Novel inlaid composite target material and preparation method thereof
By opening threaded through holes in the base material of the inlaid composite target and optimizing the freezing embedding process of the inlaid material, the problems of material skew and gaps during the inlay process are solved, and the bonding strength and preparation simplicity of the inlaid composite target are improved.
Patent Information
- Application Number
- CN202410754304.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-12
AI Technical Summary
Existing inlaid composite targets are easily skewed and stuck during the inlay process due to excessive material diameter, resulting in loose integration between the matrix material and the inlay material. When the number of inlay materials is increased, the risk of interface gaps increases, and the preparation process is complicated.
Design a new preparation method for inlaid composite targets. By opening circular through holes in the base material and processing threads, the inlaid material is embedded in the through holes after freezing, and the height and interference of the threads are optimized to ensure that the inlaid material goes down vertically and improves bonding. strength.
It achieves a tight combination between the inlaid material and the matrix material, reduces the risk of interface gaps, simplifies the preparation process and improves the bonding strength of the inlaid composite target material.
Smart Images

Figure BDA0004889003250000061 
Figure BDA0004889003250000071 
Figure HDA0004889003260000011
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of physical vapor deposition, and in particular to a novel inlaid composite target material and a preparation method thereof. Background Art
[0002] Physical Vapor Deposition (PVD) is a method of vaporizing the coating material by physical methods (such as evaporation, sputtering, etc.) to deposit a coating on the surface of the substrate material. PVD has the advantages of low deposition temperature, fast deposition speed, simple equipment structure, and no pollution. It has developed rapidly in recent years and is widely used in the automotive, medical, electronic, aerospace and other fields. By depositing different coatings, it gives the substrate material new functions and material properties, providing more excellent performance and solutions for various application scenarios.
[0003] The target material plays a vital role in the coating process. It not only provides the required materials, but its structure and quality also affect the sputtering process and the quality of the coating. High-quality target materials can ensure the uniformity, density and stability of the coating, and improve the performance and service life of the coating. Mosaic composite target refers to the combination of other materials inlaid on the base material. By flexibly adjusting the type, proportion and layout of the inlaid materials, a specific coating structure and performance can be deposited. It is an important type of target material.
[0004] Usually, inlaid composite targets are inlaid with other materials by interference fit. The diameter of the inlaid material is generally not more than 40mm. If the diameter is too large, the inlaid material will be skewed and stuck when it goes down. After being forced in with a press, a gap will appear between the inlaid material and the base material, resulting in a loose combination of the inlaid material and the base material, and the inlay fails. Due to the small diameter of the inlaid material, when preparing an inlaid composite target with a high proportion of inlaid material, the only way is to increase the amount of inlaid material, which makes the preparation process complicated. At the same time, due to the increase in the amount of inlaid material, the interface length between the inlaid material and the base material also increases, and the risk of gaps appearing at the interface during the use of the target also increases accordingly. Summary of the invention
[0005] In order to solve the above technical problems, the present application provides a new type of inlaid composite target material and a preparation method and application thereof.
[0006] The present application provides a method for preparing a novel inlaid composite target material, which is composed of a base material and an inlaid material, and specifically comprises the following steps in sequence: The base material is cylindrical in shape, the upper and lower end surfaces are leveled, a circular through hole is opened at the center, the upper end surface of the through hole is chamfered, the chamfer size is 0.5mm×45°~1.0mm×45°, and the inner wall of the through hole is perpendicular to the upper and lower end surfaces; The inner wall of the through hole of the base material is processed into a thread, the thread height is 0.1-0.3 mm, and the pitch is 0.2-0.5 mm; The inlay material is cylindrical, the outer diameter of the cylinder of the inlay material is 0.12-0.19% larger than the inner diameter of the circular through hole of the base material, and the height of the cylinder of the inlay material is the same as the thickness of the base material; The embedded material is placed in liquid nitrogen for freezing, taken out and embedded into the circular hole of the base material, and left for 5 to 10 minutes to obtain an embedded composite target blank; The novel inlaid composite target material is obtained through post-processing.
