Method for determining pseudo-eutectic forming area of aluminum-silicon alloy through melt purification and temperature-controlled solidification
Through melt purification and temperature-controlled solidification methods, the aluminum-silicon alloy is treated with a brine salt purifier to determine its pseudo-eutectic formation area, which solves the problem of reduced mechanical properties of the aluminum-silicon alloy and realizes a high-strength and toughness aluminum-silicon alloy with fine particles. The formation of dense pseudoeutectic structure broadens its application fields.
Patent Information
- Application Number
- CN202410701714.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-11
AI Technical Summary
It is difficult to accurately determine the pseudo-eutectic formation area of aluminum-silicon alloys with existing technology, resulting in a decrease in the mechanical properties of aluminum-silicon alloys. Moreover, the morphology of primary crystal silicon and eutectic silicon in hypereutectic aluminum-silicon alloys is not ideal and prone to fracture.
Using melt purification and temperature-controlled solidification methods, the aluminum-silicon alloy is purified by preparing a halide salt purifier (such as Na3AlF6, NaCl, MgCl2 compound) to completely dissolve the primary silicon, and perform temperature-controlled solidification in the metal mold to determine the aluminum Pseudoeutectic formation region of silicon alloy.
It achieves the formation of fine and dense pseudo-eutectic structures in aluminum-silicon alloys, improves the mechanical properties of the alloy, broadens its application fields, and is simple to operate, low in raw material prices, and environmentally friendly.
Smart Images

Figure CN118755984A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of nonferrous alloy processing, and in particular relates to a method for determining a pseudo-eutectic formation region of an aluminum-silicon alloy by utilizing melt purification and temperature-controlled solidification. Background Art
[0002] Al-Si alloys are increasingly used in the automotive, aviation and other processing and manufacturing industries, such as engine blocks, cylinder liners, brake pads and pistons. This alloy is the most typical lightweight material and an important cast aluminum alloy. It has the advantages of light weight, high wear resistance, high specific strength, good high temperature resistance, excellent castability, outstanding isotropic mechanical properties and low production cost.
[0003] In the casting production of hypereutectic aluminum-silicon alloy, primary silicon and eutectic silicon are mostly polygonal, star-shaped (primary silicon) and coarse needle-shaped (eutectic silicon), and the size and distribution are very unsatisfactory, which makes them prone to fracture and mechanical properties deteriorate. Therefore, it is necessary to refine or eliminate the primary silicon in the alloy and refine the eutectic structure, which is an effective way to obtain good mechanical properties of hypereutectic aluminum-silicon alloy.
[0004] Hypereutectic Al-Si alloy has a simple eutectic phase diagram, such as Fig.19 As shown in the figure, the position of the pseudo-eutectic region is biased towards the Si phase. The metal mold temperature can be controlled to allow the alloy melt to solidify in the pseudo-eutectic region of the aluminum-silicon alloy. The α-Al phase and the Si phase can precipitate and grow simultaneously in the liquid phase, thereby forming a structure with pseudo-eutectic organizational characteristics, thereby improving the comprehensive mechanical properties of the hypereutectic aluminum-silicon alloy. The pseudo-eutectic region in the alloy phase diagram is usually determined by simulation calculation. At present, there has been no report on the experimental analysis and determination of the pseudo-eutectic region of the aluminum-silicon alloy system. Therefore, it is necessary to use effective means to accurately determine the pseudo-eutectic region of the high-silicon hypereutectic aluminum-silicon alloy. Summary of the invention
[0005] In view of the above problems existing in the prior art, the present invention is proposed.
[0006] The purpose of the present invention is to remove impurities and gas from the metal melt by melt purification, and then to achieve thermodynamic supercooling by temperature-controlled solidification to determine the pseudo-eutectic formation region of the aluminum-silicon alloy.
[0007] The present invention provides the following technical solution to solve the above technical problems: using melt purification and temperature-controlled solidification to determine the pseudo-eutectic formation area of aluminum-silicon alloy, including:
[0008] Prepare halide salt purifier; prepare hypereutectic aluminum-silicon alloys with different silicon contents;
[0009] The hypereutectic aluminum-silicon alloy is immersed in a molten halide purifier for smelting and then kept warm to completely dissolve the primary silicon;
[0010] Keep the metal mold warm and quickly pour the alloy melt into the metal mold to form it;
[0011] Based on the solidification structure analysis, the critical temperature of the pseudo-eutectic zone formed in aluminum-silicon alloys with different silicon contents is found, and the pseudo-eutectic formation area of the aluminum-silicon alloy system is determined.
[0012] As a preferred embodiment of the method of the present invention, the halide purifier is compounded by Na3AlF6, NaCl and MgCl2.
[0013] As a preferred embodiment of the method of the present invention, the halide salt purifier, calculated by weight percentage of raw materials, has a Na3AlF6 content of 25%, a NaCl content of 55%, and a MgCl2 content of 20%.
[0014] As a preferred embodiment of the method of the present invention, the smelting temperature is 850° C. and the holding time is 35 minutes.
[0015] As a preferred embodiment of the method of the present invention, the inner cavity size of the metal mold is φ5×100, the temperature of temperature-controlled solidification is 530°C to 380°C, and the insulation time is 3 minutes.
[0016] As a preferred embodiment of the method described in the present invention, the hypereutectic aluminum-silicon alloys with different silicon contents include Al-13%Si, Al-14%Si, Al-15Si, Al-16%Si, Al-17%Si, Al-18%Si, and Al-19%Si hypereutectic aluminum-silicon alloys.
