anti-adhesive layer. An overlapping interface with a length of 80 mm is arranged at one end of the second permeable reactive adhesive layer. The second insulating membrane and the overlapping interface are respectively located on both sides of the anti-adhesive layer. A third insulating membrane is arranged on the upper surface of the inner wall of the overlapping interface, and a fourth insulating membrane is arranged on the lower surface of the inner wall of the overlapping interface.
[0061] The waterproof membranes obtained in Examples 1 to 17 and Comparative Example 1 were tested for tensile properties according to the method in GB / T 23457-2017 "Pre-laid waterproof membranes". The maximum longitudinal tensile force and the maximum transverse tensile force were both the average values of 5 specimens as the final test results, and the test results are recorded in Table 1.
[0062] Table 1 Tensile properties of waterproof membrane
[0063] It can be seen from Table 1 that the waterproof membrane provided by the present invention has good tensile properties, with a maximum longitudinal tensile force of more than 1438 N / 50 mm and a maximum transverse tensile force of more than 1348 N / 50 mm.
[0064] Compared with Comparative Example 1, in Example 1, a second polymer film base layer is arranged between the second permeable reaction adhesive layer and the third permeable reaction adhesive layer, and one end of the second polymer film base layer extends into the overlap interface. The maximum longitudinal tensile force and the maximum transverse tensile force of the waterproof roll obtained in Example 1 are higher than those in Comparative Example 1, indicating that the second polymer film base layer is arranged between the second permeable reaction adhesive layer and the third permeable reaction adhesive layer, which can improve the strength of the waterproof roll. In addition, in the actual production process of the waterproof roll of Example 1, the adhesive layer at the overlap interface will not stick the third isolation film and the fourth isolation film together, so that the third isolation film and the fourth isolation film are easy to tear off without excess glue remaining, and the construction is simple.
[0065] The maximum longitudinal tensile force and the maximum transverse tensile force of the waterproof membrane obtained in Examples 6 to 15 are higher than those in Examples 1 to 5, indicating that the combination of the polyurethane modified filler and the poly (N-isopropylacrylamide) modified filler can further improve the strength of the waterproof membrane.
[0066] The maximum longitudinal tensile force and the maximum transverse tensile force of the waterproof membrane obtained in Examples 7 to 15 are higher than those in Example 6, indicating that the mass of the polyurethane modified filler is ≥ the mass of the poly-N-isopropylacrylamide modified filler, which can further improve the strength of the waterproof membrane.
[0067] The maximum longitudinal tensile force and the maximum transverse tensile force of the waterproof membrane obtained in Examples 8 to 15 are higher than those in Example 7, indicating that the quality of the polyurethane modified filler is greater than the quality of the poly (N-isopropylacrylamide) modified filler, and the strength of the waterproof membrane can be further improved.
[0068] The maximum longitudinal tensile force and the maximum transverse tensile force of the waterproof membrane obtained in Examples 9 to 10 are higher than those in Examples 8 and 11, indicating that the mass ratio of the polyurethane modified filler to the poly (N-isopropylacrylamide) modified filler is 4:1 to 5:2, which can further improve the strength of the waterproof membrane.
[0069] The maximum longitudinal tensile force and the maximum transverse tensile force of the waterproof membrane obtained in Examples 12 to 15 are higher than those in Example 9, indicating that adding styrene-acryl alcohol copolymer resin to the reactive adhesive layer can further improve the strength of the waterproof membrane.
[0070] The maximum longitudinal tensile force and the maximum transverse tensile force of the waterproof membrane obtained in Examples 13 to 14 are higher than those in Examples 12 and 15, indicating that the mass ratio of styrene-acryl alcohol copolymer resin to polyurethane modified filler is 3 to 5:25, which can further improve the strength of the waterproof membrane.
[0071] The maximum longitudinal tensile force and the maximum transverse tensile force of the waterproof membrane obtained in Example 14 are higher than those in Example 16 and Example 17, indicating that the strength of the waterproof membrane can be further improved by adding the polyurethane modified filler and the poly (N-isopropylacrylamide) modified filler separately, and adding the polyurethane modified filler first and then adding the poly (N-isopropylacrylamide) modified filler.
[0072] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A three-base double-pass prefabricated occlusal overlap waterproofing membrane, characterized in that: From bottom to top, it includes a first isolation membrane, a first permeable reaction adhesive layer, a first polymer film base layer, a second permeable reaction adhesive layer, a second polymer film base layer, a third permeable reaction adhesive layer, a third polymer film base layer, a fourth permeable reaction adhesive layer and a surface layer. The surface layer is formed by connecting the second isolation membrane and the anti-adhesive layer. An overlap interface is set at the second permeable reaction adhesive layer and the third permeable reaction adhesive layer. One end of the second polymer film base layer extends into the overlap interface. The second isolation membrane and the overlap interface are respectively located on both sides of the anti-adhesive layer. The inner wall of the overlap interface is provided with a third isolation membrane and a fourth isolation membrane.
