Cast aluminum alloy and preparation method thereof
By introducing the Al-Ca system and controlling the eutectic structure into the aluminum-manganese aluminum alloy, optimizing the element content and grain structure, the problems of easy cracking and poor feeding performance of aluminum alloys are solved, and high strength, low thermal cracking and High temperature stability, good casting performance and high temperature thermal processing performance.
Patent Information
- Application Number
- CN202411129599.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-10-11
AI Technical Summary
Aluminum-manganese aluminum alloys are prone to cracking, poor feeding performance, and low mechanical properties during the metal film casting process. The addition of existing strengthening elements will lower the melting point and worsen high-temperature processing performance, making it difficult to combine casting performance, mechanical properties, and high-temperature thermal processing. performance.
Cast aluminum alloy is used, containing Mn, Fe, Ca, Cr, Zr, Ti, Si and other elements to form an α-Al matrix and eutectic structure. The Al-Ca system is introduced to delay solidification and control the eutectic structure ratio and element content. Refinement agents and high-temperature treatments optimize the grain structure and reduce the risk of void defects and thermal cracking.
It significantly improves the strength, shrinkage and high-temperature stability of aluminum alloys, reduces the risk of hot cracking, maintains a high melting point, and achieves good mechanical properties and high-temperature thermal processing properties.
Smart Images

Figure CN118756005A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum alloys, and in particular to a casting aluminum alloy and a preparation method thereof. Background Art
[0002] Aluminum-manganese aluminum alloys have the characteristics of high corrosion resistance and high melting point, and have great potential in brazing, anodizing and other fields. However, during the metal film casting process, aluminum-manganese aluminum alloy castings are prone to cracking, have poor shrinkage compensation performance, and low mechanical properties, which restricts their application to a certain extent.
[0003] In order to balance the casting process performance, mechanical properties, high-temperature hot processing performance, etc. of Al-Mn aluminum alloys, adding strengthening elements is currently the main technical means. In view of the problems of low strength and easy cracking of this series of alloys, adding traditional strengthening elements such as Cu, Mg, Si, Zn, etc. will aggravate the cracking characteristics of the alloy, reduce the melting point of the casting alloy, and deteriorate the high-temperature processing performance of the casting. Therefore, these strengthening elements are often controlled in a small addition amount, and improving the strength of the alloy has become a greater difficulty.
[0004] In order to improve the casting performance of aluminum-manganese aluminum alloys, improve the quality of castings, and enhance the mechanical properties of castings, certain research work has been carried out in the industry. For example, the invention patent application CN113897519A discloses an aluminum-manganese-magnesium-silicon-titanium-tin casting alloy for brazing by vacuum die casting and a preparation method thereof. On the basis of the aluminum-manganese eutectic composition, magnesium and silicon are added, which improves the strength and toughness of the alloy without reducing the thermal conductivity of the alloy. Titanium and tin are added to refine the grains and improve the strength and toughness of the alloy. However, the addition of magnesium and silicon will significantly increase the solidification range and aggravate the tendency of hot cracking.
[0005] Invention patent CN112853178B discloses an aluminum-manganese-zinc-magnesium-iron-titanium-zirconium alloy, which adds zinc, magnesium, manganese and iron elements to the aluminum alloy, which not only improves the solid solution strengthening effect of the alloy, but also transforms the Mn-containing phase into a fine dispersed second phase, reduces the color difference between the matrix and the second phase, effectively improves the anodic oxidation performance of the alloy, and improves the mechanical properties. However, the addition of zinc and magnesium elements to the alloy will greatly expand the solidification range, making it difficult to ensure casting formability and prone to hot cracking.
[0006] Therefore, it is of great significance to develop an aluminum alloy material that has both casting properties, mechanical properties and good high-temperature hot working properties. Summary of the invention
[0007] The purpose of the present invention is to provide a cast aluminum alloy to address the deficiencies in the prior art, so as to solve the technical problems existing in the prior art such as easy thermal cracking, difficulty in shrinkage compensation, insufficient strength and poor machining performance of the aluminum alloy.
