Preparation method of p-type high-purity germanium
By carrying out specific treatment in the zone melting furnace and selecting high-purity p-type zone-melting germanium ingots as the pulling growth material, the problem of insufficient proportion of p-type crystals and reduced purity in the traditional method was solved, and a higher proportion of p-type 13N was achieved. Crystal growth and preparation of high-purity germanium.
Patent Information
- Application Number
- CN202410768297.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-11
AI Technical Summary
In the traditional preparation method of p-type high-purity germanium, the proportion of grown p-type crystals is insufficient to meet the production needs of large-size detectors, and traditional doping methods will reduce the purity of high-purity germanium.
By loading corroded germanium ingots with a purity of over 5N and p-type dopants in a specific ratio in a zone melting furnace, zone melting is carried out in a high-purity nitrogen and hydrogen environment, and induction coils are used for heating to control the zone melting speed and Gas flow pressure, high purity p-type zone molten germanium ingot is selected as the pulling growth material to pull and grow the crystal.
A higher proportion of p-type 13N crystal growth is achieved to meet the needs of large-size detectors and improve the purity of high-purity germanium.
Smart Images

Figure BDA0004893285840000061
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of high-purity germanium, and more specifically to a method for preparing p-type high-purity germanium. Background Art
[0002] The crystals grown by the traditional preparation method are only 40-60% p-type at the head, and only part of them have a purity of 13N. Due to the length limitation, it cannot meet the production requirements of large-sized detectors. It is necessary to develop a p-type high-purity germanium preparation method to make the p-type crystals account for a higher proportion and increase the length of p-type high-purity germanium to meet the production requirements of large-sized detectors. Other single crystal p-type preparation methods currently published use the traditional doping method, adding solid dopants during pulling. This method is not suitable for high-purity germanium and will reduce the purity of high-purity germanium. Summary of the invention
[0003] In view of the problems existing in the background technology, an object of the present disclosure is to provide a method for preparing p-type high-purity germanium, which can obtain a higher proportion of p-type 13N crystals.
[0004] Thus, a method for preparing p-type high-purity germanium includes the following steps: S1, loading the corroded germanium ingot with a purity of 5N or more and the p-type dopant with a purity of 5N or more into a zone furnace at a mass ratio of 1000:(1-2); S2, introducing high-purity nitrogen with a purity of 9N or more through the air inlet and opening the exhaust port to maintain the flow pressure at normal pressure for 2 hours; S3, after the completion of step S2, switching the air inlet to introduce high-purity hydrogen with a purity of 9N or more for 2 hours, and maintaining the exhaust port to exhaust to maintain the flow pressure At normal pressure; S4, using an induction coil with a power of 70-85Kw to heat and heat up the zone melting of the chemical material, the zone melting speed is 200-300mm / h, and the zone melting is 30-40 times; S5, after the completion of step S4, stop the induction coil heating, switch the air inlet to the high-purity nitrogen gas of 9N or more and maintain the exhaust port to maintain normal pressure until the cooling is completed and the zone melting high-purity germanium ingot is taken out from the zone melting furnace; S6, detect the zone melting high-purity germanium ingot and select the p-type purity <2E11 / cm 3 The part is used as the pulling growth material to pull and grow the crystal to obtain a p-type high-purity germanium single crystal.
[0005] The beneficial effects of the present disclosure are as follows: by selecting a p-type purity <2E11 / cm 3 Part of it is used as the pulling growth material to pull and grow crystals, which can produce a higher proportion of p-type 13N crystals. DETAILED DESCRIPTION
[0006] It will be understood that the disclosed embodiments are merely examples of the present disclosure, which may be implemented in various forms, and therefore, the specific details disclosed herein should not be interpreted as limiting, but merely as a basis for the claims and as a representative basis for teaching one of ordinary skill in the art to implement the present disclosure in various ways.
[0007] [Preparation method of p-type high-purity germanium]
[0008] The method for preparing p-type high-purity germanium according to the present disclosure comprises the steps of:
[0009] S1, loading the etched germanium ingot with a purity of 5N or more and the p-type dopant with a purity of 5N or more into the zone furnace at a mass ratio of 1000:(1-2);
[0010] S2, introduce high-purity nitrogen gas of 9N or above through the air inlet and open the exhaust port to maintain the flow pressure at normal pressure for 2 hours;
[0011] S3, after step S2 is completed, the inlet is switched to allow high-purity hydrogen with a purity of 9N or above to pass for 2 hours, and the exhaust port is kept exhausted to keep the flow pressure at normal pressure;
[0012] S4, using an induction coil with a power of 70-85Kw to heat and heat the material to perform zone melting, the zone melting speed is 200-300mm / h, and the zone melting is 30-40 times;
[0013] S5, after step S4 is completed, the induction coil heating is stopped, the air inlet is switched to introduce high-purity nitrogen gas of 9N or above and the exhaust port is maintained to exhaust gas to maintain normal pressure until the cooling is completed and the zone melting high-purity germanium ingot is taken out from the zone melting furnace;
[0014] S6, test the zone melting high purity germanium ingot and select the p-type purity <2E11 / cm 3 The part is used as the pulling growth material to pull and grow the crystal to obtain a p-type high-purity germanium single crystal.
