Pre-baked anode for aluminum and composition of pre-baked anode

By adding large particles of residual anode material and optimizing the proportion of coke material in the formula of the prebaked anode for aluminum, the problem of the balance between the anode's voltage strength and resistivity under high-sulfur petroleum coke was solved, and the voltage strength and resistance were improved. The efficiency is reduced and it is suitable for high current production of aluminum electrolysis.

CN118756252AActive Publication Date: 2024-10-11ALAR NANJIANG CARBON NEW MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410929058.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-11
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

When using high-sulfur petroleum coke to produce prebaked anodes for aluminum, it is difficult to increase its compressive strength while maintaining the apparent density and not increasing the resistivity, and cannot meet the requirements of aluminum electrolysis companies for high current efficiency.

Method used

By adjusting the formula, increasing the residual anode material content of large particle materials, and optimizing the proportions of coarse coke, medium coke, fine coke and powdered coke in the composition, the anode's compressive strength is improved, while the consumption of asphalt is reduced, and the pressure resistance is achieved. Balance of strength, apparent density and resistivity.

Benefits of technology

The voltage-resistant strength of the prebaked anode for aluminum is increased, the resistivity is reduced, and the apparent density is maintained. It is suitable for industrial production, increases the current intensity and output of electrolytic aluminum, and reduces consumables.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004939110800000051
    Figure BDA0004939110800000051
  • Figure BDA0004939110800000052
    Figure BDA0004939110800000052
  • Figure BDA0004939110800000061
    Figure BDA0004939110800000061
Patent Text Reader

Abstract

The invention relates to a prebaked anode for aluminum and a composition thereof. The invention relates to a composition of a prebaked anode for aluminum. The composition comprises coarse coke, medium coke, fine coke, anode scrap and coke breeze, the proportion of the material with the particle size of 3-6cm in the coarse coke is greater than 90wt%; the material with the particle size of 1-3cm in the medium coke accounts for more than 85wt%; the proportion of the material with the particle size of 0.075-1cm in the fine coke is greater than 90wt%; in the coke breeze, the proportion of the material with the particle size of less than 0.075 cm is greater than 60 + / -5wt%; the proportion of materials with the particle size of 6-12cm in the anode scrap material is not less than 35wt%. According to the prebaked anode for aluminum and the composition of the prebaked anode for aluminum, disclosed by the invention, the compressive strength of the prebaked anode for aluminum is improved, and meanwhile, the apparent density is not reduced and the resistivity is not increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrode materials, and in particular relates to a prebaked anode using high-sulfur coke as a raw material and a composition thereof. Background Art

[0002] Aluminum prebaked anode is the electrode material for aluminum electrolysis. It is responsible for conducting electricity and participating in electrochemical reactions. It is called the "heart" of the electrolytic cell. Its quality has a direct impact on electrolytic production. The non-ferrous metal industry standard YS / T 285-2012 recommends its apparent density, true density, compressive strength, flexural strength, room temperature resistivity and other indicators. In order to improve the current efficiency, some aluminum electrolysis enterprises have increased the anode current density to 0.82A / cm 2 The above puts higher requirements on the resistivity and compressive strength of prebaked anodes for aluminum.

[0003] With the development of the negative electrode material industry, better quality low-sulfur and low-impurity petroleum coke has been increasingly used in the production of negative electrode materials. However, in order to reduce production costs, prebaked anodes for aluminum can only be produced using a large amount of high-sulfur petroleum coke. The high-sulfur petroleum coke has a low stacking density after calcination, which results in reduced volume density and compressive strength of prebaked anodes for aluminum.

[0004] Therefore, it is an urgent problem for carbon plants to produce prebaked anodes with high compressive strength suitable for aluminum electrolysis using high-sulfur petroleum coke as the main raw material. In view of this, the present invention proposes a new prebaked anode and its composition, which can produce prebaked anodes with high compressive strength using high-sulfur coke as the raw material. Summary of the invention

[0005] The object of the present invention is to provide a composition for a prebaked anode for aluminum. The prebaked anode for aluminum prepared by the composition increases the compressive strength of the prebaked anode for aluminum without reducing the apparent density or increasing the resistivity.

