Matting gloss oil and application

By properly proportioning matt resin, bright resin, additives and special microspheres in matt varnish, and adopting a specific mixing process, the problem of unbalanced performance of existing matt varnish is solved and high mattness and good physical properties are achieved. and leveling properties, suitable for coating of high-end leather products, improving the overall performance and competitiveness of the product.

CN118755889APending Publication Date: 2024-10-11CHENGDU PENGZHOU MINGZHONG CHEM CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410906996.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing matt varnishes are difficult to achieve a balance of overall performance in terms of mattness, physical properties, transparency, leveling and feel, and cannot meet the high requirements for these properties of high-end leather products.

Method used

Using components such as matting resin, bright resin, additives and special microspheres, a new matting varnish is prepared through a specific ratio and stirring process, including 15 to 30 parts of matting resin and 25 to 35 parts of bright resin. 0.8 to 2.7 parts of agent, 1 to 4 parts of special microspheres and 55 to 70 parts of deionized water to ensure the comprehensive performance of the product.

Benefits of technology

It achieves the high matting degree, good physical properties, transparency and leveling properties, durability and naturalness of the matting varnish. It is suitable for coating of high-end leather products and enhances the competitiveness of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004932429050000021
    Figure BDA0004932429050000021
  • Figure BDA0004932429050000022
    Figure BDA0004932429050000022
  • Figure BDA0004932429050000081
    Figure BDA0004932429050000081
Patent Text Reader

Abstract

The invention relates to the technical field of leather manufacturing, and provides extinction gloss oil and application thereof.The extinction gloss oil is prepared from, by weight, 15-30 parts of extinction resin, 25-35 parts of bright resin, 0.8-2.7 parts of auxiliaries, 1-4 parts of special microspheres and 55-70 parts of deionized water. The extinction gloss oil disclosed by the invention has good comprehensive performance, mainly embodied in the aspects of extinction degree, physical property, transparency and leveling property, is expected to be applied to the tanning industry in China, and is specifically applied to the surface of a leather product as a coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of leather products, and in particular relates to a matte varnish and its application. Background Art

[0002] Leather finishing varnish is one of the most important chemical materials in the leather industry. This is because varnish is the material on the outermost layer of leather and gives consumers the most intuitive feeling. At the same time, the performance of varnish determines the protective effect of the coating to a large extent.

[0003] There are many styles and types of finishing varnishes used in the current leather industry. In recent years, the matte finishing style has become more and more popular among the public, so the use of polyurethane matte varnish has become more and more, and its importance in the leather industry has become more and more important; at the same time, people's requirements for the performance of matte varnish are also getting higher and higher, requiring not only high matte degree of varnish, but also good physical properties, good transparency and good leveling of matte varnish. At the same time, because real leather is a material used only in high-end furniture, the requirements for hand feel are particularly high, and it cannot be polished, that is, the gloss of the leather surface cannot change during use.

[0004] There is no product with such well-balanced performance on the market now, so the development of such a matte varnish will surely have broad market prospects. Summary of the invention

[0005] The purpose of the present application is to provide a matte varnish and a preparation method and application thereof, aiming to solve the problem that there is no matte varnish with well-balanced properties on the market.

[0006] The present invention provides a matte varnish, comprising the following components in parts by weight:

[0007] 15-30 parts of matting resin

[0008] 25-35 parts of bright resin

[0009] Additives 0.8~2.7 parts

[0010] Special microspheres 1 to 4 parts

[0011] 55-70 parts of deionized water.

[0012] As a possible design, a matte varnish includes the following components in parts by weight:

[0013] As a possible design, a matte varnish includes the following components in parts by weight:

[0014] As a possible design, the matte resin includes at least one of the following.

[0015] As a possible design, the bright resin includes at least one of the following.

[0016] As a possible design, the auxiliary agent includes at least one of the following.

[0017] As a possible design, the special microspheres include at least one of the following.

[0018] Beneficial effects of the present invention:

[0019] The matte varnish disclosed in the present invention has good comprehensive performance, which is mainly reflected in matte degree, physical properties, transparency and leveling properties, and is expected to be applied in my country's leather industry, specifically as a coating applied to the surface of leather products.