[0007] The present application utilizes the above technical solution, and the selected base material is provided with a through hole, so that when the inlay material moves downward, the gas can be discharged from the lower part of the base material. If there is no through hole, the gas will hinder the smooth downward movement of the inlay material; if the upper and lower end faces of the base material are not leveled, it is easy to cause the processed through hole to be misaligned, and there will be a gap between the inlay material and the base material after inlay; the upper end face of the through hole is provided with a chamfer, so that the inlay material can move downward vertically during inlay without being skewed or stuck; threads are processed on the inner wall of the through hole of the base material, which can greatly improve the bonding strength; if the interference is too small, the bonding strength between the inlay material and the base material is not high, and if the interference is too large, it will cause difficulty in inlaying, and the inlay material is easy to get stuck during the downward movement.
[0008] Preferably, in the base material, the thread height is 0.15-0.25 mm, and the thread pitch is 0.3-0.4 mm.
[0009] In some specific embodiments, in the matrix material, the thread height can be 0.1-0.15 mm, 0.1-0.2 mm, 0.1-0.25 mm, 0.1-0.3 mm, 0.15-0.2 mm, 0.15-0.3 mm, 0.2-0.25 mm, 0.2-0.3 mm, 0.25-0.3 mm, and the pitch can be 0.2-0.3 mm, 0.2-0.35 mm, 0.3-0.4 mm, 0.3-0.5 mm, 0.3-0.35 mm, 0.3-0.5 mm, 0.35-0.4 mm, 0.35-0.5 mm, 0.4-0.5 mm.
[0010] In a specific embodiment, in the matrix material, the thread height can be 0.1 mm, 0.15 mm, 0.2 mm, 0.25 mm, 0.3 mm, and the thread pitch can be 0.2 mm, 0.3 mm, 0.35 mm, 0.4 mm, 0.5 mm.
[0011] Through experimental analysis, it can be known that the application selects the above-mentioned specification and size of the thread, which can further improve the bonding strength of the embedded composite target material.
[0012] Preferably, the outer diameter of the cylinder of the inlay material is 0.14-0.17% larger than the inner diameter of the circular through hole of the base material.
[0013] In some specific embodiments, the cylindrical outer diameter of the inlay material is 0.12%, 0.14%, 0.15%, 0.16%, 0.17%, or 0.19% larger than the circular through-hole inner diameter of the base material.
[0014] In a specific embodiment, the cylindrical outer diameter of the inlay material is 0.12-0.14%, 0.12-0.15%, 0.12-0.16%, 0.12-0.17%, 0.12-0.19%, 0.14-0.15%, 0.14-0.16%, 0.14-0.19%, 0.15-0.16%, 0.15-0.17%, 0.15-0.19%, 0.16-0.17%, 0.16-0.19%, 0.17-0.19% larger than the inner diameter of the circular through hole of the base material.
[0015] Through experimental analysis, it can be known that the present application selects the interference within the above range to further improve the bonding strength of the embedded composite target material.
[0016] Preferably, the inlay material is any one of TiAl, CrAl and Al, and the atomic percentage content of Al in the inlay material is 50 to 100 at.%.
[0017] Preferably, the matrix material is any one of TiSi and Ti.
[0018] In the technical solution provided in the present application, the specific type of the matrix material has little effect on the inlaid composite target. The main thing is that the inlaid material needs to contain Al, and the atomic percentage of Al is: 50-100at.%. If the Al content is too low, the shrinkage after liquid nitrogen freezing is small, and it cannot be put into the hole after freezing, and it cannot be inlaid. The lower Al content will also make the bonding strength of the inlaid composite target lower.
[0019] Preferably, the dimensions of the base material are: diameter of 60-200 mm, thickness of 10-100 mm, and through-hole wall thickness of >15 mm.
[0020] In the technical solution provided in the present application, the size of the base material needs to be controlled within the above range. If the wall thickness is too thin, there is a risk of cracking of the base material after embedding.
[0021] Preferably, the diameter of the inlay material is 30-170 mm.
[0022] Preferably, the freezing time in liquid nitrogen is 20 to 30 minutes.
[0023] In the technical solution provided in the present application, the embedding material is placed in liquid nitrogen and frozen for 20 to 30 minutes, mainly to ensure that the embedding material is cooled thoroughly. If the freezing time is short, the embedding material may not shrink enough and cannot be embedded, or may get stuck halfway through the embedding.
