Method for researching influence of rare earth on molten steel cleanliness

By using ferrocerium rare earth alloys in the smelting and rolling process of vacuum medium frequency induction furnaces, the impact of different rare earth contents on the cleanliness of molten steel was studied, and the problem of rare earth element contamination in molten steel was solved. It was found that an appropriate amount of rare earths can effectively reduce the T.O content, providing The research basis for the application of rare earths in steel is provided.

CN118755902AInactive Publication Date: 2024-10-11BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410755107.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Rare earth elements easily react with oxygen and sulfur in molten steel to form high melting point oxides, sulfides and oxysulfides, which lead to contamination of molten steel. Existing technologies are difficult to effectively remove and affect the cleanliness of molten steel.

Method used

It is smelted using a 25kg vacuum medium frequency induction furnace, using 10% ferrocerium alloy as the rare earth alloy, and using inert gas protection to control the vacuum degree and heating process. After adding the rare earth alloy, it is evenly melted and then rolled to detect the T.O content in the steel plate. Research Effect of different rare earth contents on the cleanliness of molten steel.

Benefits of technology

It was found that an appropriate amount of rare earths can reduce the T.O content in steel, but if the amount is too high, it will increase. It can only play a purifying role within a suitable range, which provides a reference for research on the application of rare earths in steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004889211080000041
    Figure BDA0004889211080000041
  • Figure BDA0004889211080000051
    Figure BDA0004889211080000051
Patent Text Reader

Abstract

The invention discloses a method for researching the influence of rare earth on the cleanliness of molten steel, and aims at a representative low-carbon steel grade Q235B, 25 kg vacuum medium-frequency induction furnace smelting and rolling tests of rare earth contents with different gradients are carried out, the influence of rare earth on the T.O content in the steel grade is found, and reference is provided for application research of rare earth in steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of application of rare earth in steel, and in particular to a method for studying the influence of rare earth on the cleanliness of molten steel. Background Art

[0002] The outermost layer of the electronic structure of all rare earth elements is S2 structure, so rare earth elements are relatively active metals. After rare earth elements are added to molten steel, they will react chemically with oxygen and sulfur in the molten steel. The affinity of rare earth elements La and Ce with oxygen and sulfur is close to that of magnesium, and slightly inferior to that of calcium. The products formed after rare earth elements La and Ce deoxidize and desulfurize molten steel are mainly rare earth oxides, rare earth sulfides and rare earth oxysulfides.

[0003] The compounds formed after molten steel is treated with rare earth deoxidation and desulfurization have a high melting point and a density close to that of molten steel (the density of molten steel is 7.0g / cm3), which makes it difficult to float and remove them, thus causing pollution of the molten steel. Therefore, rare earth elements are generally not used as deoxidizers and desulfurizers for molten steel.

[0004] 1. The patent "A method for improving the cleanliness of IF steel molten steel" adds carbon powder for pre-deoxidation after converter smelting, achieving precise control of the oxygen content in the molten steel. The present invention conducts smelting and rolling tests in a 25kg vacuum medium frequency induction furnace with different rare earth contents for the representative low-carbon steel grade Q235B, and studies the effects of different rare earth contents on the cleanliness of molten steel.

[0005] 2. The patent "A production method for improving the cleanliness of molten steel for track steel" is based on converter smelting. The high carbon drawing and one-time blowing method is used to control the final carbon content to be above 0.14%, thereby reducing the generation of oxide inclusions from the source. The present invention targets the representative low-carbon steel grade Q235B, and conducts 25kg vacuum medium-frequency induction furnace smelting and rolling tests with different rare earth contents to study the effects of different rare earth contents on the cleanliness of molten steel.

[0006] 3. The patent "A smelting method for improving the cleanliness of molten steel for automobile beams" improves the cleanliness of beam steel by accurately controlling the end composition and temperature of the converter carbon pulling, reducing the oxygen level of molten steel and reducing deoxidation inclusions, optimizing the feeding mode during the steelmaking process, shortening the refining and strong stirring time, reducing the amount of N and H absorbed by molten steel, and the degree of secondary oxidation. The present invention targets the representative low-carbon steel grade Q235B, and conducts 25kg vacuum medium-frequency induction furnace smelting and rolling tests with different rare earth contents to study the effects of different rare earth contents on the cleanliness of molten steel. Summary of the invention

[0007] The purpose of the present invention is to provide a research method for the influence of rare earth on the cleanliness of molten steel, to carry out smelting and rolling tests in a 25kg vacuum medium frequency induction furnace with different rare earth contents, to find the influence of rare earth in the steel on the TO content under different rare earth contents, and to provide a reference for the research on the application of rare earth in steel.