[0008] To achieve the above-mentioned purpose, the present invention proposes the following technical solution: a cast aluminum alloy, comprising the following components by mass percentage:
[0009] Mn: 1.0-2.0%; Fe: 0.1-0.5%; Ca: 1.0-5.5%; Cr: 0.01-0.5%; Zr: 0.01-0.3%; Ti: 0.01-0.3%; Si: not more than 0.2%; Mg: not more than 0.2%; the rest is Al;
[0010] The cast aluminum alloy includes an α-Al matrix and a eutectic structure, the eutectic structure includes a first eutectic and a second eutectic, the first eutectic includes (α-Al+Al6(Fe,Mn,Cr)Si) eutectic and / or (α-Al+Al6(Fe,Mn,Cr) eutectic, the second eutectic includes (α-Al+Al4Ca) eutectic, and the mass fraction of the (α-Al+Al4Ca) eutectic in the aluminum alloy is 6.7 to 60%.
[0011] In one or more embodiments of the present invention, during the formation of the eutectic structure, the second eutectic reaction occurs after the first eutectic reaction to compensate for the solidification shrinkage.
[0012] In one or more embodiments of the present invention, in the (α-Al+Al4Ca) eutectic, the α-Al phase and the Al4Ca phase are distributed alternately, and the Al4Ca phase has a fine lamellar structure, which is transformed into a spherical or short rod shape after high-temperature treatment.
[0013] In one or more embodiments of the present invention, in the (α-Al+Al4Ca) eutectic, the size of the Al4Ca phase is 1-5 um.
[0014] In one or more embodiments of the present invention, the mass fraction of the (α-Al+Al4Ca) eutectic in the aluminum alloy is 20-50%.
[0015] In one or more embodiments of the present invention, the mass percentage of Fe+Mn in the aluminum alloy is 1.2-2.3%.
[0016] In one or more embodiments of the present invention, the morphology of the first eutectic structure is large-sized α-Al dendrites and Al6(Fe, Mn, Cr)Si phase and / or Al6(Fe, Mn, Cr) phase particles formed between the dendrites.
[0017] In one or more embodiments of the present invention, in the first eutectic structure, the size of the Al6(Fe, Mn, Cr)Si phase and / or the Al6(Fe, Mn, Cr) phase is 1-25 um.
[0018] In one or more embodiments of the present invention, the cast aluminum alloy is a polyeutectic system, which introduces an Al-Ca system on the basis of the Al-Mn eutectic system to delay dendrite bridging during the alloy solidification process.
[0019] The present invention also provides a method for preparing a cast aluminum alloy, comprising the following preparation steps:
[0020] S1. Weigh each component according to the formula amount, melt them in stages, and obtain a melt;
[0021] S2, adding a refiner to the melt, waiting for it to be completely melted and stirring it evenly, and obtaining a metal melt after refining;
[0022] S3, pouring, and cooling at a cooling rate greater than or equal to 2°C / s to obtain the cast aluminum alloy.
[0023] In one or more embodiments of the present invention, the S1 includes:
[0024] Weigh each component according to the formula, keep the temperature at 750-800°C to melt the aluminum ingot, add aluminum-manganese master alloy or manganese agent, aluminum-iron master alloy or iron agent to the melt, and melt them completely;
[0025] The melt is cooled to 750-780°C, and titanium, chromium, zirconium and other elements are added in sequence and completely melted;
[0026] At 740-770°C, the aluminum-calcium master alloy is pressed into the melt using a bell jar until it is completely absorbed.
[0027] In one or more embodiments of the present invention, the refiner in S2 is selected from one or more of Al-Ti-B, Al-Ti-C, Al-Ti-CB, Al-Zr-B or Al-Nb-B.
[0028] In the cast aluminum alloy proposed by the present invention, by controlling Mn within the hypoeutectic range, the formation of coarse primary Al6Mn-type phases can be avoided and a fine Al6Mn-type eutectic structure can be obtained; in addition, the addition of Mn can also improve the demolding effect during the alloy casting process.
[0029] Furthermore, the Fe element can effectively refine the size of Al6Mn-like phases and regulate the morphology of Al6Mn-like phases; on the other hand, since the alloy has a high Fe content, the alloy can be repeatedly recycled and reused, and its preparation process has the advantage of low carbon emissions.
