A kind of polyamide-imide binder, preparation method and application of positive electrode sheet
By adding amide groups and performing thermal imidation treatment in the lithium-ion battery binder, the problems of poor adhesion and flexibility are solved, the safety and service life of the lithium-ion battery are improved, and the preparation process is simplified. Suitable for different models of lithium battery positive electrode materials.
Patent Information
- Application Number
- CN202411222984.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The adhesives of existing lithium-ion batteries have poor adhesion and flexibility, which leads to thick coating of positive electrode sheets that are prone to cracking, low battery safety and service life, and catalysts and high temperature treatment are required during the preparation process, which increases costs and complex production sex.
Polyamic acid is prepared by polymerization from diamine monomers and dianhydride monomers, and diisocyanate crosslinking is added to form a polyamide-imide binder, which increases amide groups to improve the flexibility and impact resistance of the electrode sheet. , reduces the risk of cracking, and is thermally imidized through the drying process to enhance the binding force and thermal stability of the binder.
Improves the flexibility and impact resistance of the positive electrode sheet, reduces the risk of cracking, extends the service life and safety of the battery, simplifies the preparation process, reduces the cost of raw materials and production complexity, and is suitable for different models of lithium batteries. Positive electrode material.
Smart Images

Figure SMS_11 
Figure QLYQS_1 
Figure QLYQS_4
Abstract
Description
Technical Field
[0001] The invention relates to a polyamide-imide binder, a preparation method of a positive electrode sheet and application thereof, and belongs to the technical field of positive electrode sheets for lithium batteries. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, high operating voltage, light weight, and no pollution. They are widely used in the field of power batteries and are currently in a rapid development stage. With the continuous acceleration of the application of lithium-ion batteries, their safety has also attracted much attention. The binder in lithium-ion batteries (LIBs) can tightly connect the active materials, conductive agents, current collectors, etc. into one, maintain the stability of the electrode structure and the integrity of the electronic channel, and directly affect the safety and cycle stability of LIBs. The design optimization of the binder molecular structure is of great significance to improving the safety and service life of lithium batteries.
[0003] Polyvinylidene fluoride (PVDF) occupies a core position in the field of LIBs binders, mainly relying on the van der Waals force between molecules to bond active materials, conductive agents and current collectors. PVDF has good electrochemical stability and electrolyte wettability. However, PVDF has many disadvantages: for example, it is easy to degrade during the charge and discharge cycle and high-temperature operation, resulting in increased internal resistance, reduced battery rate and cycle performance; gel will be produced during the pulping process, making coating difficult; and toxic fluorine-containing gases will be produced during the high-temperature cutting process of the pole piece.
[0004] Polyimide has the advantages of high temperature resistance, good adhesion, and low expansion rate. It can be designed based on molecular structure to achieve better matching with positive electrode materials, greatly improving the rate capability, safety, and service life of lithium-ion batteries. It has broad development prospects in the field of new lithium battery materials. However, polyimide is highly rigid and has the risk of cracking during coating, rolling, and winding. In the case of thick coating, the cracking phenomenon is more significant, which limits the energy density of the battery.
[0005] Chinese patent application CN111403745A discloses a high temperature resistant adhesive for lithium ion batteries and a battery pole piece using the adhesive. It proposes to prepare polyamic acid by polymerization of functional diamine and dianhydride, add active material and conductive agent to mix, apply it on the current collector, heat it up to perform thermal imidization to form polyimide, and then obtain the battery pole piece. The adhesive has high bonding strength and good high and low temperature performance. However, the pole piece prepared by polyamic acid is relatively brittle, easy to crack, has poor processing performance, and poor battery stability. The addition of functional groups increases the cost of raw materials, and the amount of adhesive used is large, and the battery energy density is low.
[0006] Chinese patent application CN105609780A discloses an electrode binder, a positive electrode material and a lithium-ion battery. The diamine monomer and the dianhydride monomer are polymerized at 160-200°C for 12-24 hours, and a catalyst is added during the imidization process to react at 30-60°C for 2-4 hours, and then at 160-200°C for 12-24 hours. Finally, the polymer binder is purified in a poor solvent to obtain a molecular weight of 1000-50000, which has good thermal stability. The polymer of the invention has a low molecular weight, poor adhesion, easy to fall off, poor battery stability, and short cycle life; it needs to add a catalyst and post-process precipitation, which not only increases the cost of raw materials, but also increases the post-processing steps, generates a large amount of waste liquid, and is not conducive to production.
[0007] Chinese patent CN117447960B discloses a polyimide binder, a positive electrode plate, and a preparation method and application thereof, wherein diamine monomers and dianhydride monomers are polymerized, chemically imidized, and post-treated to obtain a high molecular polymer. This preparation method also requires the addition of a catalyst and post-treatment, which is not conducive to production; although the coating layer has a high peel strength and a high battery capacity retention rate, the binder's imide ring has strong rigidity and there is a risk of cracking during coating, rolling, and winding. When the coating layer thickness is increased, the cracking phenomenon is more significant, limiting the energy density of the battery.
[0008] In summary, existing binders have problems such as poor adhesion and flexibility, easy cracking of thickly coated positive electrode sheets, and low battery safety and service life. Summary of the invention
[0009] In view of the deficiencies in the prior art, the present invention provides a polyamide-imide binder, a method for preparing a positive electrode plate and applications thereof. The polyamide-imide binder adds a portion of amide groups on the basis of polyimide, retains the high tensile strength and elastic modulus of the imide groups, improves the flexibility and impact resistance of the plate, reduces the risk of cracking of thickly coated plates, improves the capacity retention rate and safety of the battery, and prolongs the service life.