[0024] Preferably, the post-processing comprises the following steps: The inlaid composite target blank is machined to remove the chamfered layer on the upper end surface, and then machined to the required size on the drawing by machining or grinding; The processed inlaid composite target material is placed in alcohol for ultrasonic cleaning for 5 to 10 minutes, and then placed in a vacuum oven and baked at 105-115°C for 10 to 20 minutes.
[0025] In a second aspect, the present application provides a novel inlaid composite target material, which is prepared using the above-mentioned method for preparing the novel inlaid composite target material.
[0026] In summary, the technical solution of this application has the following effects: The inlaid composite target material prepared in the present application has a tight bond with the matrix material and a high bonding strength; the preparation method provided in the present application can inlay large-sized inlaid materials. Compared with inlaying multiple small-sized inlaid materials, the interface length between the inlaid material of the present application and the matrix material is smaller, and the risk of gaps appearing at the interface during the use of the target material is lower; the process for preparing the inlaid composite target material in the present application is simple, which can save processing costs.
[0027] The present application can further improve the bonding strength of the embedded composite target material by optimizing the specification size of the thread in the base material and the interference between the embedded material and the base material. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a cross-sectional schematic diagram of the inlaid composite target material of the present application, wherein 1 is the base material, 2 is the inlaid material, and 3 is a detail view of the chamfer.
[0029] Figure 2 This is a top view of the inlaid composite target prepared in Example 1.
[0030] Figure 3 This is a top view of the embedded composite target prepared in Comparative Example 1. DETAILED DESCRIPTION
[0031] The present application is further described in detail below in conjunction with examples, comparative examples and performance testing experiments. These examples should not be construed as limiting the scope of protection claimed in the present application. Example
[0032] Example 1 Example 1 provides a new type of mosaic composite target material.
[0033] The preparation method of the novel inlaid composite target material in this embodiment specifically includes the following steps: In this embodiment, the matrix material is Ti / Si 80 / 20at%, the diameter is 160mm, the thickness is 50mm, and the through hole wall thickness is 25mm; the embedded material is Ti / Al 30 / 70at%.
[0034] (1) Level the upper and lower end surfaces of the base material, open a circular through hole at the center, the through hole diameter is 110 mm, the upper end surface of the through hole is chamfered, the chamfer size is 0.5 mm × 45°, and the inner wall of the through hole is perpendicular to the upper and lower end surfaces; (2) The inner wall of the through hole of the base material is processed into a thread with a thread height of 0.2 mm and a pitch of 0.3 mm; (3) Processing the inlay material into a cylindrical shape, the outer diameter of the cylinder is 0.15% larger than the inner diameter of the circular hole of the base material (interference), and the height of the cylinder is the same as the thickness of the base material; (4) placing the embedded material in liquid nitrogen and freezing it for 25 minutes, taking it out and embedding it into the circular hole of the base material, leaving it for 10 minutes, and obtaining an embedded composite target blank; (5) The inlaid composite target blank is machined to remove the chamfered layer on the upper end surface, and then further machined to the required size of the drawing by means of turning or grinding; (6) The processed inlaid composite target material was placed in alcohol for ultrasonic cleaning for 10 minutes, and then placed in a vacuum oven and baked at 110° C. for 15 minutes.
[0035] like Figure 1 As shown, it is a cross-sectional schematic diagram of the inlaid composite target material of the present application, wherein 1 is the base material, 2 is the inlaid material, and 3 is a detail diagram of the chamfer.
[0036] like Figure 2 The figure shows a top view of the inlaid composite target material prepared in Example 1; the inlaid material and the matrix material of the prepared inlaid composite target material are tightly bonded and have high bonding strength.
[0037] Embodiment 2-5 Examples 2-5 respectively provide a new type of inlaid composite target material.
[0038] The difference between the above embodiment and embodiment 1 is that the thread process parameters are different, as shown below.
[0039] In Example 2: the thread height is 0.1 mm and the thread pitch is 0.3 mm.
[0040] In Example 3: the thread height is 0.3 mm and the thread pitch is 0.3 mm.
[0041] In Example 4: thread height 0.2 mm, thread pitch 0.2 mm.
[0042] In Example 5: the thread height is 0.2 mm and the thread pitch is 0.5 mm.
[0043] The above embodiment is the same as that of Embodiment 1 in terms of the base material and the inlay material of the novel inlay composite target material and the remaining steps of the preparation method.