[0008] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0009] The present invention discloses a method for studying the influence of rare earth on the cleanliness of molten steel, which adopts a 25kg vacuum medium frequency induction furnace for smelting and inert gas protection; the rare earth alloy is a ferrocerium alloy, and the total number of experimental furnaces is N furnaces;

[0010] When the vacuum degree is below 200Pa, heating begins. When the power rises to 30kw, the vacuum valve begins to close. At this time, the vacuum degree is 20-30Pa. Protective argon gas is filled to 0.05-0.07MPa. When the temperature rises to 30kw, pure iron begins to melt. When the temperature reaches 35kw, it turns into molten iron with a temperature of 1520±10℃. When the temperature rises to 1520℃-1600℃, the molten steel is completely melted, and the power is reduced to add alloy elements and rare earths. The order of addition is Si, Mn, C, RE. After the alloy is added, it is uniformly added for a certain period of time, and the temperature reaches 1620±10℃ for steel casting;

[0011] The experimental billet is heated to 1200±10℃ with the furnace, and the holding time is 1.3-1.7 hours. The billet is kept in the furnace for 110-130 minutes. The experimental billet is rolled in a continuous rolling process without waiting for the temperature in the middle, and the interval between each rolling pass is increased to ensure the temperature drop gradient between passes. After the billet is removed from the furnace and the iron oxide scale is removed, the rolling temperature is guaranteed to be greater than or equal to 1100℃, and the finished product thickness is 20mm through 9 passes. The interval between passes is adjusted to ensure the final rolling temperature is 900±10℃.

[0012] After the steel ingot is rolled into steel plate, the TO content is tested.

[0013] Furthermore, the rare earth alloy is a 10% ferrocerium alloy.

[0014] Furthermore, the alloy was homogenized for 5 min after addition.

[0015] Furthermore, the detection location is the middle of the steel plate.

[0016] Furthermore, the experimental steel grade is Q235B.

[0017] Furthermore, the chemical composition of the experimental steel grade Q235B by mass percentage is: C≤0.22, Si≤0.35, Mn≤1.40, P≤0.045, S≤0.045, and the rest is Fe and impurities.

[0018] Furthermore, there were a total of 10 experimental furnaces, one of which was without rare earth added for blank comparison. The target rare earth stocks were 20ppm, 50ppm, 100ppm, 200ppm, 300ppm, 400ppm, 500ppm, 700ppm and 900ppm respectively.

[0019] Compared with the prior art, the beneficial technical effects of the present invention are:

[0020] A representative grade of low carbon steel, Q235B, was selected to carry out smelting and rolling tests in a 25kg vacuum medium frequency induction furnace with different rare earth contents. The influence of rare earth in this steel grade on TO content at different rare earth contents was found, which provides a reference for the research on the application of rare earth in steel.

[0021] Adding an appropriate amount of rare earth to steel can play a strong role in purifying molten steel. As the rare earth content in steel increases, the TO content in steel shows a trend of first decreasing → increasing → decreasing → increasing. Rare earth deoxidation in steel can produce rare earth oxide inclusions. An appropriate amount of rare earth in steel can reduce TO in steel, but the higher the rare earth content, the better. Only within the appropriate range can it play a role in purifying molten steel. When the rare earth content in steel is 20ppm and 60ppm, the TO content in steel decreases, and the TO content is 16ppm and 15ppm. When the rare earth content is 330ppm, 400ppm, and 560ppm, the TO content in steel decreases, and the TO content is 11ppm, 14ppm, and 13ppm. DETAILED DESCRIPTION

[0022] A research method for the effect of rare earth on the cleanliness of molten steel:

[0023] The experimental steel grade Q235B was smelted in a 25kg vacuum medium frequency induction furnace with inert gas protection. The rare earth alloy was 10% ferrocerium alloy. A total of 10 experimental furnaces were used, of which 1 furnace was not added with rare earth for blank comparison. The target rare earth stocks were 20ppm, 50ppm, 100ppm, 200ppm, 300ppm, 400ppm, 500ppm, 700ppm, and 900ppm, respectively. The composition range of Q235B steel is shown in Table 1 below.

[0024] Table 1 Experimental steel composition (%)

[0025] Element Name C Si Mn P S Ingredient Range ≤0.22 ≤0.35 ≤1.40 ≤0.045 ≤0.045

[0026] When the vacuum degree is below 200Pa, heating begins. When the power rises to 30kw, the vacuum valve begins to close. At this time, the vacuum degree is about 20-30Pa. Protective argon gas is filled to about 0.06MPa. When the temperature rises to 30kw, pure iron begins to melt. When it reaches 35kw, it turns into molten iron with a temperature of about 1520℃. When the temperature rises to 1520℃-1600℃, the molten steel is completely melted, and the power is reduced to add alloy elements and rare earths. The order of addition is Si, Mn, C, RE. After the alloy is added, it is evenly mixed for about 5 minutes, and the temperature is about 1620℃ for steel casting.

[0027] The experimental billet is heated to 1200±10℃ with the furnace, and the holding time is 1.5 hours. The billet is kept in the furnace for 120 minutes. The experimental billet is rolled in a continuous rolling process without waiting for the temperature, and the interval between each rolling pass is increased to ensure the temperature drop gradient between passes. After the billet is removed from the furnace and the iron oxide scale is removed, the rolling temperature is guaranteed to be greater than or equal to 1100℃, and the finished product thickness is 20mm through 9 passes. The interval between passes is adjusted to ensure the final rolling temperature is 900±10℃.

