Single crystal nitride growth and controllable stripping method based on highly oriented graphene buffer layer
By growing highly oriented graphene on an epitaxial substrate and annealing pretreatment, combined with the use of a metal stress layer, the controlled peeling and transfer of single crystal nitride is achieved, solving the problem of single crystal nitride film quality and transfer in the existing technology. Defect problems in the process are applicable to a variety of semiconductor devices.
Patent Information
- Application Number
- CN202410747934.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-11
AI Technical Summary
It is difficult to stably obtain large-area single-crystal nitride self-supporting films with existing technology, and the two-dimensional material transfer process is time-consuming, laborious, and prone to defects, which limits the heterogeneous integration of nitride and other materials and the application of flexible devices.
Highly oriented graphene is grown on an epitaxial substrate, and the covalent bonding between nitride and graphene is enhanced through annealing pretreatment to grow a single crystal nitride epitaxial layer, and then a metal stress layer is deposited on the nitride surface to induce a graphene layer separation to achieve controllable peeling and transfer of single crystal nitride.
It achieves controllable peeling and transfer of high-quality single crystal nitride, avoids the problems of self-peeling and incomplete peeling, simplifies the process, and ensures the quality of graphene crystals. It is suitable for large-scale preparation of high-quality self-supporting nitride films and is suitable for Vertical structure devices and flexible devices.
Smart Images

Figure CN118756341A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductors and relates to a single crystal nitride growth and controllable stripping method based on a highly oriented graphene buffer layer. Background Art
[0002] Compared with the first two generations of semiconductor materials, the third generation of semiconductor materials represented by gallium nitride (GaN) has the advantages of large bandgap, high thermal conductivity, high breakdown field strength, high saturated electron drift rate and strong radiation resistance. Therefore, group III nitride semiconductor materials are currently new materials with great potential and have received extensive attention from academia and industry in recent years. Due to the strong covalent bond between nitride and epitaxial substrate, it is impossible to transfer nitride films by simple mechanical peeling, which greatly limits the heterogeneous integration of nitride and other materials and their application in flexible devices.
[0003] Although laser lift-off and chemical etching can produce self-supporting GaN films, both methods have major drawbacks. Laser lift-off produces a large number of gallium droplets at the lift-off interface, resulting in a rough lift-off interface and high energy consumption. The sacrificial layer relied on by the chemical etching method is difficult to be compatible with the nitride epitaxial process. The etching liquid is a hazardous reagent and the etching process is time-consuming. Therefore, the quality of the self-supporting GaN film is poor and the efficiency is low.
[0004] In recent years, researchers have proposed a strategy for epitaxial growth of GaN on two-dimensional materials, relying on the weak van der Waals force between the two-dimensional material and GaN or the epitaxial substrate to achieve mechanical exfoliation of GaN. However, the single crystallinity of the nitride and the complete van der Waals interface between the nitride / epitaxial substrate are difficult to guarantee at the same time, and self-exfoliation of polycrystalline nitrides or incomplete exfoliation of single-crystalline nitrides often occurs. This strategy is difficult to stably obtain large-area single-crystalline GaN self-supporting films, and still needs to be improved. In addition, the process of transferring the two-dimensional material from the catalytic substrate to the epitaxial substrate is not only time-consuming and labor-intensive, but also produces defects in the two-dimensional material. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a method for the growth and controllable stripping of a single crystal nitride based on a highly oriented graphene buffer layer. Highly oriented graphene is directly grown on an epitaxial substrate, and the covalent bonding of the nitride on the graphene surface is promoted by an annealing pretreatment process, thereby continuing the in-plane orientation consistency of the graphene and growing a single crystal nitride epitaxial layer. The bonding force between the nitride epitaxial layer and the epitaxial substrate is regulated by adjusting the growth thickness of the graphene and the annealing pretreatment process to avoid self-stripping or incomplete stripping of the epitaxial layer. Finally, a metal stress layer of appropriate thickness is deposited on the surface of the single crystal nitride epitaxial layer to induce separation of graphene layers with weak van der Waals forces, so as to achieve controllable stripping and transfer of the single crystal nitride.