[0010] The technical solution of the present invention to solve the above technical problems is as follows: a polyamide-imide binder, wherein the polyamide-imide binder is prepared by polymerizing a diamine monomer and a dianhydride monomer to prepare a polyamic acid intermediate A, and then adding a diisocyanate for cross-linking to obtain a polyamide-imide binder precursor, wherein the polyamide-imide binder precursor is mixed with a conductive agent and a positive electrode material to prepare a slurry and coated to prepare an electrode sheet, and finally converted into the polyamide-imide binder during the drying process of the electrode sheet;
[0011] The dianhydride monomer is , the diamine monomer is , the diisocyanate is , wherein R1~R3 are independently selected from aromatic groups, aliphatic groups or alicyclic groups;
[0012] The structure of the polyamide-imide binder is: , A repeating unit structure.
[0013] Further, the dianhydride monomer is one or a combination of pyromellitic dianhydride, diphenyl ether tetracarboxylic dianhydride, bisphenol A diether dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, and 2,3,4-cyclobutanetetracarboxylic dianhydride;
[0014] The diamine monomers are m-phenylenediamine, p-phenylenediamine, 2,4-toluenediamine, 2,6-toluenediamine, 4,4'-diaminodiphenylmethane, p-phenylenediamine, m-phenylenediamine, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis( Any one or a combination of the following: 4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 2,2'-bis[4-(4-aminophenoxyphenyl)]propane, 4,4'-diaminodiphenyl sulfone, 4,4'-bis(4-aminophenoxy)diphenyl sulfone, 4,4'-diaminobenzanilide, 9,9-bis(4-aminophenyl)fluorene, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,10-diaminodecane, 1,12-diaminododecane, 1,4-cyclohexanediamine, 4,4'-diaminodicyclohexylmethane, and isophoronediamine.
[0015] The diisocyanate is any one or a combination of hexamethylene diisocyanate, p-phenylene diisocyanate, 4,4'-methylenebis(isocyanate), toluene diisocyanate, isophorone diisocyanate, 3,3'-dimethylbiphenyl-4,4'-diisocyanate, 4,4-diisocyanate dicyclohexylmethane, and 1,3-bis(isocyanatomethyl)cyclohexane.
[0016] Furthermore, the number average molecular weight of the polyamide-imide binder is 50,000 to 300,000.
[0017] The present invention also discloses a method for preparing a polyamide-imide binder, wherein the method comprises:
[0018] S1, polymerization: diamine monomers and dianhydride monomers are polymerized in an organic solvent to obtain a polyamic acid intermediate A;
[0019] S2, cross-linking: adding diisocyanate to the reaction system after the polymerization reaction in step S1 for chemical cross-linking to obtain a polyamide-imide binder precursor.
[0020] Furthermore, in step S1, the polymerization reaction temperature is 10-100°C; the molar ratio of the diamine monomer to the dianhydride monomer is 1:(0.8-1.3);
[0021] The mass fraction of the solid content in the polymerization reaction process is 10% to 35%, and the organic solvent is a polar aprotic solvent.
[0022] Furthermore, in step S2, the molar ratio of the diisocyanate to the diamine monomer is 1:(0.05-0.2); and the chemical crosslinking reaction temperature is 40-120°C.
[0023] The present invention also discloses a positive electrode plate, wherein the positive electrode plate comprises the polyamide-imide binder.
[0024] Further, the positive electrode sheet includes 90-99 parts of positive electrode material, 0.5-5 parts of conductive agent, and 0.5-5 parts of polyamide-imide binder precursor in parts by weight, and the positive electrode sheet preparation method is:
[0025] S1. Slurry preparation: adding positive electrode material, conductive agent, binder precursor and solvent in proportion to obtain positive electrode slurry;
[0026] S2, coating: using a coating machine to evenly coat the obtained slurry on the current collector aluminum foil;
[0027] S3, drying: the first stage of drying removes the solvent and CO2, the second stage of drying performs thermal imidization, the polyamide-imide binder precursor becomes polyamide-imide, and finally rolls to obtain the positive electrode sheet;
[0028] The positive electrode material may be one or a combination of lithium iron phosphate, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide;
[0029] The conductive agent may be one or a combination of carbon black, conductive polymer, acetylene black, Ketjen black, carbon fiber, carbon nanotube, graphite.
[0030] The solvent is a high boiling point polar aprotic solvent, which may be, but is not limited to, any one or a combination of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
[0031] The drying conditions of step S3 are: first stage drying temperature 80-160° C., drying time 1-12 h; second stage drying temperature 160-300° C., drying time 1-12 h.
[0032] The invention also discloses the application of a positive electrode plate, and the positive electrode plate is applied in a lithium battery.
[0033] The beneficial effects of the present invention are:
[0034] (1) Due to the strong rigidity of the imide ring of polyimide, there is a risk of cracking during the coating, rolling and winding processes, which reduces the safety of battery use and the capacity retention rate. When the thickness of the coating layer is increased, the cracking phenomenon is more significant, which limits the energy density of the battery. The molecular structure of the polyamide-imide binder described in the present invention contains both amide groups and imide groups. A portion of amide groups is added to the polyimide, and the high tensile strength and elastic modulus of the imide group are retained, thereby improving the flexibility and impact resistance of the pole piece, reducing the risk of cracking of the pole piece, improving the capacity retention rate and safety of the battery, and extending the service life. Thick coating can also be used to increase the energy density of the battery.
[0035] (2) The first step of the reaction to prepare polyamic acid is a conventional reaction that does not require any special equipment. The preparation method is mature and simple. The use of fluorine-free raw materials avoids the generation of hydrogen fluoride in the pulping process that causes gelation, and does not produce toxic fluorine-containing gases in the electrode cutting process. The addition of isocyanate cross-linking in the second step of the reaction can not only increase the number of amide groups, but also increase the viscosity, improve the adhesion between the coating layer and the current collector, reduce the risk of cracking and falling off of the coating layer, and improve the safety and life of the battery. By controlling the amount of isocyanate added, the viscosity can be adjusted, which is suitable for lithium battery positive electrode materials from different manufacturers or models.