[0006] In order to achieve the above purpose, the technical solution adopted is:

[0007] A composition of a prebaked anode for aluminum, comprising: coarse coke, medium coke, fine coke, residual anode material and powdered coke;

[0008] The coarse coke has a particle size of 3-6 cm accounting for more than 90wt%;

[0009] The proportion of the particles with a diameter of 1-3 cm in the middle coke is greater than 85wt%;

[0010] The fine coke has a particle size of 0.075-1 cm accounting for more than 90wt%;

[0011] The powdered coke has a particle size of less than 0.075 cm accounting for 60±5wt%;

[0012] The residual electrode material having a particle size of 6-12 cm accounts for no less than 35wt%.

[0013] Furthermore, the residual electrode material includes: coarse coke, medium coke, fine powder coke and large particle material.

[0014] The particle size of the large particles is 6-12 cm;

[0015] The coarse coke particle size is 3-6 cm;

[0016] The particle size of the middle coke is 1-3 cm;

[0017] The particle size of the fine coke powder is 0-1 cm.

[0018] Furthermore, the content of large particles in the composition is not less than 5wt%.

[0019] Furthermore, the contents of the components in the residual electrode material are as follows: large particle material ≥ 35wt%, coarse coke 25-30wt%, medium coke 15-25wt%, and fine powder coke less than 25wt%.

[0020] Furthermore, the contents of the components in the composition are: coarse coke 18-20wt%, medium coke 25-27wt%, fine coke 7-10wt%, residual electrode material 15-18wt%, and powder coke 32-34wt%.

[0021] Another object of the present invention is to provide a prebaked anode for aluminum, which is prepared using the above-mentioned composition and has the advantages of high compressive strength, good apparent density and low resistivity.

[0022] In order to achieve the above purpose, the technical solution adopted is:

[0023] A prebaked anode for aluminum is prepared by using the above composition.

[0024] Furthermore, the prebaked anode has a compressive strength greater than 40 MPa, a resistivity less than 60 μΩ·m, and a volume density greater than 1.55 g / cm 3 .

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. The prebaked anode for aluminum and the composition thereof described in the present invention improve the compressive strength of the prebaked anode for aluminum by adjusting the formula and adding residual electrode materials containing large particles, thereby improving the impact resistance of the prebaked anode for aluminum to strong currents, so that aluminum electrolysis can increase the current intensity, increase production and reduce consumption, and have the basis of electrode materials without reducing the apparent density or increasing the resistivity.

[0027] 2. The prebaked anode for aluminum and its composition described in the present invention reduces the consumption of asphalt (0.2-0.5%) by adding residual electrode material containing large particles to replace part of the coarse, medium and fine coke in the original formula, thereby reducing the specific surface area of ​​the particles of the composition.

[0028] 3. The prebaked anode for aluminum and the composition thereof described in the present invention are simple in method, easy to implement and suitable for industrial production. DETAILED DESCRIPTION

[0029] In order to further illustrate the prebaked anode for aluminum and its composition of the present invention and achieve the intended purpose of the invention, the following is a detailed description of the specific implementation, structure, features and efficacy of the prebaked anode for aluminum and its composition according to the present invention in combination with the preferred embodiments. In the following description, different "one embodiment" or "embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics in one or more embodiments may be combined in any suitable form.

[0030] The following will further introduce the aluminum prebaked anode and its composition in detail in conjunction with specific embodiments:

[0031] According to the existing formula theory of prebaked anodes for aluminum, increasing the proportion of large-particle formula appropriately will help improve the compressive strength of prebaked anodes for aluminum. However, with the increase of large-particle materials, its resistivity increases and its apparent density decreases, and its appearance deteriorates. The existing technology must form a balance between the proportion of large-particle materials and the resistivity and apparent density. However, the existing technology increases the proportion of large-particle materials in calcined coke, which can appropriately improve the compressive strength of the anode, but its powder resistivity increases and its apparent density decreases, which cannot meet the requirements of electrolytic aluminum enterprises to strengthen current. When using high-sulfur petroleum coke to calcine calcined coke for production, it is difficult to achieve a balance between apparent density, resistivity and compressive strength under the current conventional formula.

[0032] In order to solve the above technical problems, the present invention proposes a prebaked anode for aluminum and its composition, which achieves the purpose of increasing the compressive strength of the prebaked anode for aluminum without reducing the apparent density and increasing the resistivity by improving the existing formula. The technical solution of the present invention is:

[0033] A composition of a prebaked anode for aluminum, comprising: coarse coke, medium coke, fine coke, residual anode material and powdered coke;

[0034] The coarse coke has a particle size of 3-6 cm accounting for more than 90wt%;

[0035] The proportion of the particles with a diameter of 1-3 cm in the middle coke is greater than 85wt%;

[0036] The fine coke has a particle size of 0.075-1 cm accounting for more than 90wt%;

[0037] The powdered coke has a particle size of less than 0.075 cm accounting for 60±5wt%;

[0038] The residual electrode material having a particle size of 6-12 cm accounts for no less than 35wt%.