2. The three-base double-pass prefabricated occlusal overlap waterproofing membrane according to claim 1, characterized in that: The raw materials of the first permeable reaction adhesive layer, the second permeable reaction adhesive layer, the third permeable reaction adhesive layer and the fourth permeable reaction adhesive layer each independently include the following components in parts by mass: 30-40 parts of asphalt, 1-3 parts of carboxylated styrene-butadiene rubber, 5-15 parts of SBS, 2-5 parts of tackifier, 3-8 parts of plasticizer, 0.1-1 part of antioxidant, and 25-45 parts of modified filler, wherein the modified filler includes a polyurethane modified filler and a poly (N-isopropylacrylamide) modified filler.
3. The three-base double-pass prefabricated occlusal overlap waterproofing membrane according to claim 2, characterized in that: The mass of the polyurethane modified filler is ≥ the mass of the poly (N-isopropylacrylamide) modified filler.
4. The three-base double-pass prefabricated occlusal overlap waterproofing membrane according to claim 3, characterized in that: The mass of the polyurethane modified filler is greater than the mass of the poly (N-isopropylacrylamide) modified filler.
5. The three-base double-pass prefabricated occlusal overlap waterproofing membrane according to claim 4, characterized in that: The mass ratio of the polyurethane modified filler to the poly (N-isopropylacrylamide) modified filler is 4:1-5:
2.
6. The three-base double-pass prefabricated occlusal overlap waterproofing membrane according to claim 2, characterized in that: The raw materials of the polyurethane modified filler include a first filler and polyurethane in a mass ratio of 1:0.05-0.3; the raw materials of the poly (N-isopropylacrylamide) modified filler include a second filler and poly (N-isopropylacrylamide) in a mass ratio of 1:0.05-0.
3.
7. The three-base double-pass prefabricated occlusal overlap waterproofing membrane according to claim 6, characterized in that: The preparation method of the polyurethane modified filler comprises the following steps: uniformly mixing polyurethane, a first filler and a solvent, separating the solid from the liquid, and drying to obtain the polyurethane modified filler; the preparation method of the poly (N-isopropylacrylamide) modified filler comprises the following steps: uniformly mixing poly (N-isopropylacrylamide), a second filler and a solvent, separating the solid from the liquid, and drying to obtain the poly (N-isopropylacrylamide) modified filler.
8. The three-base double-pass prefabricated occlusal overlap waterproofing membrane according to claim 2, characterized in that: The preparation methods of the first permeable reactive adhesive layer, the second permeable reactive adhesive layer, the third permeable reactive adhesive layer and the fourth permeable reactive adhesive layer each independently comprise the following steps: Heat the asphalt to 180-190°C, mix it evenly with carboxylated styrene-butadiene rubber, SBS and modified filler, then cool it to 135-140°C and add the remaining components to mix.
9. A three-base double-pass prefabricated occlusal overlap waterproofing membrane according to any one of claims 2 to 8, characterized in that: The raw materials of the first permeation reaction adhesive layer, the second permeation reaction adhesive layer, the third permeation reaction adhesive layer and the fourth permeation reaction adhesive layer each independently further include 1 to 7 parts of styrene-acryl alcohol copolymer resin.
10. The three-base double-pass prefabricated occlusal overlap waterproofing membrane according to claim 9, characterized in that: The mass ratio of the styrene-acryl alcohol copolymer resin to the polyurethane modified filler is 3-5:25.
Citation Information
Patent Citations
Double-lap-joint polymer waterproof coiled material
CN116769416A
Occlusion type lap joint polymer waterproof material and preparation method thereof
CN118109138A
High-durability, puncture-resistant polymer waterproof coiled material and preparation method therefor
WO2024087525A1
Cited By
Three-tire-base double-prefabricated double-occlusion lap joint waterproof coiled material
CN120503483A
Three-ply base double-channel prefabricated double-bite lap joint waterproof roll
CN120503483B
Three-tire-base double-channel prefabricated occlusion lap joint waterproof coiled material with hook-and-loop fastener
CN121105488A
Three-ply base double-channel prefabricated waterproofing roll with hook-and-loop fastener
CN121105488B
Exposed type double-channel prefabricated three-tire-base occlusion lap joint waterproof coiled material
CN121429136A