[0015] In the preparation method of p-type high-purity germanium according to the present disclosure, the high-purity germanium ingot is selected from the zone melting to have a p-type purity of less than 2E11 / cm 3 Part of it is used as the pulling growth material to pull and grow crystals, which can produce a higher proportion of p-type 13N crystals.
[0016] The detection of step S6 is performed by HL9900 detection of Toho Technology Company of the United States.
[0017] In one example, the p-type dopant is selected from boron (B).
[0018] In one example, in step S1, the etching is performed using a mixture of 68% HNO3:49% HF in a volume ratio of 1:4. Further, the etched high-purity germanium polycrystal is repeatedly rinsed in a pure water tank and blown dry with 9N high-purity nitrogen.
[0019] In step S6, the net impurity carrier concentration of the seed crystal used for pulling is less than 2E11 / cm 3 .
[0020] In one example, the pulling of the growing material in step S6 includes the steps of:
[0021] Sa, the purity of the etched product is p-type purity <2E11 / cm 3 The zone melting high purity germanium ingot is loaded into the crucible of the pulling furnace, wherein the etching is carried out with a mixture of 68% HNO3:49% HF in a volume ratio of 1:4. The etched high purity germanium polycrystal is repeatedly rinsed in a pure water tank and blown dry with 9N high purity nitrogen;
[0022] Sb, evacuate the pulling furnace and maintain the pressure at 1×10 -4 2h below Pa;
[0023] Sc, after step Sb is completed, 9N high-purity nitrogen is introduced into the pulling furnace, and the exhaust port is opened for exhaust, with a flow rate of 2-5L / min and a flow pressure of 0.04-0.05MPa, for 2h:
[0024] Sd, switch the exhaust port to allow high-purity hydrogen with a purity of 9N to flow for 2 hours at a flow rate of 2-5L / min, and maintain exhaust at the exhaust port to maintain a flow pressure of 0.095-0.105MPa;
[0025] Se, keep high-purity hydrogen flowing and keep the flow pressure, and heat up to melt the material;
[0026] Sf, after the completion of step Se, continue to introduce high-purity hydrogen and maintain the flow pressure, and carry out pulling until the cooling of the pulling is completed, then switch to 9N high-purity nitrogen, maintain exhaust at the exhaust port to maintain the flow pressure of 0.095-0.105MPa, and finally take out of the furnace.
[0027] The pulling in step Sf is performed as follows:
[0028] The crystal pulling rod rotates at 7rpm, and the crucible rotates at 7rpm.
[0029] Seeding: slowly insert the seed crystal into the melt in the crucible, adjust the power according to the melt interface, wait for 15 minutes after a certain width of aperture appears, start seeding, gradually increase the pulling speed of the crystal pulling rod to 24mm / h, maintain this pulling speed for 15 minutes, and control the crystal diameter to be stable at 6mm as the standard;
[0030] Neck shrinkage, manually increase the pulling speed, evenly increase the pulling speed by 15mm / h every 10min until the pulling speed reaches 100mm / h, and control the crystal diameter to be stable at 4mm as the standard;
[0031] Thin neck, keep the pulling speed at 100mm / h, pull the thin neck at this high pulling speed, and the pulling length at this stage is 120mm;
[0032] Shoulder release 1, open the crucible and raise it, the raising speed is 0.9mm / h; evenly reduce the pulling speed to 24mm / h, the frequency of reducing the pulling speed is to evenly reduce the pulling speed by 30mm / h every 10min; control the power to evenly cool down, the cooling frequency is 150w / h, shoulder release 1.5h, the crystal diameter gradually grows to 60mm;
[0033] Shoulder release 2, control the power to evenly cool down, reduce the rotation speed of the crystal pulling rod to 4rpm, reduce the number of crucible revolutions to 4rpm, and evenly increase the pulling speed of the crystal pulling rod to 32mm / h; the cooling frequency is 100w / h, continue shoulder release for 1.5h, and stop cooling when the crystal diameter is stabilized at 78mm;
[0034] Equalize the diameter, uniformly restore the pulling speed to 24mm / h, observe the crystal diameter, manually control the power to keep the crystal diameter at 78mm, and the equalize diameter process takes 5h;
[0035] At the end, lower the crucible lifting speed to 0.5mm / h, control the power to evenly cool down, the cooling frequency is 110w / h, and finish for 2.5h until the melt in the crucible is completely pulled out;
[0036] Cool down, turn off the pulling rod and crucible, control the power to cool down to room temperature, the cooling is divided into three stages: the first stage is 350w / h, cooling for 1h, the second stage is 550w / h, cooling for 2h; the third stage is 900w / h, cooling for 5-7h to room temperature; turn off the rotation of the pulling rod and crucible to complete the crystal pulling.