[0039] Preferably, the residual electrode material includes: coarse coke, medium coke, fine powder coke and large particle material.

[0040] The particle size of the large particles is 6-12 cm;

[0041] The coarse coke particle size is 3-6 cm;

[0042] The particle size of the middle coke is 1-3 cm;

[0043] The particle size of the fine coke powder is 0-1 cm.

[0044] Further preferably, the content of large particles in the composition is not less than 5 wt %.

[0045] Further preferably, the contents of the components in the residual electrode material are as follows: large particle material ≥ 35wt%, coarse coke 25-30wt%, medium coke 15-25wt%, and fine powder coke less than 25wt%.

[0046] Preferably, the contents of the components in the composition are: coarse coke 18-20wt%, medium coke 25-27wt%, fine coke 7-10wt%, residual electrode material 15-18wt%, and powder coke 32-34wt%.

[0047] Another object of the present invention is to provide a prebaked anode for aluminum, which is prepared using the above-mentioned composition and has the advantages of extremely high compressive strength, good apparent density and low resistivity.

[0048] In order to achieve the above purpose, the technical solution adopted is:

[0049] A prebaked anode for aluminum is prepared by using the above composition.

[0050] Preferably, the prebaked anode has a compressive strength greater than 40 MPa, a resistivity less than 60 μΩ·m, and a bulk density greater than 1.55 g / cm 3 .

[0051] In the above technical solution, the residual electrode material with higher volume density and higher strength is added to the composition, and the particle size of the residual electrode material is increased, so as to increase the compressive strength of the prebaked anode without increasing the resistivity or reducing the apparent quality.

[0052] The differences between the calcined coke and the residual electrode material in the embodiments include not only the difference in elemental composition, but also the following differences:

[0053] The coarse coke, medium coke, fine coke, powder coke in the examples and the calcined coke in the comparative examples are prepared by calcining high-sulfur petroleum coke, and their physical and chemical indicators are: true density 2.07g / cm 3 , ash 0.3%, volatile matter 1.07%, sulfur 2.47%, powder resistivity 430μΩ.m, bulk density 0.68g / cm 3 .

[0054] The residual anode material is the residual anode produced by the electrolytic aluminum enterprise. Its physical and chemical indicators are: true density 2.09g / cm 3 , ash 1.47%, volatile matter 1.24%, sulfur 2.45%, powder resistivity 437μΩ.m, bulk density 0.82g / cm 3 ;

[0055] Example 1.

[0056] The specific steps are as follows:

[0057] (1) Obtaining residual electrode material

[0058] The pre-baked anode residues from the aluminum electrolysis are recovered and cleaned and then crushed in two stages. The first stage crushing uses a deep-cavity jaw crusher, and the second stage crushing uses a variable frequency impact crusher. The crushed materials are screened with a 12CM screen, and the materials larger than 12CM are returned to the second stage for secondary crushing.

[0059] The crushed materials are screened according to 6-12, 3-6, 1-3, and 0-1 cm to ensure that large particles of 6-12 cm account for 35wt% and above. If this is not achieved, fine-tune the secondary residual pole crushing frequency or the gap between the impact plates to ensure that large particles of 6-12 cm in the residual pole crushing account for 35% and above.

[0060] Finally, the contents of each component in the residual electrode material are: large particles (6-12cm) 35wt%, coarse coke (3-6cm) 25wt%, medium coke (1-3cm) 20wt%, and fine powder coke (0-1cm) 20wt%.

[0061] (2) The contents of the components in the prebaked anode composition for aluminum are: 20 wt% coke, 25 wt% medium coke, 10 wt% fine coke, 13 wt% residual anode material, and 32 wt% powder coke.

[0062] The proportion of coarse coke with a particle size of 3-6 cm is greater than 90wt%;

[0063] The proportion of particles with a diameter of 1-3 cm in the medium coke is greater than 85wt%;

[0064] The proportion of fine coke particles with a particle size of 0.075-1 cm is greater than 90wt%;

[0065] The particle size of the coke powder is less than 0.075 cm, accounting for 60±5wt%.