[0017] As a preferred embodiment of the method of the present invention, the temperature gradient of the metal mold insulation temperature is first set to 30°C, and then the approximate temperature range of the pseudo-eutectic zone is obtained based on the solidification structure analysis, and the temperature gradient is further changed to accurately determine the pseudo-eutectic formation area of the Al-Si alloy.
[0018] Optimally, the alloy liquid purified by the melt is subjected to non-equilibrium solidification in a metal mold with a preheating temperature of 530°C to 380°C and an inner cavity size of φ5×100, primary silicon will precipitate in the solidification structure near the upper boundary temperature of the pseudo-eutectic zone, and some primary aluminum will precipitate in the solidification structure near the lower boundary temperature of the pseudo-eutectic zone, and a fine and dense pseudo-eutectic structure will be obtained in the middle area between the upper and lower boundaries of the pseudo-eutectic zone.
[0019] Beneficial effects of the present invention:
[0020] (1) The present invention adopts melt purification and temperature-controlled solidification to determine the pseudo-eutectic formation region of aluminum-silicon alloy, and uses a halide purifier with a composition ratio of 25% Na3AlF6+55% NaCl+20% MgCl2 to cover the alloy liquid to eliminate the adverse effects of factors such as inclusions and gas on the microstructure and performance; to ensure that the solidification temperature is the same as the insulation temperature, after the smelting is completed, the alloy liquid is quickly poured into a metal mold with an inner diameter of 5mm and an insulation temperature of 530℃~380℃ in a pit furnace, so that the alloy melt is quickly supercooled to these temperatures for solidification, thereby achieving thermodynamic supercooling; when the alloy melt is quickly supercooled to the pseudo-eutectic region, a fine and dense pseudo-eutectic structure can be obtained.
[0021] (2) The operation is simple, the raw materials are cheap, and there is no pollution to the environment. Determining the pseudo-eutectic region of aluminum-silicon alloy lays the foundation for obtaining high-strength and high-toughness high-silicon hypereutectic aluminum-silicon alloy, which is of great significance for broadening the application field of hypereutectic aluminum-silicon alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0023] Figure 1 It is the solidification structure diagram of the metal mold temperature in comparative example 1 of the present invention;
[0024] Figure 2 This is a solidification structure diagram of the casting under the condition of a metal mold temperature of 450° C. in Comparative Example 2 of the present invention;
[0025] Figure 3 This is the solidification structure diagram in Comparative Example 3 of the present invention;
[0026] Figure 4 This is the solidification structure diagram in Comparative Example 4 of the present invention;
[0027] Figure 5 This is the solidification structure diagram in Comparative Example 5 of the present invention;
[0028] Figure 6 This is the solidification structure diagram in Comparative Example 6 of the present invention;
[0029] Figure 7 This is the solidification structure diagram in Comparative Example 7 of the present invention;
[0030] Figure 8 This is the solidification structure diagram in Comparative Example 8 of the present invention;
[0031] Fig. 9 This is the solidification structure diagram in Comparative Example 9 of the present invention;
[0032] Fig.10 is the solidification structure diagram in Example 1 of the present invention;
[0033] Fig.11 This is a microstructure diagram of the cross section of the sample in Example 2 of the present invention;
[0034] Fig.12 This is a microstructure diagram of the cross section of the sample in Example 3 of the present invention;
[0035] Fig.13 This is a microstructure diagram of the cross section of the sample in Example 4 of the present invention;
[0036] Fig.14 This is a microstructure diagram of the cross section of the sample in Example 5 of the present invention;
[0037] Fig.15 This is a microstructure diagram of the cross section of the sample in Example 6 of the present invention;
[0038] Fig.16 This is a microstructure diagram of the cross section of the sample in Example 7 of the present invention;
[0039] Fig.17 This is a microstructure diagram of the cross section of the sample in Example 8 of the present invention;
[0040] Fig.18 This is the pseudo-eutectic formation region of the aluminum-silicon alloy determined by melt purification and temperature-controlled solidification in Examples 2 to 8 of the present invention.
[0041] Fig.19 Hypereutectic Al-Si alloy has a simple eutectic phase diagram. DETAILED DESCRIPTION
[0042] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0043] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0044] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0045] Unless otherwise specified, the raw materials used in the examples of the present invention are commercially available.
[0046] The composition of Al-13%Si hypereutectic aluminum-silicon alloy is: Al: balance, Fe: 0.34%, Si: 13%, Cu: 0.02%, Mg: 0.03%, Mn: 0.03%, Zn: 0.02%, Ti: 0.01%, Pb: 0.01%.
[0047] The composition of Al-14%Si hypereutectic aluminum-silicon alloy is: Al: balance, Fe: 0.34%, Si: 14%, Cu: 0.02%, Mg: 0.03%, Mn: 0.03%, Zn: 0.02%, Ti: 0.01%, Pb: 0.01%;
[0048] The composition of Al-15%Si hypereutectic aluminum-silicon alloy is: Al: balance, Fe: 0.34%, Si: 15%, Cu: 0.02%, Mg: 0.03%, Mn: 0.03%, Zn: 0.02%, Ti: 0.01%, Pb: 0.01%;
[0049] The composition of Al-16%Si hypereutectic aluminum-silicon alloy is: Al: balance, Fe: 0.34%, Si: 16%, Cu: 0.02%, Mg: 0.03%, Mn: 0.03%, Zn: 0.02%, Ti: 0.01%, Pb: 0.01%;
[0050] The composition of Al-17%Si hypereutectic aluminum-silicon alloy is: Al: balance, Fe: 0.34%, Si: 17%, Cu: 0.02%, Mg: 0.03%, Mn: 0.03%, Zn: 0.02%, Ti: 0.01%, Pb: 0.01%;
[0051] The composition of Al-18%Si hypereutectic aluminum-silicon alloy is: Al: balance, Fe: 0.34%, Si: 18%, Cu: 0.02%, Mg: 0.03%, Mn: 0.03%, Zn: 0.02%, Ti: 0.01%, Pb: 0.01%;
[0052] The composition of Al-19%Si hypereutectic aluminum-silicon alloy is: Al: balance, Fe: 0.34%, Si: 19%, Cu: 0.02%, Mg: 0.03%, Mn: 0.03%, Zn: 0.02%, Ti: 0.01%, Pb: 0.01%; purchased from Shanghai Xincheng Aluminum, a strong supplier.