[0036] (3) After coating, CO2 is removed through the drying process, so that more pores are formed in the active layer, and the porosity of the positive electrode plate is increased, which can not only increase the migration rate of lithium ions, but also increase the contact area between the positive electrode material and the electrolyte, improve the wettability of the plate, and thus improve the capacity retention rate of the battery. Through the drying process, thermal imidization is carried out, and the polyamic acid undergoes intermolecular or intramolecular cross-linking to form polyimide, which has a more stable structure. It not only improves the binding force of the binder to the active material and the current collector, but also improves the thermal stability of the plate. During the continuous charge and discharge process of the battery, the binder is not easy to degrade, the shedding of the coating layer is reduced, and the battery capacity retention rate is further improved.
[0037] (4) The preparation process of the polyamide-imide binder has mild reaction conditions, low equipment requirements, and is easy to industrialize. The reaction process is simple, no catalyst is used, and the cost of raw materials is reduced. At the same time, the step of post-processing to remove the catalyst is omitted, avoiding the influence of catalyst residue on battery performance; the product does not need precipitation and purification, avoiding solvent waste, and does not generate waste gas, waste liquid, and waste solid, thereby reducing production costs. It can be applied to the field of lithium battery materials and has broad application prospects.
[0038] In summary, the polyamide-imide binder preparation method of the present invention has low raw material cost, simple and reasonable preparation process, easy production, adjustable viscosity of the binder, strong applicability, and good economic benefits. When the polyamide-imide binder is used, the electrode sheet has good wettability and high temperature resistance; the battery has a long cycle life and high safety, and has good application prospects. DETAILED DESCRIPTION
[0039] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, and the present invention is not limited by the specific embodiments disclosed.
[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.
[0041] A polyamide-imide binder, wherein the polyamide-imide binder is prepared by polymerizing a diamine monomer and a dianhydride monomer to prepare a polyamic acid intermediate A, and then adding diisocyanate to crosslink to obtain a polyamide-imide binder precursor, the polyamide-imide binder precursor is mixed with a conductive agent and a positive electrode material to prepare a slurry and apply it to a pole piece, and finally converted into the polyamide-imide binder during the drying process of the pole piece. The specific principle is as follows:
[0042] ;
[0043] , , are dianhydride monomers, diamine monomers and diisocyanates, respectively, wherein R1 to R3 are independently selected from aromatic groups, aliphatic groups or alicyclic groups, A repeating unit structure.
[0044] Specifically, the dianhydride monomer is one or a combination of pyromellitic dianhydride, diphenyl ether tetracarboxylic dianhydride, bisphenol A diether dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, and 1,2,3,4-cyclobutanetetracarboxylic dianhydride;
[0045] Specifically, the diamine monomers are m-phenylenediamine, p-phenylenediamine, 2,4-toluenediamine, 2,6-toluenediamine, 4,4'-diaminodiphenylmethane, p-phenylenediamine, m-phenylenediamine, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis( Any one or a combination of the following: 4-(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 2,2'-bis[4-(4-aminophenoxyphenyl)]propane, 4,4'-diaminodiphenyl sulfone, 4,4'-bis(4-aminophenoxy)diphenyl sulfone, 4,4'-diaminobenzanilide, 9,9-bis(4-aminophenyl)fluorene, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,10-diaminodecane, 1,12-diaminododecane, 1,4-cyclohexanediamine, 4,4'-diaminodicyclohexylmethane, and isophoronediamine.
[0046] Specifically, the diisocyanate is any one or a combination of hexamethylene diisocyanate, p-phenylene diisocyanate, 4,4'-methylenebis(isocyanate), toluene diisocyanate, isophorone diisocyanate, 3,3'-dimethylbiphenyl-4,4'-diisocyanate, 4,4-diisocyanate dicyclohexylmethane, and 1,3-bis(isocyanatomethyl)cyclohexane.
[0047] Specifically, the number average molecular weight of the polyamide-imide binder is 50,000 to 300,000.
[0048] A method for preparing a polyamide-imide binder, the preparation method comprising:
[0049] S1, polymerization: diamine monomers and dianhydride monomers are polymerized in an organic solvent to obtain a polyamic acid intermediate A;
[0050] S2, cross-linking: adding diisocyanate to the reaction system after the polymerization reaction in step S1 for chemical cross-linking to obtain a polyamide-imide binder precursor.
[0051] Specifically, in step S1, the polymerization reaction temperature is 10-100°C, and the reaction time is 1-24h; the molar ratio of the diamine monomer to the dianhydride monomer is 1:(0.8-1.3), and the closer the molar ratio of the diamine monomer to the dianhydride monomer is to 1, the larger the molecular weight, the greater the viscosity, and the better the adhesion.
[0052] The mass fraction of the solid content in the polymerization reaction process is 10% to 35%, and the organic solvent is a high-boiling point polar aprotic solvent, which is but not limited to any one or a combination of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
[0053] Specifically, in step S2, the molar ratio of the diisocyanate to the diamine monomer is 1:(0.05-0.2); and the chemical crosslinking reaction temperature is 40-120°C.
[0054] A positive electrode plate comprises the polyamide-imide binder.
[0055] Specifically, the positive electrode sheet includes 90-99 parts of positive electrode material, 0.5-5 parts of conductive agent, and 0.5-5 parts of polyamide-imide binder precursor in parts by weight;
[0056] The positive electrode material may be one or a combination of lithium iron phosphate, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide;
[0057] The conductive agent may be one or a combination of carbon black, conductive polymer, acetylene black, Ketjen black, carbon fiber, carbon nanotube, graphite.