[0037] [test]
[0038] Example 1
[0039] Example 1 adopts the following steps:
[0040] S1, loading the etched 5N purity germanium ingot and 5N purity p-type dopant B into the zone furnace at a mass ratio of 1000:1. The etching is carried out using a mixed solution of 68% HNO3:49% HF at a volume ratio of 1:4. The etched high-purity germanium polycrystal is repeatedly rinsed in a pure water tank and blown dry with 9N high-purity nitrogen;
[0041] S2, introduce 9N high-purity nitrogen through the air inlet and open the exhaust port to maintain the flow pressure at normal pressure for 2 hours;
[0042] S3, after step S2 is completed, the inlet is switched to allow 9N high-purity hydrogen to pass for 2 hours, and the exhaust port is kept exhausted to keep the flow pressure at normal pressure;
[0043] S4, using an induction coil with a power of 80Kw to heat and heat the material to perform zone melting, the zone melting speed is 250mm / h, and the zone melting is 35 times;
[0044] S5, after step S4 is completed, the induction coil heating is stopped, the air inlet is switched to introduce 9N high-purity nitrogen and the exhaust port is maintained to exhaust to maintain normal pressure until the cooling is completed and the zone melting high-purity germanium ingot is taken out from the zone melting furnace;
[0045] S6, test the zone melting high purity germanium ingot and select the p-type purity <2E11 / cm 3 The part is used as the pulling growth material to pull and grow the crystal to obtain a p-type high-purity germanium single crystal.
[0046] Among them, the pulling of the growing material in step S6 includes the steps of:
[0047] Sa, the purity of the etched product is p-type purity <2E11 / cm 3 The zone melting high purity germanium ingot is loaded into the crucible of the pulling furnace, wherein the etching is carried out with a mixture of 68% HNO3:49% HF in a volume ratio of 1:4. The etched high purity germanium polycrystal is repeatedly rinsed in a pure water tank and blown dry with 9N high purity nitrogen;
[0048] Sb, evacuate the pulling furnace and maintain the pressure at 1×10 -4 Pa is measured for 2 hours;
[0049] Sc, after step Sb is completed, 9N high-purity nitrogen is introduced into the pulling furnace, and the exhaust port is opened for exhaust, with a flow rate of 3L / min and a flow pressure of 0.045MPa, for 2h:
[0050] Sd, switch the exhaust port to allow high-purity hydrogen with a purity of 9N to flow for 2 hours at a flow rate of 3L / min, and maintain exhaust at the exhaust port to maintain a flow pressure of 0.098MPa;
[0051] Se, keep high-purity hydrogen flowing and keep the flow pressure, and heat up to melt the material;
[0052] Sf, after the completion of step Se, continue to introduce high-purity hydrogen and maintain the flow pressure, and carry out pulling until the cooling of the pulling is completed, then switch to 9N high-purity nitrogen, maintain exhaust at the exhaust port to maintain the flow pressure of 0.098MPa, and finally take out of the furnace.