[0053] MgCl2, BaCl2, NaCl, KCl, and Na3AlF6 were purchased from Runyou Chemical Co., Ltd.
[0054] The metal mold with an inner cavity size of φ5×100 was purchased from Foshan Shike Chemical Glass Instrument Laboratory.
[0055] Example 1
[0056] Melting at 850℃, using 25%Na3AlF6+55%NaCl+20%MgCl2 halide purifier to purify the melt and keep it warm for 35 minutes, pouring into a metal mold with a preheating temperature of 450℃ and an inner cavity size of φ5×100, the specific operation is as follows:
[0057] Using Al2O3 crucible, place the halide purifier prepared according to the composition ratio of 25% Na3AlF6 + 55% NaCl + 20% MgCl2 in a 850℃ pit furnace to melt in an amount required to completely immerse the alloy;
[0058] Al-17%Si hypereutectic aluminum-silicon alloy was prepared using 99.9wt.% industrial pure aluminum and Al-30Si alloy as raw materials. 10g of Al-17%Si hypereutectic aluminum-silicon alloy was immersed in molten halide purifier. The alloy was smelted at 850℃ and kept warm for 35min. The primary silicon in the solidified structure of Al-17%Si hypereutectic aluminum-silicon alloy was completely dissolved. After adding the purifier, the mixture was stirred to promote uniform reaction. Then, the mixture was left to stand for a while to allow inclusions and gas to float up for easy removal. At the same time, a metal mold with an inner cavity size of φ5×100 was placed in a pit furnace for heat preservation at a temperature of 450℃.
[0059] After the alloy is melted, the alloy melt is quickly poured into a metal mold with an inner cavity size of φ5×100 placed in a pit furnace for molding and kept warm for 3 minutes.
[0060] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Figure 4 shown.
[0061] Fig.10The solidification microstructure of Al-17Si hypereutectic alloy using a halide salt purifier with a composition ratio of 25% Na3AlF6 + 55% NaCl + 20% MgCl2 and cast at a metal mold temperature of 450°C obtained an ideal pseudo-eutectic structure, with eutectic silicon in the form of fine snowflakes and no primary silicon and primary aluminum precipitated. This is because in the purification process of the halide salt purifier with a composition ratio of 25% Na3AlF6 + 55% NaCl + 20% MgCl2, the combination of only three components makes the reaction simple and easy to control, which helps to achieve a consistent purification effect. KCl is usually used in combination with NaCl, which can react with impurities in the melt to form scum, which is easy to remove, but when used alone, the effect of removing certain specific impurities may not be satisfactory. Therefore, choosing NaCl as a purifier can provide sufficient degassing effect and has relatively low material and storage costs. In the purification process, MgCl2 has a significant effect on the removal of magnesium oxides, which helps to refine the eutectic silicon phase. In addition, a slightly higher content of Na3AlF6 can effectively remove oxides and other inclusions in the melt, significantly improve the purification degree and fluidity of the melt, and promote the formation of eutectic structure.
[0062] Example 2
[0063] Al-13Si hypereutectic alloy was melted at 850℃, purified and kept warm for 35 minutes, and then poured into metal molds with inner cavity size of φ5×100 and preheated temperatures of 530℃, 510℃, 500℃, 490℃ and 470℃, respectively. The specific operations are as follows:
[0064] A halide purifier prepared in the proportion of 25% Na3AlF6+55% NaCl+20% MgCl2 is placed in an Al2O3 crucible and melted in a pit furnace at 850°C in an amount required to completely immerse the alloy;
[0065] Al-13%Si hypereutectic aluminum-silicon alloy was prepared using 99.9wt.% industrial pure aluminum and Al-30Si alloy as raw materials. 10g of Al-13%Si hypereutectic aluminum-silicon alloy was immersed in a molten halide purifier. The alloy was smelted at 850°C and kept warm for 35 minutes to completely dissolve the primary silicon in the solidified structure of the Al-13%Si hypereutectic aluminum-silicon alloy. At the same time, a metal mold with an inner cavity size of φ5×100 was placed in a pit furnace for insulation at temperatures of 530°C, 510°C, 500°C, 490°C, and 470°C, respectively.
[0066] After the alloy is melted, the alloy melt is quickly poured into a metal mold with an inner cavity size of φ5×100 placed in a pit furnace for molding and kept warm for 3 minutes.
[0067] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Fig.11 shown.