[0044] Embodiment 6-7 Examples 6-7 respectively provide a new type of inlaid composite target material.
[0045] The difference between the above embodiment and embodiment 1 is that the interference process parameters are different, as shown below.
[0046] In Example 6, the interference process parameter is: the cylindrical outer diameter of the embedded material is 0.12% larger than the inner diameter of the circular through hole of the base material.
[0047] In Example 7, the interference process parameter is: the cylindrical outer diameter of the embedded material is 0.19% larger than the inner diameter of the circular through hole of the base material.
[0048] The above embodiment is the same as that of Embodiment 1 in terms of the base material and the inlay material of the novel inlay composite target material and the remaining steps of the preparation method.
[0049] Examples 8-10 Examples 8-10 respectively provide a new type of mosaic composite target material.
[0050] The difference between the above embodiment and embodiment 1 is that the inlay materials are different, as shown below.
[0051] In Example 8: the inlay material is Ti / Al 55 / 45at%.
[0052] In Example 9: the inlay material is Ti / Al 50 / 50at%.
[0053] In Example 10: the embedded material is Al.
[0054] The above embodiment is the same as that of Embodiment 1 in terms of the base material and the inlay material of the novel inlay composite target material and the remaining steps of the preparation method.
[0055] Comparative Example Comparative Example 1 This comparative example provides a new type of inlaid composite target material.
[0056] The difference between this comparative example and Example 1 is that the upper and lower end surfaces of the base material are not leveled, and the inner wall of the central through hole is not perpendicular to the upper and lower end surfaces.
[0057] The base material and the embedding material of the novel embedded composite target material in this comparative example are the same as those in Example 1, as well as the remaining steps of the preparation method.
[0058] like Figure 3 As shown, the gap between the inlaid material and the base material of the inlaid composite target prepared in Comparative Example 1.
[0059] Comparative Example 2 This comparative example provides a new type of inlaid composite target material.
[0060] The difference between this comparative example and Example 1 is that no thread is processed on the inner wall of the through hole of the base material.
[0061] The base material and the embedding material of the novel embedded composite target material in this comparative example are the same as those in Example 1, as well as the remaining steps of the preparation method.
[0062] Comparative Example 3 This comparative example provides a new type of inlaid composite target material.
[0063] The difference between this comparative example and Example 1 is that the embedded material is processed into a cylindrical shape, and the outer diameter of the cylinder is 0.09% larger than the inner diameter of the circular hole of the base material.
[0064] The base material and the embedding material of the novel embedded composite target material in this comparative example are the same as those in Example 1, as well as the remaining steps of the preparation method.
[0065] Comparative Example 4 This comparative example provides a new type of inlaid composite target material.
[0066] The difference between this comparative example and Example 1 is that the embedded material is processed into a cylindrical shape, and the outer diameter of the cylinder is 0.22% larger than the inner diameter of the circular hole of the base material.
[0067] The base material and the embedding material of the novel embedded composite target material in this comparative example are the same as those in Example 1, as well as the remaining steps of the preparation method.
[0068] Performance test bonding strength: Place the inlaid composite target horizontally under the pressure head of the press, with a pad under the inlaid composite target. The pressure of the press acts on the inlaid material. When the pressure increases to a certain value P, the inlaid material will be ejected. The surface area of the inner wall of the substrate through hole is S, and the bonding strength P = F / S.
[0069] Test results: as shown in Table 1.
[0070] Table 1 Performance test results of the new embedded composite target materials in Examples 1-10 and Comparative Examples 1-4 Combined with the test results in Table 1, using the technical solution provided by the present invention, in the inlaid composite target materials prepared in Examples 1-10, the inlaid material and the base material are tightly bonded and have a high bonding strength.
[0071] In the process of preparing the inlaid composite target material in Comparative Example 1, the upper and lower end surfaces of the base material were not leveled, the through hole was not straight, and there was a gap between the inlaid material and the base material after inlaying. Figure 3 shown.
[0072] In the process of preparing the inlaid composite target material in Comparative Example 2, no threads were processed on the inner wall of the through hole of the base material; in the process of preparing the inlaid composite target material in Comparative Example 3, the interference fit was too small, and the bonding strength of the inlaid composite target material was lower than that of the embodiments of the present application.