[0030] Furthermore, Ca is a rare metal that expands in volume during solidification, and its volume expansion rate can reach 3.2%. The Al4Ca phase formed by the Ca element during solidification has a low density and a high molar volume. The present invention can effectively control the volume shrinkage of the alloy during solidification by controlling the amount of Ca added, thereby fundamentally reducing the generation of pore defects. In the present invention, the Ca content is selected to be controlled in the range of 1.0 to 5.5%. On the one hand, sufficient Ca content can effectively reduce shrinkage defects and effectively improve strength.
[0031] Furthermore, since the (α-Al+Al4Ca) eutectic reaction occurs after the Al-Mn eutectic reaction, i.e., the first eutectic reaction, the solidification shrinkage can be effectively fed, and by controlling the mass percentage of the (Al+Al4Ca) eutectic structure to 6.7-60%, or by controlling the area percentage of the (α-Al+Al4Ca) eutectic structure to not exceed 70% on the microstructure diagram, when the first eutectic ends, the α-Al dendrites are in an unbridged (or feeding channel is not closed) state, thereby further improving the feeding property of the alloy.
[0032] Furthermore, control is performed to ensure that there is an appropriate amount of α-Al in the alloy to coordinate deformation and achieve the unity of strength and toughness.
[0033] Furthermore, the Al4Ca phase in the cast state is in the form of fine lamellar sheets, or fine short rods, or fine spheres, so that the (α-Al+Al4Ca) eutectic has a strong eutectic strengthening effect, thereby obtaining better mechanical properties.
[0034] Furthermore, the Cr element is added to the composition of the cast aluminum alloy of the present invention to achieve further regulation of the Mn and Fe phases.
[0035] Furthermore, the addition of Zr and Ti elements can refine the alloy grains, delay dendrite bridging during solidification, improve the shrinkage feeding effect, and reduce the risk of thermal cracking. The addition of Zr elements can also precipitate Al3M dispersed phase inside the α-Al grains, further improving the strength of the α-Al grains.
[0036] Furthermore, in the present invention, since the addition of Si element does not exceed 0.2%, the first eutectic formed includes (α-Al+Al6(Fe,Mn,Cr)Si) eutectic and / or (α-Al+Al6(Fe,Mn,Cr) eutectic, depending on the amount of Si added. That is, when the addition amount of Si element is within a certain range, the first eutectic mainly forms (α-Al+Al6(Fe,Mn,Cr)Si) eutectic, and when the addition amount of Si element is low or no Si element is added, the first eutectic mainly forms (α-Al+Al6(Fe,Mn,Cr) eutectic.
[0037] Furthermore, the content of impurities in the cast aluminum alloy of the present invention is less than 0.1% by mass percentage.
[0038] Due to the low shrinkage rate during the (Al+Al4Ca) eutectic reaction, the shrinkage stress of the alloy in the two-phase region and the high-temperature solid phase temperature range is greatly reduced, greatly reducing the risk of hot cracking of castings.
[0039] Since the second phase of the (Al+Al4Ca) eutectic structure is small and dispersed, it has a higher eutectic strengthening effect and effectively improves the strength of the alloy.
[0040] Since the (Al+Al4Ca) eutectic structure has a high solidus temperature, the alloy has excellent high temperature stability and high temperature brazing performance.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] The Al-Mn-Ca casting alloy and preparation method proposed in the present invention introduce a second eutectic (α-Al+Al4Ca) on the basis of the Al-Mn alloy binary system. The second eutectic (α-Al+Al4Ca) has a low density and a high molar volume, so that the volume shrinkage of the alloy during solidification is greatly reduced, fundamentally reducing the occurrence of pore defects inside the casting; at the same time, after adding a certain amount of Ca, the eutectic content is increased, the thermal cracking tendency is reduced, and a certain shrinkage feeding space is provided.
[0043] The Al-Mn-Ca alloy system is adopted. While containing a large amount of high-temperature stable phases, the addition amount of low-melting-point elements is strictly controlled to ensure the high melting point of the aluminum alloy; and the large amount of (α-Al+Al4Ca) eutectic structure introduced effectively improves the mechanical properties of the alloy; and with the help of the addition of dispersed phase forming elements Zr, Ti, and Cr, the α-Al grains and Al-Mn intermetallic compounds are further refined, and co-grow with the eutectic Al4Ca phase, further improving the thermal stability of the Al4Ca phase.