[0068] Fig.11 This is the solidification structure diagram of Al-13Si hypereutectic aluminum-silicon alloy at different metal mold temperatures after purification treatment. Fig.11 The metal mold temperatures of (a) and (b) are 530℃ and 510℃, respectively. Obvious blocky primary silicon and a small amount of aluminum matrix were observed under a metallographic microscope. Fig.11 The mold temperature of (c) is 500℃, and an ideal pseudo-eutectic structure is observed. The eutectic structure is very dense and fibrous, and no primary silicon and primary aluminum are found. This shows that the solidification point of the Al-13Si hypereutectic aluminum-silicon alloy at a mold temperature of 500℃ is located on the upper boundary of the pseudo-eutectic zone. Fig.11 The metal mold temperatures of (d) and (e) are 490℃ and 470℃, respectively. Obvious primary aluminum was observed through a metallographic microscope, but no primary silicon was found. This indicates that the solidification structure point of the Al-13Si hypereutectic aluminum-silicon alloy at a metal mold temperature of 500℃ is located at the lower boundary line of the pseudo-eutectic zone. In summary, the upper and lower boundaries of the pseudo-eutectic formation zone of the Al-13Si hypereutectic aluminum-silicon alloy are both located at 500℃.
[0069] Example 3
[0070] Al-14Si hypereutectic alloy was melted at 850℃, purified and kept warm for 35 minutes, and then poured into metal molds with inner cavity size of φ5×100 and preheated temperatures of 530℃, 500℃, 490℃, 470℃, 450℃ and 440℃, respectively. The specific operations are as follows:
[0071] A halide purifier prepared in the proportion of 25% Na3AlF6+55% NaCl+20% MgCl2 is placed in an Al2O3 crucible and melted in a pit furnace at 850°C in an amount required to completely immerse the alloy;
[0072] Al-14%Si hypereutectic aluminum-silicon alloy was prepared using 99.9wt.% industrial pure aluminum and Al-30Si alloy as raw materials. 10g of Al-14%Si hypereutectic aluminum-silicon alloy was immersed in a molten halide purifier. The alloy was smelted at 850°C and kept warm for 35 minutes to completely dissolve the primary silicon in the solidified structure of the Al-14%Si hypereutectic aluminum-silicon alloy. At the same time, a metal mold with an inner cavity size of φ5×100 was placed in a pit furnace for insulation at temperatures of 530°C, 500°C, 490°C, 470°C, 450°C, and 440°C, respectively.
[0073] After the alloy is melted, the alloy melt is quickly poured into a metal mold with an inner cavity size of φ5×100 placed in a pit furnace for molding and kept warm for 3 minutes.
[0074] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Fig.12 shown.
[0075] Fig.12 This is the solidification structure diagram of Al-14Si hypereutectic aluminum-silicon alloy at different metal mold temperatures after purification treatment. Fig.12 The metal mold temperatures of (a) and (b) are 530℃ and 500℃, respectively. Obvious blocky primary silicon and a small amount of aluminum matrix were observed under a metallographic microscope. Fig.12 The mold temperatures of (c), (d), and (e) are 490°C, 470°C, and 450°C, and an ideal pseudo-eutectic structure is observed. The eutectic structure is very dense and fibrous, and no primary silicon and primary aluminum are found. This indicates that the solidification point of the Al-14Si hypereutectic aluminum-silicon alloy at a mold temperature of 490°C is located on the upper boundary line of the pseudo-eutectic zone. Fig.12 The metal mold temperature of (f) is 440℃. The primary aluminum is obviously observed by metallographic microscope, but no primary silicon is found. This indicates that the solidification point of the Al-14Si hypereutectic aluminum-silicon alloy at the metal mold temperature of 450℃ is located at the lower boundary line of the pseudo-eutectic zone. In summary, the temperature range of the pseudo-eutectic formation area of the Al-14Si hypereutectic aluminum-silicon alloy is 490℃~450℃.
[0076] Example 4
[0077] Al-15Si hypereutectic alloy is melted at 850℃, purified and kept warm for 35 minutes, and then poured into metal molds with inner cavity size of φ5×100 and preheated temperatures of 530℃, 500℃, 490℃, 480℃, 440℃ and 430℃, respectively. The specific operations are as follows:
[0078] A halide purifier prepared in the proportion of 25% Na3AlF6+55% NaCl+20% MgCl2 is placed in an Al2O3 crucible and melted in a pit furnace at 850°C in an amount required to completely immerse the alloy;
[0079] Al-15%Si hypereutectic aluminum-silicon alloy was prepared using 99.9wt.% industrial pure aluminum and Al-30Si alloy as raw materials. 10g of Al-15%Si hypereutectic aluminum-silicon alloy was immersed in a molten halide purifier. The alloy was smelted at 850°C and kept warm for 35 minutes to completely dissolve the primary silicon in the solidified structure of the Al-15%Si hypereutectic aluminum-silicon alloy. At the same time, a metal mold with an inner cavity size of φ5×100 was placed in a pit furnace for insulation at temperatures of 530°C, 500°C, 490°C, 480°C, 440°C, and 430°C, respectively.
[0080] After the alloy is melted, the alloy melt is quickly poured into a metal mold with an inner cavity size of φ5×100 placed in a pit furnace for molding and kept warm for 3 minutes.
[0081] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Fig.13 shown.
[0082] Fig.13 This is the solidification structure diagram of Al-15Si hypereutectic aluminum-silicon alloy at different metal mold temperatures after purification treatment. Fig.13 The metal mold temperatures of (a), (b), and (c) are 530°C, 500°C, and 490°C, and obvious blocky primary silicon and a small amount of aluminum matrix are observed through a metallographic microscope. Fig.13 The mold temperatures of (d) and (e) are 480°C and 440°C, respectively, and an ideal pseudo-eutectic structure is observed. The eutectic structure is very dense and fibrous, and no primary silicon or primary aluminum is found. This indicates that the solidification point of the Al-15Si hypereutectic aluminum-silicon alloy at a mold temperature of 480°C is located on the upper boundary of the pseudo-eutectic zone. Fig.13 The metal mold temperature of (f) is 430℃. The primary aluminum is obviously observed by metallographic microscope, but no primary silicon is found. This indicates that the solidification point of the Al-15Si hypereutectic aluminum-silicon alloy at the metal mold temperature of 440℃ is located at the lower boundary line of the pseudo-eutectic zone. In summary, the temperature range of the pseudo-eutectic formation zone of the Al-15Si hypereutectic aluminum-silicon alloy is 480℃~440℃.