[0058] More specifically, the positive electrode sheet preparation process is as follows: adding the positive electrode material, conductive agent, and binder precursor into the solvent according to the formula ratio, adjusting the mass fraction of the solid content of the slurry to 40-60%, stirring and mixing at high speed, sieving, coating on aluminum foil, and then drying in two stages and roller pressing to obtain the positive electrode sheet.
[0059] The solvent is a high boiling point polar aprotic solvent, which may be, but is not limited to, any one or a combination of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide.
[0060] The two-stage drying is as follows: the first stage drying temperature is 80-160° C., the drying time is 1-12 hours, and the second stage drying temperature is 160-300° C., the drying time is 1-12 hours.
[0061] The positive electrode plate is used in a lithium battery.
[0062] Example 1
[0063] Preparation of polyamide-imide adhesive:
[0064] Add 4.334g 1,6-diaminohexane, 6.973g m-phenylenediamine and 180.101g N-methylpyrrolidone to a 1000mL three-necked flask in sequence, dissolve, add 52.258g bisphenol A diether dianhydride and 180.101g N-methylpyrrolidone, and react at 10-15°C for 24h. Add 1.251g 4,4'-methylenebis(isocyanate), and continue to react at 50-55°C for 20h. After the reaction is completed, a polyamide-imide binder precursor is obtained.
[0065] Positive electrode preparation:
[0066] In parts by weight, 92 parts of lithium manganese oxide, 4 parts of carbon black and 4 parts of binder precursor were added to a sealed container, and then N-methylpyrrolidone solvent was added to adjust the slurry solid content to 52%, and the mixture was stirred at high speed to mix evenly, and then sieved and coated on aluminum foil. First, vacuum dried at 100°C for 12 hours, then vacuum dried at 200°C for 5 hours, and roller pressed to obtain the positive electrode sheet.
[0067] Example 2
[0068] Preparation of polyamide-imide adhesive:
[0069] Add 11.919g 4,4'-diaminodiphenylmethane, 8.673g 1,8-diaminooctane and 115.934g N,N-dimethylformamide to a 500mL three-necked flask in sequence, dissolve, add 37.375g diphenyl ether tetracarboxylic dianhydride and 115.934g N,N-dimethylformamide, and react at 25-30°C for 16h. Add 2.018g hexamethylene diisocyanate and continue to react at 70-75°C for 10h. After the reaction is completed, a polyamide-imide binder precursor is obtained.
[0070] Positive electrode preparation:
[0071] In parts by weight, 95 parts of lithium cobalt oxide, 2.5 parts of acetylene black and 2.5 parts of binder precursor were added to a sealed container, and then N,N-dimethylformamide solvent was added to adjust the slurry solid content to 45%, and the mixture was stirred at high speed to mix evenly, and then sieved and coated on aluminum foil. First, vacuum dried at 140℃ for 6h, then vacuum dried at 180℃ for 8h, and roller pressed to obtain the positive electrode sheet.
[0072] Example 3
[0073] Preparation of polyamide-imide adhesive:
[0074] Add 5.423g p-phenylenediamine, 7.227g 1,8-diaminooctane and 183.908g N-methylpyrrolidone to a 1000mL three-necked flask in turn. After dissolving, add 52.258g bisphenol A diether dianhydride and 183.908g N-methylpyrrolidone, and react at 50-55℃ for 8h. Add 3.203g p-phenylene diisocyanate and continue to react at 110-115℃ for 2h. After the reaction is completed, a polyamide-imide binder precursor is obtained. Preparation of positive electrode sheet:
[0075] In parts by weight, 98.4 parts of lithium nickel oxide, 0.8 parts of Ketjen black and 0.8 parts of binder precursor were added to a sealed container, and then N-methylpyrrolidone solvent was added to adjust the slurry solid content to 58%, and the mixture was stirred at high speed to mix evenly, sieved, and coated on aluminum foil. The mixture was first vacuum dried at 120°C for 8 hours, then vacuum dried at 160°C for 10 hours, and rolled to obtain the positive electrode sheet.
[0076] Example 4
[0077] Preparation of polyamide-imide adhesive:
[0078] Add 25.898g 1,10-diaminodecane and 102.699g N,N-dimethylacetamide to a 500mL three-necked flask, dissolve, add 9.865g pyromellitic anhydride, 32.703g diphenyl ether tetracarboxylic anhydride and 102.699g N,N-dimethylacetamide, and react at 60-65℃ for 6h. Add 5.001g isophorone diisocyanate, and continue to react at 60-65℃ for 12h. After the reaction is completed, a polyamide-imide binder precursor is obtained.
[0079] Positive electrode preparation:
[0080] In parts by weight, 97.6 parts of lithium iron phosphate, 1.2 parts of carbon nanotubes and 1.2 parts of binder precursor were added to a sealed container, and then N, N-dimethylacetamide solvent was added to adjust the slurry solid content to 57%, and the mixture was stirred at high speed to mix evenly, and then sieved and coated on aluminum foil. First, vacuum dried at 160℃ for 4h, then vacuum dried at 220℃ for 6h, and rolled to obtain the positive electrode sheet.
[0081] Example 5
[0082] Preparation of polyamide-imide adhesive:
[0083] 9.933g 4,4'-diaminodiphenylmethane, 5.811g 1,6-diaminohexane and 90.567g N,N-dimethylformamide were added to a 500mL three-necked flask in sequence. After dissolving, 29.540g 3,3',4,4'-biphenyltetracarboxylic acid dianhydride and 90.567g N,N-dimethylformamide were added and reacted at 70-75℃ for 6h. 1.306g toluene diisocyanate was added and the reaction was continued at 80-85℃ for 6h. The reaction was completed to obtain a polyamide-imide binder precursor.