[0044] The cast aluminum alloy of the present invention has a tensile strength of more than 180 MPa, a yield strength of more than 100 MPa and an elongation of more than 6% at room temperature in a cast state.
[0045] After the cast aluminum alloy is heat-insulated at 600° C., the tensile strength is above 150 MPa, the yield strength is above 80 MPa, and the elongation is greater than or equal to 10% at room temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1a , Figure 1b They are respectively microstructure diagrams of the cast aluminum alloy in the as-cast state and the heat-treated state prepared in Example 1 of the present invention;
[0047] Figure 2a , Figure 2b They are respectively microstructure diagrams of the cast aluminum alloy in the as-cast state and the heat-treated state prepared in Example 2 of the present invention;
[0048] Figure 3a-3d They are respectively microstructure diagrams of the cast aluminum alloy prepared in Example 3 of the present invention in the as-cast state and the heat-treated state at different magnifications;
[0049] Figure 3e , Figure 3f They are respectively SEM images of the heat-treated cast aluminum alloy prepared in Example 3 of the present invention;
[0050] Figure 4 is a microstructure diagram of the cast aluminum alloy prepared in comparative example 1 of the present invention;
[0051] Figure 5 is a microstructure diagram of the cast aluminum alloy prepared in comparative example 2 of the present invention;
[0052] Figure 6 This is a microstructure diagram of the cast aluminum alloy prepared in comparative example 3 of the present invention.
[0053] In the above figures, arrow 1 indicates the (α-Al+Al6(Fe,Mn,Cr)Si) eutectic, arrow 2 indicates the α-Al+Al4Ca eutectic, arrow 3 indicates the spherical Al6(Fe,Mn,Cr)Si phase, arrow 4 indicates the Al4Ca phase, and arrow 5 indicates the coarse lath-like Al6(Fe,Mn,Cr)Si phase. DETAILED DESCRIPTION
[0054] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific implementation modes.
[0055] Unless explicitly stated otherwise, throughout the specification and claims, the term "comprise" or variations such as "include" or "comprising" etc. will be understood to include the stated elements or components but not to exclude other elements or components.
[0056] The present invention will be described in detail below in conjunction with the specific embodiments shown in the accompanying drawings. However, these embodiments do not limit the present invention, and any structural, methodological, or functional changes made by a person skilled in the art based on these embodiments are all within the scope of protection of the present invention.
[0057] Example 1
[0058] The aluminum alloy casting and its preparation method provided in this embodiment, the casting includes the following contents in mass percentage: Mn: 1.5%; Fe: 0.2%; Ca: 1.7%; Ti: 0.096%; Zr: 0.06%; Cr: 0.08%; Mg: 0.04%; Si: 0.06%, and the rest is Al and unavoidable impurities.
[0059] The preparation method comprises the following preparation steps:
[0060] (1) weighing industrial pure Al ingot, Al-Mn master alloy and Fe agent according to the designed amount, placing them in a melting furnace, heating them to 790±10°C, cooling the melting furnace to 760±10°C after the raw materials in the melting furnace are melted, and then adding other master alloys: Al-Ti master alloy, Al-Zr master alloy and Al-Cr master alloy into the melting furnace respectively to completely melt, cooling to 750±10°C, and pressing the Al-Ca master alloy below the liquid surface with a bell jar to completely melt to obtain a melt;
[0061] (2) The melt is kept at 750±10°C, and a refiner (Shenzhen Xinxing Al-Ti5-B refiner) accounting for 5.0‰ of the melt mass is added into the smelting furnace, the gas medium is argon gas of more than 99.99%, and the rotary rotor is used for stirring and degassing for 20 minutes. After standing for 20 minutes, the slag is removed to obtain the refined metal melt;
[0062] (3) When the temperature of the molten metal is 740±10°C, the molten metal is poured into a steel mold preheated at 175±10°C to obtain a casting; wherein the cooling rate of the casting is controlled to be 4±1°C / s during the casting process.
[0063] The microstructures of the cast and heat-treated states prepared by the above method are as follows: Figure 1a , Figure 1b As shown, the heat treatment state in each embodiment of the present invention and the accompanying drawings is the brazing state, and the brazing condition is 605° C. welding for 15 minutes. In other embodiments of the present invention, the heat treatment state can be under other heat treatment conditions.