[0020] The matte varnish disclosed in the present invention has the characteristic of self-matting, that is, no matte filler is added externally, so the durability and naturalness of the matte are much higher than similar products, and it has relatively high competitiveness. DETAILED DESCRIPTION

[0021] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0022] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0023] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0024] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0025] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0026] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0027] The term "PET" is the abbreviation of "Polyethylene terephthalate", which means polyethylene terephthalate; the term "PU" is the abbreviation of "polyurethane", which means polyurethane material and is the abbreviation of polyurethane.

[0028] my country's leather industry is still one of the important pillars of light industry. As a global manufacturing factory, my country's leather products account for more than half of the world's annual production. The surface of leather products is coated with a layer of matte varnish, which is not only used to protect leather products, but also to enhance the gloss of leather products. However, the matte varnishes on the market are all good in one or several aspects, and it is difficult to make a matte varnish with a good balance of performance in all aspects.

[0029] In view of the above problems, the present invention provides a matte varnish, comprising the following components in parts by weight: 15 to 30 parts of matte resin, 25 to 35 parts of bright resin, 0.8 to 2.7 parts of additives, 1 to 4 parts of special microspheres, and 55 to 70 parts of deionized water.

[0030] Wherein, the matte resin includes at least one of, for example.

[0031] The bright resin includes at least one of, for example.

[0032] The auxiliary agent includes at least one of, for example.

[0033] The special microspheres include at least one of, for example.

[0034] As a preferred embodiment, the matte varnish comprises the following components in parts by weight: 20-30 parts of matte resin, 30-35 parts of bright resin, 2-2.7 parts of additives, 3-4 parts of special microspheres, and 65-70 parts of deionized water.

[0035] As a more preferred embodiment, the matte varnish comprises the following components in parts by weight: 20 parts of matte resin, 30 parts of bright resin, 2 parts of additives, 3 parts of special microspheres, and 65 parts of deionized water.

[0036] The present invention also discloses a method for preparing the above-mentioned matt varnish, which specifically comprises the following steps:

[0037] Add deionized water into the dispersion barrel, stir at low speed, then add the feel agent, wetting agent, and thickener one by one until the thickener is completely dissolved, then slowly add the matte resin, bright resin, and special microspheres, stir quickly (1000-1500rpm) for 20-30 minutes after wetting, then switch to low speed (500rpm) and continue stirring for 1 hour.

[0038] Example 1

[0039] This embodiment discloses a matte varnish, the raw material composition of which is shown in Table 1.

[0040] Table 1

[0041] raw material Mass (unit: kg) Polyurethane self-matting resin 15 Deionized waterborne polyurethane 25 Additives 0.8 Polyurethane self-matting microspheres 1 Deionized water 55

[0042] The additives consist of 0.2 kg of feel agent LA-322, 0.3 kg of wetting agent YF-98 and 0.3 kg of thickener PUA-102.

[0043] This embodiment also discloses a method for preparing a matte varnish, comprising the following steps:

[0044] Add deionized water into the dispersion barrel, stir at low speed, then add the feel agent, wetting agent and thickener one by one until the thickener is completely dissolved, then slowly add the polyurethane self-matting resin, deionized water-based polyurethane and polyurethane self-matting microspheres, stir rapidly (1000-1500rpm) for 20-30 minutes after wetting, then switch to low speed (500rpm) and continue stirring for 1 hour.

[0045] Example 2

[0046] This embodiment discloses a matte varnish, and its raw material composition is shown in Table 2.

[0047] Table 2

[0048] raw material Mass (unit: kg) Polyurethane self-matting resin 20 Deionized waterborne polyurethane 30 Additives 2 Polyurethane self-matting microspheres 3 Deionized water 65

[0049] The additives consist of 0.5 kg of feel agent LA-322, 0.8 kg of wetting agent YF-98 and 0.7 kg of thickener PUA-102.