[0083] Example 5
[0084] Al-16Si hypereutectic alloy is melted at 850℃, purified and kept warm for 35 minutes, and then poured into metal molds with inner cavity size of φ5×100 and preheated temperatures of 530℃, 500℃, 480℃, 470℃, 430℃ and 420℃, respectively. The specific operations are as follows:
[0085] A halide purifier prepared in the proportion of 25% Na3AlF6+55% NaCl+20% MgCl2 is placed in an Al2O3 crucible and melted in a pit furnace at 850°C in an amount required to completely immerse the alloy;
[0086] Al-16%Si hypereutectic aluminum-silicon alloy was prepared using 99.9wt.% industrial pure aluminum and Al-30Si alloy as raw materials. 10g of Al-16%Si hypereutectic aluminum-silicon alloy was immersed in a molten halide purifier. The alloy was smelted at 850°C and kept warm for 35 minutes to completely dissolve the primary silicon in the solidified structure of the Al-16%Si hypereutectic aluminum-silicon alloy. At the same time, a metal mold with an inner cavity size of φ5×100 was placed in a pit furnace for insulation at temperatures of 530°C, 500°C, 480°C, 470°C, 430°C, and 420°C, respectively.
[0087] After the alloy is melted, the alloy melt is quickly poured into a metal mold with an inner cavity size of φ5×100 placed in a pit furnace for molding and kept warm for 3 minutes.
[0088] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Fig.14 shown.
[0089] Fig.14 This is the solidification structure diagram of Al-16Si hypereutectic aluminum-silicon alloy at different metal mold temperatures after purification treatment. Fig.14 The metal mold temperatures of (a), (b), and (c) are 530°C, 500°C, and 480°C, and obvious blocky primary silicon and a small amount of aluminum matrix are observed through a metallographic microscope. Fig.14 The mold temperatures of (d) and (e) are 470°C and 430°C, respectively, and an ideal pseudo-eutectic structure is observed. The eutectic structure is very dense and fibrous, and no primary silicon or primary aluminum is found. This indicates that the solidification point of the Al-16Si hypereutectic aluminum-silicon alloy at a mold temperature of 470°C is located on the upper boundary of the pseudo-eutectic zone. Fig.14 The metal mold temperature of (f) is 420℃. The primary aluminum and a small amount of primary silicon are observed through the metallographic microscope, which indicates that the solidification point of the Al-16Si hypereutectic aluminum-silicon alloy at the metal mold temperature of 430℃ is located at the lower boundary line of the pseudo-eutectic zone. In summary, the temperature range of the pseudo-eutectic formation area of the Al-16Si hypereutectic aluminum-silicon alloy is 470℃~430℃.
[0090] Example 6
[0091] Al-17Si hypereutectic alloy was melted at 850℃, purified and kept warm for 35 minutes, and then poured into metal molds with inner cavity size of φ5×100 and preheated temperatures of 530℃, 500℃, 470℃, 460℃, 420℃, and 410℃, respectively. The specific operations are as follows:
[0092] Using Al2O3 crucible, place the halide purifier prepared according to the composition ratio of 25% Na3AlF6 + 55% NaCl + 20% MgCl2 in a 850℃ pit furnace to melt in an amount required to completely immerse the alloy;
[0093] Al-17%Si hypereutectic aluminum-silicon alloy was prepared using 99.9wt.% industrial pure aluminum and Al-30Si alloy as raw materials. 10g of Al-17%Si hypereutectic aluminum-silicon alloy was immersed in a molten halide purifier. The alloy was smelted at 850°C and kept warm for 35 minutes to completely dissolve the primary silicon in the solidified structure of the Al-17%Si hypereutectic aluminum-silicon alloy. At the same time, a metal mold with an inner cavity size of φ5×100 was placed in a pit furnace for insulation at temperatures of 530°C, 500°C, 470°C, 460°C, 420°C, and 410°C, respectively.
[0094] After the alloy is melted, the alloy melt is quickly poured into a metal mold with an inner cavity size of φ5×100 placed in a pit furnace for molding and kept warm for 3 minutes.
[0095] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Fig.15 shown.
[0096] Fig.15 This is the solidification structure diagram of Al-17Si hypereutectic aluminum-silicon alloy at different metal mold temperatures after purification treatment. Fig.15 The metal mold temperatures of (a), (b), and (c) are 530°C, 500°C, and 470°C, and obvious blocky primary silicon and a small amount of aluminum matrix are observed through a metallographic microscope. Fig.15 The mold temperatures of (d) and (e) are 460°C and 420°C, respectively, and an ideal pseudo-eutectic structure is observed. The eutectic structure is very dense and fibrous, and no primary silicon or primary aluminum is found. This indicates that the solidification point of the Al-17Si hypereutectic aluminum-silicon alloy at a mold temperature of 460°C is located on the upper boundary of the pseudo-eutectic zone. Fig.15The metal mold temperature of (f) is 410℃, and obvious primary aluminum and a small amount of primary silicon are observed through a metallographic microscope, which indicates that the solidification structure point of the Al-16Si hypereutectic aluminum-silicon alloy at a metal mold temperature of 420℃ is located at the lower boundary line of the pseudo-eutectic zone. In summary, the temperature range of the pseudo-eutectic formation area of the Al-17Si hypereutectic aluminum-silicon alloy is 460℃~420℃.