[0066] See the table below for specific ingredients:

[0067] Table 1 Content of each component in the prebaked anode composition for aluminum

[0068]

[0069] Table 2: Composition of residual electrode materials

[0070]

[0071] Example 2.

[0072] The specific operation steps are the same as those in Example 1, except for the differences shown in the table below:

[0073] Table 3 Content of each component in the prebaked anode composition for aluminum

[0074]

[0075] Table 4: Composition of residual electrode materials

[0076]

[0077] Example 3.

[0078] The specific operation steps are the same as those in Example 1, except for the differences shown in the table below:

[0079] Table 5 Content of each component in the prebaked anode composition for aluminum

[0080]

[0081] Table 6: Composition of residual electrode materials

[0082]

[0083] Example 4.

[0084] The specific operation steps are the same as those in Example 1, except for the differences shown in the table below:

[0085] Table 7 Content of each component in the prebaked anode composition for aluminum

[0086]

[0087]

[0088] Table 8: Composition of residual electrode materials

[0089]

[0090] Example 5.

[0091] The specific operation steps are the same as those in Example 1, except for the differences shown in the table below:

[0092] Table 9 Content of each component in the prebaked anode composition for aluminum

[0093]

[0094] Table 10: Composition of residual electrode materials

[0095]

[0096] Example 6.

[0097] The specific operation steps are the same as those in Example 1, except for the differences shown in the table below:

[0098] Table 11 Content of each component in the prebaked anode composition for aluminum

[0099]

[0100] Table 12: Composition of residual electrode materials

[0101]

[0102] Example 7.

[0103] The specific operation steps are the same as those in Example 1, except for the differences shown in the table below:

[0104] Table 13 Content of each component in the prebaked anode composition for aluminum

[0105]

[0106] Table 14: Composition of residual electrode materials

[0107]

[0108] Example 8.

[0109] The specific operation steps are the same as those in Example 1, except for the differences shown in the table below:

[0110] Table 15 Content of each component in the prebaked anode composition for aluminum

[0111]

[0112] Table 16: Composition of residual electrode materials

[0113]

[0114]

[0115] Comparative Example 1.

[0116] The specific operation steps are the same as those in Example 1, except for the differences shown in the table below:

[0117] Table 17 Content of each component in the prebaked anode composition for aluminum

[0118]

[0119] Table 18 Composition of calcined coke

[0120]

[0121] Comparative Example 2.

[0122] The specific operation steps are the same as those in Example 1, except for the differences shown in the table below:

[0123] Table 19 Content of each component in the prebaked anode composition for aluminum

[0124]

[0125] Table 20 Composition of calcined coke

[0126]

[0127]

[0128] Comparative Example 3.

[0129] The specific operation steps are the same as those in Example 1, except for the differences shown in the table below:

[0130] Table 21 Content of each component in the prebaked anode composition for aluminum

[0131]

[0132] Table 22 Composition of calcined coke

[0133]

[0134] Comparative Example 4.

[0135] The specific operation steps are the same as those in Example 1, except for the differences shown in the table below:

[0136] Table 23 Content of each component in the prebaked anode composition for aluminum

[0137]

[0138] Comparative Example 5.

[0139] The specific operation steps are the same as those in Example 1, except for the differences shown in the table below:

[0140] Table 24 Content of each component in the prebaked anode composition for aluminum

[0141]

[0142]

[0143] Table 25: Composition of residual electrode materials

[0144]

[0145] Comparative Example 6.

[0146] The specific operation steps are the same as those in Example 1, except for the differences shown in the table below:

[0147] Table 26 Content of each component in the prebaked anode composition for aluminum

[0148]

[0149] Table 27: Composition of residual electrode materials

[0150]

[0151] The formulations of Examples 1-8 and Comparative Examples 1-6 were prepared into products by a vibration molding process. The specific operation is to weigh the ingredients of the above composition, put them into a high-temperature kneading pot for heating and premixing according to the formulation, add modified liquid asphalt to knead into a plastic paste after the temperature reaches above 130°C, cool it to 140°C, send it into a molding machine mold box for vibration pressure molding, and then send it to a baking furnace to heat it to 1050°C for baking to become a prebaked anode for electrolytic aluminum.