[0084] Positive electrode preparation:
[0085] In parts by weight, 93 parts of lithium cobalt oxide, 3.5 parts of carbon black and 3.5 parts of binder precursor were added to a sealed container, and then N,N-dimethylformamide solvent was added to adjust the slurry solid content to 55%, and the mixture was stirred at high speed to mix evenly, and then sieved and coated on aluminum foil. First, vacuum dried at 140℃ for 7h, then vacuum dried at 240℃ for 3h, and roller pressed to obtain the positive electrode sheet.
[0086] Example 6
[0087] Preparation of polyamide-imide adhesive:
[0088] 9.650g 4,4'-diaminodiphenyl ether, 12.431g 1,10-diaminodecane and 91.415g N,N-dimethylacetamide were added to a 500mL three-necked flask in sequence. After dissolving, 38.862g 3,3',4,4'-benzophenone tetracarboxylic dianhydride and 91.415g N,N-dimethylacetamide were added and reacted at 80-85°C for 5h. 3.904g 4,4'-methylenebis(isocyanate) was added and the reaction was continued at 100-105°C for 3h. After the reaction was completed, a polyamide-imide binder precursor was obtained.
[0089] Positive electrode preparation:
[0090] In parts by weight, 96 parts of lithium manganese oxide, 2 parts of graphite and 2 parts of binder precursor were added to a sealed container, and then N, N-dimethylacetamide solvent was added to adjust the slurry solid content to 55%, and the mixture was stirred at high speed to mix evenly, and then sieved and coated on aluminum foil. First, vacuum dried at 120℃ for 8h, then vacuum dried at 260℃ for 2h, and roller pressed to obtain the positive electrode sheet.
[0091] Example 7
[0092] Preparation of polyamide-imide adhesive:
[0093] Add 5.209g 1,12-diaminododecane, 20.660g 4,4'-diaminodiphenylmethane and 101.955g N,N-dimethylformamide to a 500mL three-necked flask, dissolve, add 42.100g 3,3',4,4'-benzophenonetetracarboxylic dianhydride and 101.955g N,N-dimethylformamide, and react at 90-95℃ for 4h. Add 1.749g hexamethylene diisocyanate and continue to react at 90-95℃ for 4h. After the reaction is completed, a polyamide-imide binder precursor is obtained.
[0094] Positive electrode preparation:
[0095] In parts by weight, 94 parts of lithium nickel oxide, 3 parts of acetylene black and 3 parts of binder precursor were added to a sealed container, and then N, N-dimethylformamide solvent was added to adjust the slurry solid content to 50%, and the mixture was stirred at high speed to mix evenly, and then sieved and coated on aluminum foil. First, vacuum dried at 150°C for 6 hours, then vacuum dried at 280°C for 1 hour, and roller pressed to obtain the positive electrode sheet.
[0096] Example 8
[0097] Preparation of polyamide-imide adhesive:
[0098] Add 9.982g of 4,4'-diaminodiphenyl sulfone, 12.022g of 1,12-diaminododecane and 108.777g of N-methylpyrrolidone to a 500mL three-necked flask, dissolve, then add 16.192g of 3,3',4,4'-benzophenone tetracarboxylic dianhydride and 108.777g of N-methylpyrrolidone, and react at 100-105°C for 2h. Add p-phenylene diisocyanate and continue to react at 115-120°C for 2h. After the reaction is completed, a polyamide-imide binder precursor is obtained.
[0099] Positive electrode preparation:
[0100] In parts by weight, 91 parts of lithium iron phosphate, 4 parts of Ketjen black and 5 parts of binder precursor were added to a sealed container, and then N-methylpyrrolidone solvent was added to adjust the slurry solid content to 47%, and the mixture was stirred at high speed to mix evenly, and then sieved and coated on aluminum foil. First, vacuum dried at 130°C for 10 hours, then vacuum dried at 300°C for 1 hour, and roller pressed to obtain the positive electrode sheet.
[0101] Comparative Example 1
[0102] The polyamic acid binder was prepared by the same method as in Example 1, except that no isocyanate was added, no crosslinking occurred, and only polyamic acid intermediate A was obtained. The specific preparation process was as follows:
[0103] To a 1000 mL three-necked flask, 4.334 g of 1,6-diaminohexane, 6.973 g of m-phenylenediamine and 180.101 g of N-methylpyrrolidone were added in sequence. After dissolution, 52.258 g of bisphenol A diether dianhydride and 180.101 g of N-methylpyrrolidone were added, and the mixture was reacted at 10-15° C. for 24 h to obtain polyamic acid intermediate A.
[0104] Positive electrode preparation:
[0105] The positive electrode sheet was prepared by the same method as in Example 1, except that the binder precursor was replaced with the polyamic acid intermediate A of this comparative example.
[0106] Comparative Example 2
[0107] The polyimide binder was prepared by the same method as in Example 1, except that no isocyanate was added, no crosslinking occurred, and after obtaining the polyamic acid intermediate A, a cyclizing agent and a cyclizing aid (pyridine and acetic anhydride) were added, and finally the product was precipitated and dried. The specific preparation process was as follows:
[0108] Add 4.334g 1,6-diaminohexane, 6.973g m-phenylenediamine and 180.101g N-methylpyrrolidone to a 1000mL three-necked flask in sequence, dissolve, add 52.258g bisphenol A type diether dianhydride and 180.101g N-methylpyrrolidone, react at 10-15°C for 24h to obtain polyamic acid intermediate A. Add 19.775g pyridine and 25.523g acetic anhydride, and continue to react at 10-15°C for 8h. After the reaction is completed, add dropwise to ethanol to precipitate solids, filter, rinse, and dry at 90°C to obtain a polyimide binder.
[0109] Positive electrode preparation:
[0110] The positive electrode sheet was prepared by the same method as in Example 1, except that the binder precursor was replaced with the polyimide binder of this comparative example.