[0097] Example 7
[0098] Al-18Si hypereutectic alloy was melted at 850℃, purified and kept warm for 35 minutes, and then poured into metal molds with inner cavity size of φ5×100 and preheated temperatures of 530℃, 500℃, 460℃, 450℃, 410℃, and 400℃, respectively. The specific operations are as follows:
[0099] A halide purifier prepared in the proportion of 25% Na3AlF6+55% NaCl+20% MgCl2 is placed in an Al2O3 crucible and melted in a pit furnace at 850°C in an amount required to completely immerse the alloy;
[0100] Al-18%Si hypereutectic aluminum-silicon alloy was prepared using 99.9wt.% industrial pure aluminum and Al-30Si alloy as raw materials. 10g of Al-18%Si hypereutectic aluminum-silicon alloy was immersed in a molten halide purifier. The alloy was smelted at 850°C and kept warm for 35 minutes to completely dissolve the primary silicon in the solidified structure of the Al-18%Si hypereutectic aluminum-silicon alloy. At the same time, a metal mold with an inner cavity size of φ5×100 was placed in a pit furnace for heat preservation at temperatures of 530°C, 500°C, 460°C, 450°C, 410°C, and 400°C, respectively.
[0101] After the alloy is melted, the alloy melt is quickly poured into a metal mold with an inner cavity size of φ5×100 placed in a pit furnace for molding and kept warm for 3 minutes.
[0102] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Fig.16 shown.
[0103] Fig.16 This is the solidification structure diagram of Al-18Si hypereutectic aluminum-silicon alloy at different metal mold temperatures after purification treatment. Fig.16 The metal mold temperatures of (a), (b), and (c) are 530°C, 500°C, and 460°C, and obvious blocky primary silicon and a small amount of aluminum matrix are observed through a metallographic microscope. Fig.16The mold temperatures of (d) and (e) are 450°C and 410°C, respectively, and an ideal pseudo-eutectic structure is observed. The eutectic structure is very dense and fibrous, and no primary silicon or primary aluminum is found. This indicates that the solidification point of the Al-18Si hypereutectic aluminum-silicon alloy at a mold temperature of 450°C is located on the upper boundary of the pseudo-eutectic zone. Fig.16 The metal mold temperature of (f) is 400℃, and obvious primary aluminum and a small amount of primary silicon are observed through a metallographic microscope, which indicates that the solidification structure point of the Al-18Si hypereutectic aluminum-silicon alloy at a metal mold temperature of 410℃ is located at the lower boundary line of the pseudo-eutectic zone. In summary, the temperature range of the pseudo-eutectic formation area of the Al-18Si hypereutectic aluminum-silicon alloy is 450℃~410℃.
[0104] Example 8
[0105] Al-19Si hypereutectic alloy is melted at 850℃, purified and kept warm for 35 minutes, and then poured into metal molds with inner cavity size of φ5×100 and preheated temperatures of 530℃, 500℃, 450℃, 440℃, 380℃ and 370℃, respectively. The specific operations are as follows:
[0106] A halide purifier prepared in the proportion of 25% Na3AlF6+55% NaCl+20% MgCl2 is placed in an Al2O3 crucible and melted in a pit furnace at 850°C in an amount required to completely immerse the alloy;
[0107] Al-19%Si hypereutectic aluminum-silicon alloy was prepared using 99.9wt.% industrial pure aluminum and Al-30Si alloy as raw materials. 10g of Al-19%Si hypereutectic aluminum-silicon alloy was immersed in a molten halide purifier. The alloy was smelted at 850°C and kept warm for 35 minutes to completely dissolve the primary silicon in the solidified structure of the Al-19%Si hypereutectic aluminum-silicon alloy. At the same time, a metal mold with an inner cavity size of φ5×100 was placed in a pit furnace for insulation at temperatures of 530°C, 500°C, 450°C, 440°C, 380°C, and 370°C, respectively.
[0108] After the alloy is melted, the alloy melt is quickly poured into a metal mold with an inner cavity size of φ5×100 placed in a pit furnace for molding and kept warm for 3 minutes.
[0109] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Fig.17 shown.
[0110] Fig.17 This is the solidification structure diagram of Al-19Si hypereutectic aluminum-silicon alloy at different metal mold temperatures after purification treatment. Fig.17The metal mold temperatures of (a), (b), and (c) are 530°C, 500°C, and 450°C, and obvious blocky primary silicon and a small amount of aluminum matrix are observed through a metallographic microscope. Fig.17 The mold temperatures of (d) and (e) are 440°C and 380°C, respectively, and an ideal pseudo-eutectic structure is observed. The eutectic structure is very dense and fibrous, and no primary silicon or primary aluminum is found. This indicates that the solidification point of the Al-19Si hypereutectic aluminum-silicon alloy at a mold temperature of 440°C is located on the upper boundary of the pseudo-eutectic zone. Fig.17 The metal mold temperature of (f) is 370℃. The metallographic microscope can be used to observe obvious primary aluminum and a small amount of primary silicon, which indicates that the solidification point of the Al-19Si hypereutectic aluminum-silicon alloy at a metal mold temperature of 380℃ is located at the lower boundary of the pseudo-eutectic zone. In summary, the temperature range of the pseudo-eutectic formation zone of the Al-19Si hypereutectic aluminum-silicon alloy is 440℃~380℃.