[0152] The performance of the manufactured prebaked anodes was tested. No less than 200 prebaked anodes were sampled for each embodiment and no less than 20 prebaked anodes were sampled for each comparative example. The average values ​​of the test results are shown in Table 28.

[0153] Table 28

[0154]

[0155] Combined with Table 28, the following conclusions can be drawn:

[0156] (1) From Comparative Examples 1-4, it can be seen that increasing the proportion of large particle formula is beneficial to improving the compressive strength of aluminum prebaked anode. However, as the large particle material increases, its resistivity increases, the apparent density decreases, and the appearance deteriorates.

[0157] (2) It can be seen from Examples 2-7 and Example 1 and Comparative Examples 4-6 that when the amount of large particles added to the residual electrode material is less than 5wt%, the improvement on the compressive strength performance is not obvious.

[0158] (3) By comparing Examples 2-7 with Example 8, it can be seen that when the residual electrode material content in the aluminum prebaked anode formula is too high, although the compressive strength and apparent density will be improved and the resistivity will be reduced, the ash content is too high and the appearance is deteriorated.

[0159] (4) By comparing Examples 2-7 with Comparative Examples 1-4, it can be seen that the formulation of the present invention increases the compressive strength of the prebaked anode for aluminum while improving the apparent density and reducing the resistivity.

[0160] Combining the above embodiments, it can be seen that the technical solution of the present invention solves the problem of difficulty in balancing the apparent density, resistivity and compressive strength, and achieves the effect of improving the compressive strength of the prebaked anode without reducing the apparent density and increasing the resistivity. After the applicant adopted the technical solution of the present invention, the compressive strength of the prebaked anode for aluminum was increased from an average of 36MPa to 41MPa, the compressive strength was not less than 40MPa, the resistivity was reduced from 60.32μΩ·m to below 60μΩ·m, and the volume density was increased from 1.54g / cm 3 Increased to 1.56g / cm 3 .

[0161] The above is only a preferred embodiment of the embodiment of the present invention, and does not impose any form of limitation on the embodiment of the present invention. Any simple modification, equivalent changes and modifications made to the above embodiment based on the technical essence of the embodiment of the present invention are still within the scope of the technical solution of the embodiment of the present invention.

Claims

1. A composition for a prebaked anode for aluminum, characterized in that: include: Coarse coke, medium coke, fine coke, residual material and powder coke; The coarse coke has a particle size of 3-6 cm accounting for more than 90wt%; The proportion of the particles with a diameter of 1-3 cm in the middle coke is greater than 85wt%; The fine coke has a particle size of 0.075-1 cm accounting for more than 90wt%; The powdered coke has a particle size of less than 0.075 cm and accounts for more than 60±5wt%; The residual electrode material having a particle size of 6-12 cm accounts for no less than 35wt%.

2. The composition according to claim 1, characterized in that The residual electrode materials include: coarse coke, medium coke, fine powder coke and large particle materials; The particle size of the large particles is 6-12 cm; The coarse coke particle size is 3-6 cm; The particle size of the middle coke is 1-3 cm; The particle size of the fine coke powder is 0-1 cm.

3. The composition according to claim 2, characterized in that The content of large particles in the composition is not less than 5wt%.

4. The composition according to claim 3, characterized in that The contents of the components in the residual electrode material are as follows: large particle material ≥ 35wt%, coarse coke 25-30wt%, medium coke 15-25wt%, and fine powder coke less than 25wt%.

5. The composition according to claim 1, characterized in that The contents of the components in the composition are as follows: 18-20wt% of coarse coke, 25-27wt% of medium coke, 7-10wt% of fine coke, 15-18wt% of residual electrode material, and 32-34wt% of powder coke.

6. A prebaked anode for aluminum, characterized in that: The composition is prepared by using the composition described in any one of claims 1 to 5.

7. The prebaked anode according to claim 6, characterized in that: The prebaked anode has a compressive strength greater than 40 MPa, a resistivity less than 60 μΩ·m, and a volume density greater than 1.55 g / cm 3 .

Citation Information

Patent Citations

  • Carbon prebaked anode

    CN101974766A

  • Method for preparing prebaked anode by using aluminum electrolysis waste carbon cathode

    CN105441979A

  • Production method of porous anode carbon block for electrolytic aluminum

    CN113336550A

  • Preparation method of low-carbon-residue prebaked anode for aluminum electrolysis

    CN114349512A

  • Blend composition comprising petroleum coke and pyrolytic carbon for electrodes

    US20210277526A1