[0111] Comparative Example 3
[0112] The polyamide-imide binder was prepared by the same method as in Example 1, except that during the preparation of the polyamide-imide binder, the solid content of the cross-linking reaction was reduced. The specific preparation process was as follows:
[0113] 4.334 g 1,6-diaminohexane, 6.973 g m-phenylenediamine and 180.101 g N-methylpyrrolidone were added to a 1000 mL three-necked flask in sequence. After dissolution, 52.258 g bisphenol A diether dianhydride and 180.101 g N-methylpyrrolidone were added, and the mixture was reacted at 10-15°C for 24 hours to obtain polyamic acid intermediate A. 1.251 g 4,4'-methylenebis(isocyanate) and 211.883 g N-methylpyrrolidone were added, and the mixture was reacted at 50-55°C for 20 hours. After the reaction was completed, a polyamide-imide binder precursor was obtained.
[0114] Positive electrode preparation:
[0115] The positive electrode sheet was prepared in the same manner as in Example 1.
[0116] Comparative Example 4
[0117] The polyamide-imide binder was prepared by the same method as in Example 2, except that during the preparation of the polyamide-imide binder, the crosslinking reaction temperature was lowered. The specific preparation process was as follows:
[0118] Add 11.919g 4,4'-diaminodiphenylmethane, 8.673g 1,8-diaminooctane and 115.934g N,N-dimethylformamide to a 500mL three-necked flask in sequence, dissolve, add 37.375g diphenyl ether tetracarboxylic dianhydride and 115.934g N,N-dimethylformamide, and react at 25-30°C for 16h. Add 2.018g hexamethylene diisocyanate and continue to react at 25-30°C for 20h. After the reaction is completed, a polyamide-imide binder precursor is obtained.
[0119] Positive electrode preparation:
[0120] The positive electrode sheet was prepared in the same manner as in Example 2.
[0121] Comparative Example 5
[0122] The polyamide-imide binder was prepared by the same method as in Example 2, except that during the preparation of the polyamide-imide binder, the crosslinking reaction temperature was increased. The specific preparation process was as follows:
[0123] Add 11.919g 4,4'-diaminodiphenylmethane, 8.673g 1,8-diaminooctane and 115.934g N,N-dimethylformamide to a 500mL three-necked flask in sequence. After dissolving, add 37.375g diphenyl ether tetracarboxylic dianhydride and 115.934g N,N-dimethylformamide, and react at 25-30℃ for 16h. Add 2.018g hexamethylene diisocyanate, and react at 140-150℃ for 1h. The gel aggregates into a jelly-like state. The state remains unchanged after cooling. It is still insoluble when N,N-dimethylformamide is added to a solid content of 5%.
[0124] Comparative Example 6
[0125] The polyamide-imide binder was prepared by the same method as in Example 2, except that during the preparation of the polyamide-imide binder, the material ratio of isocyanate in the cross-linking reaction was increased. The specific preparation process was as follows:
[0126] Add 11.919g 4,4'-diaminodiphenylmethane, 8.673g 1,8-diaminooctane and 115.934g N,N-dimethylformamide to a 500mL three-necked flask in sequence. After dissolving, add 37.375g diphenyl ether tetracarboxylic dianhydride and 115.934g N,N-dimethylformamide, and react at 25-30℃ for 16h. Add 6.055g hexamethylene diisocyanate, and react at 70-75℃ for 3h. The gel aggregates into a jelly-like state. The state remains unchanged after cooling. It is still insoluble when N,N-dimethylformamide is added to a solid content of 5%.
[0127] Comparative Example 7
[0128] The polyamide-imide binder was prepared by the same method as in Example 3, except that the pole piece was not subjected to secondary drying. The specific pole piece preparation process was as follows:
[0129] Positive electrode preparation:
[0130] In parts by weight, 98.4 parts of lithium nickel oxide, 0.8 parts of Ketjen black and 0.8 parts of binder precursor were added to a sealed container, and N-methylpyrrolidone solvent was added to adjust the slurry solid content to 58%, and the mixture was stirred at high speed to mix evenly, sieved, and coated on aluminum foil. The mixture was vacuum dried at 120°C for 8 hours, and roller pressed to obtain a positive electrode sheet.
[0131] Comparative Example 8
[0132] The polyamide-imide binder was prepared by the same method as in Example 4, except that the pole piece was directly dried at high temperature. The specific pole piece preparation process was as follows:
[0133] Positive electrode preparation:
[0134] By weight, 97.6 parts of lithium iron phosphate, 1.2 parts of carbon nanotubes and 1.2 parts of binder precursor were added to a sealed container, and then N, N-dimethylacetamide solvent was added to adjust the slurry solid content to 57%, and the mixture was stirred at high speed to mix evenly, sieved, and coated on aluminum foil. The positive electrode was dried at 220℃ in vacuum for 6 hours and rolled to obtain the positive electrode sheet.
[0135] Comparative Example 9
[0136] The purchased Solvay PVDF 5130 was used as a binder and dissolved with N-methylpyrrolidone to a solid content of 5%. The positive electrode was prepared according to the steps and methods of Example 1 and the performance was tested.
[0137] Performance Testing:
[0138] 1. Method for measuring the properties of the polyamide-imide binder precursor obtained in the above examples and comparative examples:
[0139] (1) Use gel permeation chromatography (GPC) to measure the number average molecular weight Mw;
[0140] (2) Use a cone and plate viscometer to test the viscosity of a 5% solid content binder.
[0141] 2. Positive electrode performance test method:
[0142] (1) Thickness test: Use a Japanese Mitutoyo digital thickness gauge to test. The total thickness of the positive electrode sheet minus the thickness of the uncoated current collector is recorded as the coating layer thickness.
[0143] (2) Porosity test: Use tweezers to select >20 discs with good appearance and no powder falling off the edges and put them into the sample cup. Record the number of discs and calculate the apparent volume. Then place the sample cup in the true density tester, close the test system, and introduce helium according to the procedure. By detecting the gas pressure in the sample chamber and the expansion chamber, calculate the real volume according to Bohr's law (PV=nRT), and then obtain the porosity of the sample to be tested. Among them, the porosity result output by the electrode does not deduct the substrate.