[0028] After the steel ingot is rolled into a steel plate, the TO content is tested (the testing location is the middle of the steel plate).

[0029] Example:

[0030] Rare earth is added to steel, and the rare earth stock and gas O content are shown in Table 1.

[0031] Table 1 Rare earth stock and gas (O, N) content

[0032]

[0033]

[0034] From the experimental data, it can be seen that as the rare earth content in steel increases, the TO content in steel shows a trend of first decreasing → increasing → decreasing → increasing. There is a small amount of rare earth in the steel. When the rare earth content is 20ppm and 60ppm, the TO content in the steel decreases, and the TO content is 16ppm and 15ppm. The rare earth content of the steel increases, and the rare earth content is 200ppm. The TO content in the steel increases, and the TO content is 37ppm and 18ppm. As the rare earth content in the steel increases further, when the rare earth content is 330ppm, 400ppm, and 560ppm, the TO content in the steel decreases again, and the TO content is 11ppm, 14ppm, and 13ppm. When the rare earth content in the steel is 670ppm and 860ppm, the TO content in the steel increases again, and the TO content is 22ppm and 44ppm. Rare earth deoxidation in steel can produce rare earth oxide inclusions. The presence of an appropriate amount of rare earth in steel can reduce TO in the steel, but the higher the rare earth content, the better. Only within the appropriate range can it play a role in purifying molten steel.

[0035] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for studying the influence of rare earth on the cleanliness of molten steel, characterized in that: A 25kg vacuum medium frequency induction furnace was used for smelting, and inert gas protection was used; the rare earth alloy was ferrocerium alloy, and the total number of experimental furnaces was N; When the vacuum degree is below 200Pa, heating begins. When the power rises to 30kw, the vacuum valve begins to close. At this time, the vacuum degree is 20-30Pa. Protective argon gas is filled to 0.05-0.07MPa. When the temperature rises to 30kw, pure iron begins to melt. When the temperature reaches 35kw, it turns into molten iron with a temperature of 1520±10℃. When the temperature rises to 1520℃-1600℃, the molten steel is completely melted, and the power is reduced to add alloy elements and rare earths. The order of addition is Si, Mn, C, RE. After the alloy is added, it is uniformly added for a certain period of time, and the temperature reaches 1620±10℃ for steel casting; The experimental billet is heated to 1200±10℃ with the furnace, and the holding time is 1.3-1.7 hours. The billet is kept in the furnace for 110-130 minutes. The experimental billet is rolled in a continuous rolling process without waiting for the temperature in the middle, and the interval between each rolling pass is increased to ensure the temperature drop gradient between passes. After the billet is removed from the furnace and the iron oxide scale is removed, the rolling temperature is guaranteed to be greater than or equal to 1100℃, and the finished product thickness is 20mm through 9 passes. The interval between passes is adjusted to ensure the final rolling temperature is 900±10℃. After the steel ingot is rolled into steel plate, the TO content is tested.

2. The method for studying the influence of rare earth on the cleanliness of molten steel according to claim 1, characterized in that: The rare earth alloy is 10% ferrocerium alloy.

3. The method for studying the influence of rare earth on the cleanliness of molten steel according to claim 1, characterized in that: After the alloy is added, allow to mix evenly for 5 minutes.

4. The method for studying the influence of rare earth on the cleanliness of molten steel according to claim 1, characterized in that: The detection area is the middle of the steel plate.

5. The method for studying the influence of rare earth on the cleanliness of molten steel according to claim 1, characterized in that: Experimental steel grade: Q235B.

6. The method for studying the influence of rare earth on the cleanliness of molten steel according to claim 1, characterized in that: The chemical composition of the experimental steel grade Q235B by mass percentage is: C≤0.22, Si≤0.35, Mn≤1.40, P≤0.045, S≤0.045, and the rest is Fe and impurities.

7. The method for studying the influence of rare earth on the cleanliness of molten steel according to claim 1 or 6, characterized in that: There were a total of 10 experimental furnaces, one of which was used as a blank comparison without adding rare earth. The target rare earth stocks were 20ppm, 50ppm, 100ppm, 200ppm, 300ppm, 400ppm, 500ppm, 700ppm and 900ppm respectively.

Citation Information

Patent Citations

  • Method for smelting molten steel and adding rear earth by vacuum induction furnace

    CN101649410A

  • Method for smelting ultrahigh-purity ultrahigh-manganese steel containing rare earth

    CN112831715A

  • Method for refining low-carbon microalloyed steel ferrite grains

    CN115323260A

  • Manufacturing method for improving low-temperature toughness of U71Mn steel rail through La-Ce mixed rare earth

    CN115537641A

  • Manufacturing method of high-purity rare earth weather-proof bridge steel

    CN117965998A