[0064] The microstructure of this embodiment in the cast state and heat treatment state Figure 1a , Figure 1b It was observed that the alloy matrix of this embodiment contained primary α-Al grains, (Al+Al4Ca) eutectic structure and a small amount of blocky primary Al6(Fe,Mn,Cr)Si phase. According to the microstructure diagram, the area fraction of (α-Al+Al4Ca) eutectic in the aluminum alloy in this embodiment was 13%.
[0065] The tensile properties of the alloy were tested and the results showed that the strength of the alloy with this composition was significantly increased compared with the control example, and the elongation was maintained at about 10%.
[0066] Example 2
[0067] The components of the cast aluminum alloy in this embodiment and their mass percentages are: Mn: 2.0%; Fe: 0.3%; Ca: 1.0%; Ti: 0.08%; Zr: 0.1%; Cr: 0.12%; Mg: 0.03%; Si: 0.12%, and the rest is Al and unavoidable impurities.
[0068] The preparation method of this embodiment is basically the same as that of embodiment 1, except that in step (1), industrial pure Al ingot, Al-Mn master alloy and Fe agent are weighed according to the designed amount, placed in a melting furnace, heated to 790±10° C., after the raw materials in the melting furnace are melted, the melt is cooled to 750±10° C., then Al-Ti master alloy, Al-Zr master alloy and Al-Cr master alloy are respectively added to the melting furnace and completely melted, and finally Al-Ca master alloy is pressed below the liquid surface with a bell jar to completely melt to obtain a melt;
[0069] The microstructures of the as-cast and heat-treated states prepared by the above method are as follows: Figure 2a , Figure 2b As shown. Through organizational observation, it is found that the alloy matrix of this embodiment contains primary α-Al grains, (Al+Al4Ca) eutectic structure and a large number of worm-like eutectic Al6(Fe,Mn,Cr)Si phases. According to the detection of the microstructure diagram, in this embodiment, the area fraction of (α-Al+Al4Ca) eutectic in the aluminum alloy accounts for 7.5%.
[0070] The tensile properties of the alloy were tested and the results showed that the strength of the alloy with this composition was significantly increased compared with the control example, and the elongation was maintained at about 7%.
[0071] Example 3
[0072] The cast aluminum alloy components and their mass percentages of this embodiment are: Mn: 1.2%; Fe: 0.45%; Ca: 4.5%; Ti: 0.12%; Zr: 0.05%; Cr: 0.15%; Mg: 0.15%; Si: 0.03%, and the rest is Al and unavoidable impurities. The preparation method of this embodiment is basically the same as the preparation method of embodiment 1.
[0073] The microstructures of the cast and heat-treated states prepared by the above method at different magnifications are shown in Figure 2. Figure 3a-3dAs shown. Through organizational observation, it is found that the alloy microstructure of this embodiment contains a large number of fine spherical α-Al grains, (Al+Al4Ca) eutectic structure and a small amount of blocky Al6(Fe,Mn,Cr)Si phase. Figure 3e , 3f As shown in the figure, after being kept at 600℃ for 30min, there is no overburning inside the alloy, and the eutectic Al4Ca phase is obviously rounded. It can be seen from SEM that after high temperature treatment, granular Al6(Fe,Mn,Cr)Si phase with a particle size of only about 1um is associated with the Al4Ca phase, which effectively improves the high temperature stability of the alloy.
[0074] According to the detection of the microstructure diagram, in this embodiment, the area fraction of the (α-Al+Al4Ca) eutectic in the aluminum alloy is 48%.
[0075] The tensile properties of the alloy were tested and the results showed that the strength of the alloy with this composition was significantly increased compared with the control example, and the elongation was maintained above 10%.
[0076] Comparative Example 1
[0077] The components of the cast aluminum alloy of this comparative example and their mass percentages are: Mn: 1.4%; Fe: 0.12%, Ca: 0.05%; Ti: 0.05%; Zr: 0.05%; Cr: 0.08%; Mg: 0.07%; Si: 0.02%; the rest are Al and unavoidable impurities.