[0073] In the process of preparing the inlaid composite target material in Comparative Example 4, the interference was too large, and the inlaid material got stuck during the downward movement, resulting in inlay failure.
[0074] By comparing the test results of Examples 1-5, the present application controls the thread height to 0.15-0.25 mm and the thread pitch to 0.3-0.4 mm in the matrix material raw material, which can further improve the bonding strength of the embedded composite target.
[0075] By comparing the test results of Examples 1, 6-7, the present application controls the interference in the base material raw material to be 0.15-0.18%, that is, the cylindrical outer diameter of the embedded material is 0.15-0.18% larger than the circular through hole inner diameter of the base material, which can further improve the bonding strength of the embedded composite target.
[0076] By comparing the test results of Examples 1, 8-10, the embedded material selected in the present application needs to contain Al. If the Al content is too low, the shrinkage after liquid nitrogen freezing is small and the bonding strength is small. Therefore, when the atomic percentage content of Al is controlled to be 50-100 at.%, the bonding strength of the embedded composite target can be further improved.
[0077] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A method for preparing a novel inlaid composite target material, characterized in that: The method is composed of a base material and an inlay material, and specifically includes the following steps in sequence: The base material is cylindrical in shape, the upper and lower end surfaces are leveled, a circular through hole is opened at the center, the upper end surface of the through hole is chamfered, the chamfer size is 0.5mm×45°~1.0mm×45°, and the inner wall of the through hole is perpendicular to the upper and lower end surfaces; The inner wall of the through hole of the base material is processed into a thread, the thread height is 0.1-0.3 mm, and the pitch is 0.2-0.5 mm; The inlay material is cylindrical, the outer diameter of the cylinder of the inlay material is 0.12-0.19% larger than the inner diameter of the circular through hole of the base material, and the height of the cylinder of the inlay material is the same as the thickness of the base material; The embedded material is placed in liquid nitrogen for freezing, taken out and embedded into the circular hole of the base material, and left for 5 to 10 minutes to obtain an embedded composite target blank; The novel inlaid composite target material is obtained through post-processing.
2. The method for preparing the novel inlaid composite target material according to claim 1, characterized in that: In the base material, the thread height is 0.15-0.25 mm, and the thread pitch is 0.3-0.4 mm.
3. The method for preparing the novel inlaid composite target material according to claim 1, characterized in that: The cylindrical outer diameter of the inlay material is 0.14-0.17% larger than the inner diameter of the circular through hole of the base material.
4. The method for preparing the novel inlaid composite target material according to claim 3, characterized in that: The inlay material is any one of TiAl, CrAl and Al, and the atomic percentage content of Al in the inlay material is 50-100 at.%.
5. The method for preparing the novel inlaid composite target material according to claim 1, characterized in that: The matrix material is any one of TiSi and Ti.
6. The method for preparing the novel inlaid composite target material according to claim 1, characterized in that: The dimensions of the base material are: diameter of 60-200 mm, thickness of 10-100 mm, and through-hole wall thickness of more than 15 mm.
7. The method for preparing the novel inlaid composite target material according to claim 1, characterized in that: The diameter of the inlay material is 30-170 mm.
8. The method for preparing the novel inlaid composite target material according to claim 1, characterized in that: The freezing time in the liquid nitrogen is 20 to 30 minutes.
9. The method for preparing the novel inlaid composite target material according to claim 1, characterized in that: The post-processing comprises the following steps: The inlaid composite target blank is machined to remove the chamfered layer on the upper end surface, and then machined to the required size on the drawing by machining or grinding; The processed inlaid composite target material is placed in alcohol for ultrasonic cleaning for 5 to 10 minutes, and then placed in a vacuum oven and baked at 105-115°C for 10 to 20 minutes.
10. A new type of inlaid composite target, characterized in that: The target is prepared by the method for preparing the novel inlaid composite target material according to any one of claims 1 to 9.
Citation Information
Patent Citations
Aluminum cerium metal target material and method for manufacturing aluminum cerium film by using same
CN102345100A
Titanium-copper composite circular target
CN109468599A
Plunger pump cylinder body structure and assembling method thereof
CN113464420A
Target material and metal tantalum surface composite gradient ceramic coating and preparation method thereof
CN115976481A
Composite PVD (Physical Vapor Deposition) target material
CN118613604A