[0144] (3) Liquid absorption rate test: Use a capillary to absorb electrolyte to a certain height, place the capillary in contact with a dry electrode, and measure the time from the electrolyte level starting to drop to the time the electrolyte is completely absorbed by the electrode.
[0145] Liquid absorption rate = (capillary bottom area × electrolyte height × electrolyte density) ÷ time.
[0146] (4) Flexibility test: Bend the electrode 180° toward the current collector and observe the crease state of the electrode under an optical microscope. Repeat three times: intact is marked as +, with a break but not falling off is marked as ○, and falling off or cracking is marked as ×.
[0147] (5) Peel strength test: The obtained electrode was cut into 10 cm × 2 cm strips and fixed to a 1 mm thick steel plate with double-sided tape on the current collector side. Transparent tape was pasted on the coating layer and a 180° pulling peeling test was performed using a universal material testing machine at a peeling speed of 10 cm / min.
[0148] 3. Battery performance test:
[0149] The button cells were assembled in a glove box, and then the first efficiency at a current density of 0.1C and the capacity retention rate after 500 cycles at a current density of 1C were tested.
[0150] 0.1C first efficiency / % = 0.1C first cycle discharge specific capacity (mAh / g) ÷ 0.1C first cycle charge specific capacity (mAh / g) × 100%.
[0151] 1C capacity retention rate / % = 1C 500th cycle discharge capacity (mAh / g) ÷ 1C first cycle discharge capacity (mAh / g) × 100%.
[0152] Table 1 Performance test results
[0153]
[0154] Comparative Example 1 does not add isocyanate crosslinking, and only prepares polyamic acid. Compared with Example 1, it can be seen that the viscosity of the binder in Comparative Example 1 is low, resulting in poor adhesion between the coating layer and the current collector and low peel strength; without amide groups, the pole piece has poor flexibility, and the coating is prone to cracking and falling off. Although the first effect of the battery is not affected, the capacity retention rate is greatly reduced. This shows that adding isocyanate crosslinking can further improve adhesion, and the introduction of amide groups can improve the flexibility of the pole piece, and the coating layer does not crack or fall off, ensuring the structural integrity and chemical stability of the battery during the cycle.
[0155] In Comparative Example 2, no isocyanate was added for crosslinking, but a cyclizing agent and a dehydrating agent were added, and polyimide was prepared after precipitation and purification. The molecular weight and viscosity of the binder were slightly improved compared with those in Comparative Example 1, but much lower than those in Example 1. The flexibility of the pole piece was improved compared with that in Comparative Example 1, and the coating layer did not fall off. However, after being bent 180° three times, obvious fracture marks could still be observed through an optical microscope, and the flexibility was still different from that in Example 1. Moreover, the capacity retention rate of the battery was 16.73% lower than that in Example 1. This indicates that in the case of thick coating, the pole piece cracking phenomenon occurs when polyamic acid or polyimide is used as a binder, which poses a safety risk and limits the energy density of the battery.
[0156] During the preparation of the binder in Comparative Example 3, the solid content of the cross-linking reaction is reduced, and the molecular weight and viscosity of the binder, the flexibility and peel strength of the electrode, and the battery performance are significantly different from those in Example 1, but are similar to those in Comparative Example 1, indicating that when the solid content is low, the cross-linking reaction is not easy to occur, and the adhesion cannot be improved, nor can the flexibility of the electrode and the battery performance be improved.
[0157] During the preparation of the binder in Comparative Example 4, the cross-linking reaction temperature was relatively low, and the molecular weight and viscosity of the binder, the flexibility and peel strength of the electrode, and the battery performance were significantly different from those in Example 2, indicating that when the cross-linking temperature is low, the cross-linking reaction is not easy to occur. Even if the cross-linking reaction time is doubled, the adhesion cannot be improved, and the flexibility of the electrode and the battery performance cannot be improved.
[0158] In the preparation process of the binder in Comparative Example 5, the crosslinking reaction temperature was relatively high. In the preparation process of the binder in Comparative Example 6, the material ratio of the crosslinking reaction isocyanate was relatively high. The crosslinking degree of the binder was too high during the reaction, and the gel agglomerated into a jelly-like state. The state remained unchanged after cooling, and the solvent could not dissolve it. This shows that during the crosslinking reaction, factors such as temperature, material ratio and solid content have an important influence on the crosslinking degree. When the temperature or solid content is too low, the crosslinking reaction does not occur; when the temperature or material ratio is too high, the crosslinking degree is too high, and the gel is easy to agglomerate.
[0159] The pole piece of comparative example 7 is not subjected to secondary drying. Compared with example 3, the flexibility of the pole piece and the first efficiency of the battery do not change much, but the peel strength is reduced by 69.5 N / m, and the capacity retention rate is reduced by 14.32%, indicating that the second-stage drying is carried out for thermal imidization, and the polyamic acid undergoes intermolecular or intramolecular cross-linking to form polyimide with a more stable structure. It can not only improve the bonding force between the coating layer and the current collector, but also improve the thermal stability of the pole piece. During the continuous charge and discharge process of the battery, the binder is not easily degraded, the shedding of the coating layer is reduced, and the battery capacity retention rate is further improved.
[0160] In Comparative Example 8, the electrode piece is directly subjected to high-temperature drying, and the solvent and CO2 are removed at the same time, and thermal imidization is performed. Compared with Example 4, the electrode piece porosity, liquid absorption rate and peel strength are reduced, the battery first efficiency is reduced to a smaller extent, and the capacity retention rate is reduced by 12.28%, indicating that step-by-step drying is beneficial to the formation of more pores in the active layer, which can not only increase the migration rate of lithium ions, but also increase the contact area between the positive electrode material and the electrolyte, improve the wettability of the electrode piece, and thus improve the capacity retention rate of the battery.