[0053] The pulling in step Sf is performed as follows:
[0054] The net impurity carrier concentration of the seed crystal installed on the crystal pulling rod is less than 2E11 / cm 3 , the crystal pulling rod rotates at 7rpm, the crucible rotates at 7rpm,
[0055] Seeding: slowly insert the seed crystal into the melt in the crucible, adjust the power according to the melt interface, wait for 15 minutes after a certain width of aperture appears, start seeding, gradually increase the pulling speed of the crystal pulling rod to 24mm / h, maintain this pulling speed for 15 minutes, and control the crystal diameter to be stable at 6mm as the standard;
[0056] Neck shrinkage, manually increase the pulling speed, evenly increase the pulling speed by 15mm / h every 10min until the pulling speed reaches 100mm / h, and control the crystal diameter to be stable at 4mm as the standard;
[0057] Thin neck, keep the pulling speed at 100mm / h, pull the thin neck at this high pulling speed, and the pulling length at this stage is 120mm;
[0058] Shoulder release 1, open the crucible and raise it, the raising speed is 0.9mm / h; evenly reduce the pulling speed to 24mm / h, the frequency of reducing the pulling speed is to evenly reduce the pulling speed by 30mm / h every 10min; control the power to evenly cool down, the cooling frequency is 150w / h, shoulder release 1.5h, the crystal diameter gradually grows to 60mm;
[0059] Shoulder release 2, control the power to evenly cool down, reduce the rotation speed of the crystal pulling rod to 4rpm, reduce the number of crucible revolutions to 4rpm, and evenly increase the pulling speed of the crystal pulling rod to 32mm / h; the cooling frequency is 100w / h, continue shoulder release for 1.5h, and stop cooling when the crystal diameter is stabilized at 78mm;
[0060] Equalize the diameter, uniformly restore the pulling speed to 24mm / h, observe the crystal diameter, manually control the power to keep the crystal diameter at 78mm, and the equalize diameter process takes 5h;
[0061] At the end, lower the crucible lifting speed to 0.5mm / h, control the power to evenly cool down, the cooling frequency is 110w / h, and finish for 2.5h until the melt in the crucible is completely pulled out;
[0062] Cool down, turn off the pulling rod and crucible, control the power to cool down to room temperature, the cooling is divided into three stages: the first stage is 350w / h, cooling for 1h, the second stage is 550w / h, cooling for 2h; the third stage is 900w / h, cooling for 6h to room temperature; turn off the rotation of the pulling rod and crucible to complete the crystal pulling.
[0063] Comparative Example 1
[0064] Except that the p-type dopant B with purity 5N in step S1 does not exist, the rest is the same as in Example 1. That is, there is no doping compared to Comparative Example 1.
[0065] The crystals obtained in Example 1 and Comparative Example 1 were cut into equal diameter parts, and then sliced from both ends of the equal diameter parts to meet the net impurity carrier concentration of ≤2E10 / cm 3 As a qualified section, the length of the qualified section is divided by the ratio of the length of the equal diameter part, and the net impurity carrier concentration and doping type are tested by HL9900 of Toho Technology Company of the United States.
[0066] Table 1 Results of Example 1 and Comparative Example 1
[0067]
[0068] It can be seen from Table 1 that, compared with Comparative Example 1, Example 1 obtains 90% of qualified segments, that is, Example 1 obtains a higher proportion of p-type 13N crystals.
[0069] The above detailed description is used to describe multiple exemplary embodiments, but this document is not intended to be limited to the explicitly disclosed combinations. Therefore, unless otherwise stated, the various features disclosed herein can be combined together to form multiple additional combinations that are not shown for the sake of simplicity.
Claims
1. A method for preparing p-type high-purity germanium, characterized in that: Includes steps: S1, loading the etched germanium ingot with a purity of 5N or more and the p-type dopant with a purity of 5N or more into the zone furnace at a mass ratio of 1000:(1-2); S2, introduce high-purity nitrogen gas of 9N or above through the air inlet and open the exhaust port to maintain the flow pressure at normal pressure for 2 hours; S3, after step S2 is completed, the inlet is switched to allow high-purity hydrogen with a purity of 9N or above to pass for 2 hours, and the exhaust port is kept exhausted to keep the flow pressure at normal pressure; S4, using an induction coil with a power of 70-85Kw to heat and heat the material to perform zone melting, the zone melting speed is 200-300mm / h, and the zone melting is 30-40 times; S5, after step S4 is completed, the induction coil heating is stopped, the air inlet is switched to introduce high-purity nitrogen gas of 9N or above and the exhaust port is maintained to exhaust gas to maintain normal pressure until the cooling is completed and the zone melting high-purity germanium ingot is taken out from the zone melting furnace; S6, test the zone melting high purity germanium ingot and select the p-type purity <2E11 / cm 3 The part is used as the pulling growth material to pull and grow the crystal to obtain a p-type high-purity germanium single crystal.
2. The method for preparing p-type high-purity germanium according to claim 1, characterized in that: The p-type dopant is selected from boron (B).
3. The method for preparing p-type high-purity germanium according to claim 1, characterized in that: In step S1, a mixed solution of 68% HNO3:49% HF in a volume ratio of 1:4 is used for etching.
4. The method for preparing p-type high-purity germanium according to claim 1, characterized in that: In step S6, the net impurity carrier concentration of the seed crystal used for pulling is less than 2E11 / cm 3 .