[0078] The preparation method of this comparative example is basically the same as that of Example 1, except that: Step (1) is: weighing industrial pure Al ingots and Al-Mn master alloys according to the designed amount, placing them in a melting furnace, heating them to 780±10° C., cooling the melting furnace to 750±10° C. after the raw materials in the melting furnace are melted, and then adding Al-Ti master alloys, Al-Zr master alloys, and Al-Cr master alloys into the melting furnace respectively and completely melting them to obtain a melt;
[0079] The as-cast microstructure prepared by the above method is as follows Figure 4 As shown, it is found through observation that a narrow (Al+AlFeMn phase) eutectic zone is distributed at the α-Al grain boundary of the alloy of this embodiment, that is, the eutectic structure content is low, which is not conducive to the shrinkage compensation of the alloy. By comparing the results of the alloy performance test table, it can be seen that the strength of the alloy is low.
[0080] Comparative Example 2
[0081] The components of the cast aluminum alloy in this comparative example and their mass percentages are: Mn: 1.9%; Fe: 0.25%; Ca: 0.12%; Ti: 0.03%; Zr: 0.02%; Cr: 0.03%; Mg: 0.05%; Si: 0.04%; the rest are Al and unavoidable impurities.
[0082] The preparation method of this comparative example is basically the same as that of Example 1, except that: Step (1) is: weighing industrial pure Al ingots and Al-Mn master alloys according to the designed amount, placing them in a melting furnace, heating them to 790±10° C., cooling the melting furnace to 750±10° C. after the raw materials in the melting furnace are melted, and then adding Al-Ti master alloys, Al-Zr master alloys, and Al-Cr master alloys into the melting furnace respectively and completely melting them to obtain a melt;
[0083] Steps (2) and (3) are the same as in Example 1;
[0084] The as-cast microstructure prepared by the above method is as follows Figure 5 Through the observation of the structure, it is found that the α-Al grain boundary of the alloy of this embodiment is distributed with a narrow (Al+AlFeMn phase) eutectic region, that is, the eutectic structure content is low, which is not conducive to the shrinkage compensation of the alloy. By comparing the results of the alloy performance test table, it can be seen that the strength of the alloy under this composition is low.
[0085] Comparative Example 3
[0086] The components of the cast aluminum alloy in this comparative example and their mass percentages are: Mn: 2.3%; Fe: 0.6%; Ca: 2.3%; Ti: 0.04%; Zr: 0.15%; Cr: 0.2%; Mg: 0.25%; Si: 0.22%; the rest are Al and unavoidable impurities.
[0087] The preparation method is different from that of Example 1 in that: Step (1): weigh industrial pure Al ingot, Al-Mn master alloy and Fe agent according to the designed amount, place them in a melting furnace, heat them to 790±10°C, and after the raw materials in the melting furnace are melted, cool the melting furnace to 750±10°C, then add Al-Ti master alloy, Al-Zr master alloy and Al-Cr master alloy into the melting furnace respectively and melt them completely, and finally press the Al-Ca master alloy below the liquid surface with a bell jar to melt it completely to obtain a melt.
[0088] The as-cast microstructure prepared by the above method is as follows Figure 6 Through the observation of the structure, it is found that there are a large number of lath-shaped primary Al6(Fe, Mn, Cr)Si phases with a size of more than 50 μm in the alloy matrix of this embodiment.
[0089] It can be seen from the results of the comparative alloy performance test table in Table 2 that the elongation of the alloy under this composition is significantly lower than that of the alloys in Examples 1 to 3. In addition, due to the high content of Mg and Si elements in Comparative Example 3, the melting point of the alloy is only 582°C, which cannot withstand high-temperature treatment above 600°C.
[0090] In summary, the Al-Mn-Ca casting alloy provided by the present invention has good casting performance, small hot cracking tendency, high melting point, good mechanical properties and high temperature hot working performance.