[0111] Fig.18 The pseudo-eutectic formation region of aluminum-silicon alloy determined by melt purification and temperature-controlled solidification is drawn based on the conclusions obtained from Examples 2 to 8. Fig.18 As shown, the red line is the upper boundary line of the pseudo-eutectic formation area of the aluminum-silicon alloy, and the corresponding specific composition and temperature are represented by red dots; the blue line is the lower boundary line of the pseudo-eutectic formation area of the aluminum-silicon alloy, and the corresponding specific composition and temperature are represented by blue dots.
[0112] Comparative Example 1
[0113] The difference from Example 1 is that the Al-17Si hypereutectic alloy is melted at 850° C. and no halide purifier is used.
[0114] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Figure 1 shown.
[0115] Figure 1 This is the solidification structure diagram of Al-17Si hypereutectic aluminum-silicon alloy at different metal mold temperatures without purification treatment. Figure 1 The metal mold temperatures of (a) and (b) are 500℃ and 450℃, respectively. Obvious feather-like primary silicon and the presence of a partial aluminum matrix were observed under a metallographic microscope. Figure 1 (c) The mold temperature is 400℃, and obvious blocky primary silicon is observed. Figure 1The metal mold temperatures of (d) and (e) are 350℃ and 300℃, respectively. Obvious primary aluminum and partial primary silicon were observed through a metallographic microscope. In summary, the solidification structure of Al-17Si hypereutectic aluminum-silicon alloy at metal mold temperatures of 500℃, 450℃, 400℃, 350℃, and 300℃ did not obtain pseudo-eutectic structure, which indicates that the pseudo-eutectic structure cannot be obtained by using the temperature-controlled solidification process alone, and other treatment processes are required.
[0116] Comparative Example 2
[0117] The difference from Example 1 is that the Al-17Si hypereutectic alloy is melted at 850°C and a halide purifier with a composition ratio of 50% MgCl2+50% BaCl2 is used for melt purification.
[0118] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Figure 2 shown.
[0119] Figure 2 In the solidification microstructure diagram of Al-17Si hypereutectic alloy cast at a mold temperature of 450℃, many blocky primary silicon precipitations were observed, with an average diameter of 10.43μm and an area fraction of 12.30%, indicating that the purification effect of the halide salt purifier with a composition ratio of 50% MgCl2+50% BaCl2 on Al-17Si hypereutectic alloy is very unsatisfactory. When high-content MgCl2 and BaCl2 are used in synergy, they will decompose to generate magnesium and barium elements during the purification process. These elements act as crystal nuclei in the melt, which helps the precipitation of the primary silicon phase and reduces the formation of pseudo-eutectic structure.
[0120] Comparative Example 3
[0121] The difference from Example 1 is that the Al-17Si hypereutectic alloy is melted at 850°C and the melt is purified using a halide purifier with a composition ratio of 40% NaCl+40% KCl+10% Na3AlF6+10% BaCl2.
[0122] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Figure 3 shown.
[0123] Figure 3The solidification microstructure of Al-17Si hypereutectic alloy using 40% NaCl + 40% KCl + 10% Na3AlF6 + 10% BaCl2 halide purifier and cast at a metal mold temperature of 450°C, a small amount of blocky primary silicon precipitation was observed, the average diameter of primary silicon was 17.50μm, and the area fraction was 3.11%, which inhibited the precipitation of some primary silicon, but the effect was not ideal. When high content of MgCl2 and BaCl2 are used in combination, the nucleation of primary silicon is promoted, and a small amount of BaCl2 needs to be used to avoid excessive nucleation.
[0124] Comparative Example 4
[0125] The difference from Example 1 is that the Al-17Si hypereutectic alloy is melted at 850° C. and a halide purifier with a composition ratio of 50% NaCl+50% MgCl2 is used for melt purification.
[0126] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Figure 4 shown.
[0127] Figure 4 In the solidification microstructure diagram of Al-17Si hypereutectic alloy cast at a mold temperature of 450°C using a halide salt purifier with a composition ratio of 50% NaCl + 50% MgCl2, many blocky primary silicon precipitations were observed, with an average diameter of 18.69 μm and an area fraction of 10.53%, indicating that the purification effect of the halide salt purifier with a composition ratio of 50% NaCl + 50% MgCl2 on Al-17Si hypereutectic alloy is very unsatisfactory. When a high content of MgCl2 is used, they will decompose to generate magnesium elements during the purification process, which will serve as crystal nuclei and help the precipitation of primary silicon phase.
[0128] Comparative Example 5
[0129] The difference from Example 1 is that the Al-17Si hypereutectic alloy is melted at 850°C and the melt is purified using a halide purifier with a composition ratio of 50% Na3AlF6+50% MgCl2.
[0130] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Figure 5 shown.
[0131] Figure 5In the solidification microstructure diagram of Al-17Si hypereutectic alloy cast at a mold temperature of 450°C using a halide salt purifier with a composition ratio of 50% Na3AlF6+50% MgCl2, many blocky primary silicon precipitations were observed, with an average diameter of 17.55 μm and an area fraction of 9.96%, indicating that the purification effect of the halide salt purifier with a composition ratio of 50% Na3AlF6+50% MgCl2 on Al-17Si hypereutectic alloy is very unsatisfactory. When a high content of MgCl2 is used, the precipitation of the primary silicon phase will be promoted during the purification process. Na3AlF6 improves the fluidity of the melt.