[0161] Comparative Example 9 uses commercial PVDF as a binder. Although the pole piece has good flexibility, the peel strength is 10% to 25% lower than that of the present invention, and the capacity retention rate is 9 to 14% lower than that of the present invention. This shows that the polyamide-imide binder prepared by the present invention has good adhesion, good pole piece flexibility and stability, high battery cyclability and safety, and good application prospects.
[0162] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0163] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.
Claims
1. A polyamide-imide adhesive, characterized in that: The polyamide-imide binder is prepared by polymerization of a diamine monomer and a dianhydride monomer to form a polyamide acid intermediate A, and then adding diisocyanate for chemical crosslinking to obtain a polyamide-imide binder precursor. The polyamide-imide binder precursor is mixed with a conductive agent and a positive electrode material to prepare a slurry for coating to prepare an electrode sheet, and finally converted into the polyamide-imide binder during the drying process of the electrode sheet; The dianhydride monomer is , the diamine monomer is , the diisocyanate is , wherein R1~R3 are independently selected from aromatic groups, aliphatic groups or alicyclic groups; The structure of the polyamide-imide binder is: , It is a repeating unit structure; The polymerization process is carried out in an organic solvent, and the mass fraction of the solid content in the polymerization reaction is 10% to 35%; The molar ratio of the diisocyanate to the diamine monomer is 1:(0.05-0.2); the reaction temperature of the chemical crosslinking is 40-120°C; The drying process is as follows: a first drying step to remove the solvent and CO2, and a second drying step to perform thermal imidization, so that the polyamide-imide binder precursor becomes a polyamide-imide binder.
2. A polyamide-imide adhesive according to claim 1, characterized in that: The dianhydride monomer is one or a combination of pyromellitic acid dianhydride, diphenyl ether tetracarboxylic acid dianhydride, bisphenol A type diether dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, 3,3',4,4'-benzophenone tetracarboxylic acid dianhydride, 2,3,3',4'-biphenyltetracarboxylic acid dianhydride, and 1,2,3,4-cyclobutanetetracarboxylic acid dianhydride; The diamine monomers are m-phenylenediamine, p-phenylenediamine, 2,4-toluenediamine, 2,6-toluenediamine, 4,4'-diaminodiphenylmethane, p-phenylenediamine, m-phenylenediamine, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis( Any one or a combination of 4,4'-diaminobenzylamine, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,10-diaminodecane, 1,12-diaminododecane, 1,4-cyclohexanediamine, 4,4'-diaminodicyclohexylmethane, and isophoronediamine; The diisocyanate is any one or a combination of hexamethylene diisocyanate, p-phenylene diisocyanate, 4,4'-methylenebis(isocyanate), toluene diisocyanate, isophorone diisocyanate, 3,3'-dimethylbiphenyl-4,4'-diisocyanate, 4,4-diisocyanate dicyclohexylmethane, and 1,3-bis(isocyanatomethyl)cyclohexane.
3. A polyamide-imide adhesive according to any one of claims 1-2, characterized in that: The number average molecular weight of the polyamide-imide binder is 50,000 to 300,000.
4. A method for preparing a polyamide-imide binder according to any one of claims 1 to 3, characterized in that: The preparation method is: S1, polymerization: diamine monomers and dianhydride monomers are polymerized in an organic solvent to obtain a polyamic acid intermediate A; S2, cross-linking: adding diisocyanate to the reaction system after the polymerization reaction in step S1 for chemical cross-linking to obtain a polyamide-imide binder precursor.
5. The method for preparing a polyamide-imide adhesive according to claim 4, characterized in that: In step S1, the polymerization reaction temperature is 10-100°C; the molar ratio of the diamine monomer to the dianhydride monomer is 1:(0.8-1.3); and the organic solvent is a polar aprotic solvent.
6. A positive electrode sheet, characterized in that: The positive electrode plate includes the polyamide-imide binder according to any one of claims 1 to 3.
7. A positive electrode sheet according to claim 6, characterized in that: According to the weight percentage, the positive electrode sheet includes 90-99 parts of positive electrode material, 0.5-5 parts of conductive agent, and 0.5-5 parts of polyamide-imide binder precursor. The preparation method of the positive electrode sheet is as follows: S1. Slurry preparation: adding positive electrode material, conductive agent, polyamide-imide binder precursor, and solvent in proportion to obtain positive electrode slurry; S2, coating: using a coating machine to evenly coat the obtained slurry on the current collector aluminum foil; S3, drying: the first stage of drying removes the solvent and CO2, the second stage of drying performs thermal imidization, the polyamide-imide binder precursor becomes polyamide-imide, and finally rolls to obtain the positive electrode sheet; The positive electrode material is one or a combination of lithium iron phosphate, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide; The conductive agent is one or a combination of carbon black, conductive polymer, carbon fiber, carbon nanotube, and graphite.
8. A positive electrode sheet according to claim 7, characterized in that: The drying conditions of step S3 in the preparation method are: a first-stage drying temperature of 80-160° C. and a drying time of 1-12 h; a second-stage drying temperature of 160-300° C. and a drying time of 1-12 h.
9. An application of the positive electrode sheet according to any one of claims 6 to 8, characterized in that: The positive electrode plate is used in a lithium battery.
Citation Information
Patent Citations
Electrode binder, positive electrode material and lithium ion battery
CN105609780A
High-temperature-resistant adhesive for lithium ion battery and battery pole piece applying the adhesive
CN111403745A
A polyimide binder, anode electrode sheet and preparation method and application thereof
CN117447960B
Polyimide foam and preparation method thereof
CN103232599A
Polyimide binder, positive pole piece as well as preparation method and application of positive pole piece
CN117447960A