[0091] Table 1 Composition of each embodiment and comparative example
[0092] Mn Ca Fe Ti Zr Cr Mg Si Example 1 1.5 1.7 0.2 0.1 0.06 0.08 0.04 0.06 Example 2 2.0 1.0 0.3 0.08 0.1 0.12 0.03 0.12 Example 3 1.2 4.5 0.45 0.12 0.05 0.15 0.15 0.03 Comparative Example 1 1.4 0.05 0.12 0.05 0.05 0.08 0.07 0.02 Comparative Example 1 1.9 0.12 0.25 0.03 0.02 0.03 0.05 0.04 Comparative Example 3 2.3 2.3 0.6 0.04 0.15 0.2 0.25 0.22
[0093] Table 2 Performance test results
[0094]
[0095] The description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A cast aluminum alloy, characterized in that: The following ingredients are included in percentage by mass: Mn: 1.0-2.0%; Fe: 0.1~0.5%; Ca: 1.0~5.5%; Cr: 0.01~0.5%; Zr: 0.01~0.3%; Ti: 0.01~0.3%; Si: not more than 0.2%; Mg: not more than 0.2%; the rest is Al; The cast aluminum alloy includes an α-Al matrix and a eutectic structure, the eutectic structure includes a first eutectic and a second eutectic, the first eutectic includes (α-Al+Al6(Fe,Mn,Cr)Si) eutectic and / or (α-Al+Al6(Fe,Mn,Cr) eutectic, the second eutectic includes (α-Al+Al4Ca) eutectic, and the mass fraction of the (α-Al+Al4Ca) eutectic in the aluminum alloy is 6.7 to 60%.
2. The cast aluminum alloy according to claim 1, characterized in that During the formation of the eutectic structure, the second eutectic reaction occurs after the first eutectic reaction to compensate for the solidification shrinkage.
3. The cast aluminum alloy according to claim 1, characterized in that: In the (α-Al+Al4Ca) eutectic, the α-Al phase and the Al4Ca phase are distributed alternately, and the Al4Ca phase has a fine lamellar structure, which is transformed into a spherical or short rod shape after high-temperature treatment.
4. The cast aluminum alloy according to claim 1 or 3, characterized in that: In the (α-Al+Al4Ca) eutectic, the size of the Al4Ca phase is 1-5um.
5. The cast aluminum alloy according to claim 1, characterized in that: The mass fraction of the (α-Al+Al4Ca) eutectic in the aluminum alloy is 20-50%.
6. The cast aluminum alloy according to claim 1, characterized in that: The mass percentage of Fe+Mn in the aluminum alloy is 1.2-2.3%.
7. The cast aluminum alloy according to claim 1, characterized in that: The morphology of the first eutectic structure is large-sized α-Al dendrites and Al6(Fe, Mn, Cr)Si phase and / or Al6(Fe, Mn, Cr) phase particles formed between the dendrites.
8. The cast aluminum alloy according to claim 1 or 7, characterized in that: In the first eutectic structure, the size of the Al6(Fe, Mn, Cr)Si phase and / or the Al6(Fe, Mn, Cr) phase is 1-25 um.
9. The cast aluminum alloy according to claim 1, characterized in that: The cast aluminum alloy is a multi-eutectic system, which introduces an Al-Ca system on the basis of an Al-Mn eutectic system to delay dendrite bridging during the alloy solidification process.
10. A method for preparing a cast aluminum alloy according to any one of claims 1 to 9, characterized in that: The method comprises the following preparation steps: S1. Weigh each component according to the formula amount, melt them in stages, and obtain a melt; S2, adding a refiner to the melt, waiting for it to be completely melted and stirring it evenly, and obtaining a metal melt after refining; S3, pouring, and cooling at a cooling rate greater than or equal to 2°C / s to obtain the cast aluminum alloy.
11. The method for preparing a cast aluminum alloy according to claim 10, characterized in that: The S1 includes: Weigh each component according to the formula, keep the temperature at 750-800°C to melt the aluminum ingot, add aluminum-manganese master alloy or manganese agent, aluminum-iron master alloy or iron agent to the melt, and melt them completely; The melt is cooled to 750-780°C, and titanium, chromium, zirconium and other elements are added in sequence and completely melted; At 740-770°C, the aluminum-calcium master alloy is pressed into the melt below the liquid surface until it is completely absorbed.
Citation Information
Patent Citations
An anodized die-cast aluminum alloy and its preparation method
CN112853178B
Al-Mn-Mg-Si-Ti-Sn casting alloy for realizing vacuum brazing through vacuum die casting and preparation method of Al-Mn-Mg-Si-Ti-Sn casting alloy
CN113897519A
Cited By
Cast aluminum alloy material as well as preparation method and application thereof
CN120575074A