[0132] Comparative Example 6
[0133] The difference from Example 1 is that the Al-17Si hypereutectic alloy is melted at 850°C, and a halide purifier with a composition ratio of 50% Na3AlF6+50% NaCl is used for melt purification.
[0134] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Figure 6 shown.
[0135] Figure 6 The solidification microstructure of Al-17Si hypereutectic alloy cast at a mold temperature of 450°C using a halide salt purifier with a composition ratio of 50% Na3AlF6 + 50% NaCl was observed. Partial blocky primary silicon was precipitated, with an average diameter of 25.30 μm and an area fraction of 3.79%, indicating that the halide salt purifier with a composition ratio of 50% Na3AlF6 + 50% NaCl has a certain purification effect on Al-17Si hypereutectic alloy. When a high content of Na3AlF6 is used, the fluidity of the melt is greatly improved during the purification process. After NaCl decomposes in the melt, it releases chlorine to form bubbles that can absorb and take away hydrogen and other harmful gases in the melt, thereby playing a degassing role.
[0136] Comparative Example 7
[0137] The difference from Example 1 is that the Al-17Si hypereutectic alloy is melted at 850°C, and a halide purifier with a composition ratio of 100% Na3AlF6 is used for melt purification.
[0138] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Figure 7 shown.
[0139] Figure 7The solidification microstructure of Al-17Si hypereutectic alloy cast at 450℃ with 100% Na3AlF6 halide purifier was observed. A large amount of blocky primary silicon was precipitated, with an average diameter of 21.48μm and an area fraction of 9.86%, indicating that the purification effect of 100% Na3AlF6 halide purifier on Al-17Si hypereutectic alloy is very unsatisfactory. Na3AlF6 has strong chemical activity and can reduce the melting point of aluminum-silicon alloy, greatly improving the fluidity and casting performance of the melt.
[0140] Comparative Example 8
[0141] The difference from Example 1 is that the Al-17Si hypereutectic alloy is melted at 850° C. and a halide purifier with a composition ratio of 100% MgCl2 is used for melt purification.
[0142] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Figure 8 shown.
[0143] Figure 8 In the solidification microstructure diagram of Al-17Si hypereutectic alloy cast at a mold temperature of 450°C using a halide salt purifier with a composition ratio of 100% MgCl2, a large amount of blocky primary silicon was observed to precipitate, with an average diameter of 25.75 μm and an area fraction of 13.24%, indicating that the purification effect of the halide salt purifier with a composition ratio of 100% MgCl2 on the Al-17Si hypereutectic alloy is very unsatisfactory.
[0144] Comparative Example 9
[0145] The difference from Example 1 is that the Al-17Si hypereutectic alloy is melted at 850° C., and a halide purifier with a composition ratio of 100% NaCl is used for melt purification.
[0146] After the heat preservation is finished, the sample is cut 10mm from the bottom of the solidified sample of the alloy test rod and observed using a metallographic microscope. The metallographic structure photo is as follows Fig. 9 shown.
[0147] Fig. 9 In the solidification microstructure diagram of Al-17Si hypereutectic alloy cast at a mold temperature of 450°C using a halide salt purifier with a composition ratio of 100% NaCl, a large amount of blocky primary silicon was observed to precipitate, with an average diameter of 28.68 μm and an area fraction of 13.85%, indicating that the purification effect of the halide salt purifier with a composition ratio of 100% NaCl on the Al-17Si hypereutectic alloy is very unsatisfactory.
[0148] Table 1 Quantitative analysis results of primary Si in the solidified structure of Al-17Si alloy after melt purification using halide purifiers with different composition ratios and temperature-controlled solidification at 450℃
[0149]
Claims
1. A method for determining the pseudo-eutectic formation region of aluminum-silicon alloy by melt purification and temperature-controlled solidification, characterized in that: include, Prepare halide salt purifier; prepare hypereutectic aluminum-silicon alloys with different silicon contents; The hypereutectic aluminum-silicon alloy is immersed in a molten halide purifier for smelting and then kept warm to completely dissolve the primary silicon; Keep the metal mold warm and quickly pour the alloy melt into the metal mold to form it; Based on the solidification structure analysis, the critical temperature of the pseudo-eutectic zone formed in aluminum-silicon alloys with different silicon contents is found, and the pseudo-eutectic formation area of the aluminum-silicon alloy system is determined.
2. The method according to claim 1, characterized in that: The halide salt purifier consists of Na3AlF6, NaCl and MgCl2.
3. The method according to claim 2, characterized in that: The halide salt purifier, calculated by raw material mass percentage, has a Na3AlF6 content of 25%, a NaCl content of 55%, and a MgCl2 content of 20%.
4. The method according to claim 1, characterized in that: The smelting temperature is 850° C. and the holding time is 35 minutes.
5. The method according to claim 1, characterized in that: The metal mold is kept warm, wherein the inner cavity size of the metal mold is φ5×100, the temperature is 530° C. to 380° C., and the keeping time is 3 minutes.
6. The method according to claim 1, characterized in that: The hypereutectic aluminum-silicon alloys with different silicon contents include Al-13%Si, Al-14%Si, Al-15Si, Al-16%Si, Al-17%Si, Al-18%Si, and Al-19%Si hypereutectic aluminum-silicon alloys.
7. The method according to claim 1, characterized in that: The temperature gradient of the metal mold insulation temperature is first set to 30° C., and then the approximate temperature range of the pseudo-eutectic zone is obtained based on the solidification structure analysis, and the temperature gradient is further changed to accurately determine the Al-Si alloy pseudo-eutectic formation area.