[0050] This embodiment also discloses a method for preparing a matte varnish, comprising the following steps:

[0051] Add deionized water into the dispersion barrel, stir at low speed, then add the feel agent, wetting agent and thickener one by one until the thickener is completely dissolved, then slowly add the polyurethane self-matting resin, deionized water-based polyurethane and polyurethane self-matting microspheres, stir rapidly (1000-1500rpm) for 20-30 minutes after wetting, then switch to low speed (500rpm) and continue stirring for 1 hour.

[0052] Example 3

[0053] This embodiment discloses a matte varnish, and its raw material composition is shown in Table 3.

[0054] Table 3

[0055] raw material Mass (unit: kg) Polyurethane self-matting resin 30 Deionized waterborne polyurethane 35 Additives 2.7 Polyurethane self-matting microspheres 4 Deionized water 70

[0056] The additives consist of 0.8 kg of feel agent LA-322, 1.2 kg of wetting agent YF-98 and 0.7 kg of thickener PUA-102.

[0057] This embodiment also discloses a method for preparing a matte varnish, comprising the following steps:

[0058] Add deionized water into the dispersion barrel, stir at low speed, then add the feel agent, wetting agent and thickener one by one until the thickener is completely dissolved, then slowly add the polyurethane self-matting resin, deionized water-based polyurethane and polyurethane self-matting microspheres, stir rapidly (1000-1500rpm) for 20-30 minutes after wetting, then switch to low speed (500rpm) and continue stirring for 1 hour.

[0059] The matt varnish obtained in Examples 1-3 is now subjected to performance testing, including gloss testing, in accordance with the 60° angle test in GB9754-1988.

[0060] Low temperature flex test: cut the leather sample into 65*40mm leather strips, flex it back and forth 20,000 times at -20℃, and observe whether the leather coating cracks.

[0061] Deionized water resistance test: The skin sample was immersed in tap deionized water at room temperature for 24 hours and then taken out to observe whether the coating had bubbles, whitening and shedding.

[0062] Adhesion test

[0063] Use the self-adhesive tape to stick to the leather coating surface, use a wooden cutting board to scrape and press hard to stick it firmly, then quickly pull it apart from one end at a 90° angle and observe whether there is any coating on the self-adhesive tape that has come off.

[0064] Scratch resistance test

[0065] Rub the surface of the skin-like coating vigorously with cheesecloth 20 times and observe the changes in the coating.

[0066] The test results of various properties are shown in Table 4. It can be seen from Table 4 that the various properties of the matte varnish disclosed in the present invention are well balanced, that is, the comprehensive performance is good.

[0067] Table 4

[0068]

[0069] It can be seen from Table 4 that the matte varnish disclosed in the present invention has good performance in all aspects.

[0070] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A matte varnish, characterized in that: The composition comprises the following components in parts by weight:

2. A matte varnish according to claim 1, characterized in that: The composition comprises the following components in parts by weight:

3. A matte varnish according to claim 2, characterized in that: The composition comprises the following components in parts by weight:

4. A matte varnish according to any one of claims 1 to 3, characterized in that: The matting resin is a polyurethane self-matting resin.

5. A matte varnish according to any one of claims 1 to 3, characterized in that: The bright resin is deionized water-based polyurethane.

6. A matte varnish according to any one of claims 1 to 3, characterized in that: The auxiliary agents are a feel agent, a wetting agent and a thickener.

7. A matte varnish according to any one of claims 1 to 3, characterized in that: The special microspheres are polyurethane self-matting microspheres.

8. Use of the matte varnish according to any one of claims 1 to 7 in the leather field.

9. The use according to claim 8, characterized in that: The matte varnish is applied as paint on the surface of leather products.

Citation Information

Patent Citations

  • Novel polyurethane extinction glass oil

    CN103725178A

  • Leather edge coat

    CN105602429A

  • Preparation method of water-based matting treatment agent for PVC (polyvinyl chloride) automobile leather

    CN108148492A

  • Water-based leather finishing agent and application thereof

    CN112876958A

  • Polyurethane brightener and preparation method thereof

    CN117431014A