[0006] To achieve the above technical objectives, the technical solution of the present invention includes the following steps:
[0007] 1) Growing highly oriented graphene on an epitaxial substrate;
[0008] 2) Annealing pretreatment of epitaxial substrate / graphene;
[0009] 3) growing a nitride epitaxial layer on the epitaxial substrate / highly oriented graphene;
[0010] 4) depositing a metal stress layer of a preset thickness on the surface of the nitride epitaxial layer;
[0011] 5) Stripping the nitride epitaxial layer and transferring to a new supporting substrate.
[0012] 5a) adding a sticky support layer on the surface of the metal stress layer;
[0013] 5b) fixing the above structure and stripping the nitride epitaxial layer;
[0014] 5c) transferring the stripped nitride epitaxial layer to a new supporting substrate;
[0015] 5d) Cleaning and recovering the epitaxial substrate.
[0016] In step 1), highly oriented graphene is grown on an epitaxial substrate, wherein the epitaxial substrate comprises one of the following substrates: sapphire, aluminum nitride, gallium oxide, silicon carbide, and diamond; the highly oriented graphene has graphene domains with substantially consistent in-plane orientation and a thickness of 2-5 layers.
[0017] In step 2), the epitaxial substrate / graphene is pre-annealed, and the gas environment of the annealing treatment includes ammonia, hydrogen or nitrogen; the annealing time is 1 to 120 minutes; and the annealing temperature is 100 to 1500°C.
[0018] In step 3), a nitride epitaxial layer is epitaxially grown on the epitaxial substrate / graphene, and the nitride epitaxial layer includes one or more of the following epitaxial layers: AlN, GaN, AlGaN, InGaN, etc.
[0019] In step 4), a metal stress layer of a preset thickness is deposited on the surface of the nitride epitaxial layer, and the deposition method includes sputtering, evaporation or electroplating; the type of the metal stress layer includes nickel or cadmium; the preset thickness is 200 to 6000 nm.
[0020] In step 5a), a sticky support layer is added on the surface of the stress layer, including a support layer such as a thermal release tape or spin-coating PI.
[0021] In step 5b), the above structure is fixed and the nitride epitaxial layer is peeled off. The fixing method is to use tape or a vacuum pump to suck the substrate; the peeling method is to clamp a corner of the support layer and slowly lift it upward to separate the nitride epitaxial layer from the epitaxial substrate.
[0022] In step 5c), the stripped nitride epitaxial layer is transferred to a new supporting substrate. After spin coating a sticky organic substance such as PI on the surface of the new supporting substrate, the nitride epitaxial layer is transferred to the surface of the new supporting substrate; the new supporting substrate includes one of the following substrates: a flexible substrate such as PET film and copper foil or a rigid substrate such as diamond; the sticky supporting layer is removed by heating, organic solvent or etching liquid; the metal stress layer is removed by using a corresponding metal etching liquid to complete the transfer of the nitride epitaxial layer.
[0023] In step 5d), the epitaxial substrate is cleaned and recovered, and the graphene remaining on the surface of the epitaxial substrate is removed by oxygen plasma, and then the residual metal and organic matter are removed by a mixture of sulfuric acid and hydrogen peroxide, followed by ultrasonic cleaning with acetone, ethanol and deionized water, and finally the epitaxial substrate is blown dry with a nitrogen gun.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The present invention directly grows highly oriented graphene on an epitaxial substrate, promotes the covalent bonding of nitrides on the graphene surface by an annealing pretreatment process, and then continues the in-plane orientation consistency of graphene to grow a single crystal nitride epitaxial layer. Not only does it avoid the cumbersome process of transferring graphene, but it also ensures the crystal quality of graphene and provides a clear source of nitride orientation. In particular, the present invention utilizes the characteristics of directly growing graphene and the epitaxial substrate having strong coupling, further enhances the bonding force between graphene and the epitaxial layer and the epitaxial substrate through annealing and nitride growth processes, and regulates the bonding force between the epitaxial layer and the epitaxial substrate to a controllable peeling range in combination with the growth thickness of graphene. This process solves the problem of incomplete peeling caused by transferred graphene defects and the problem of epitaxial layer self-peeling caused by multilayer graphene.
[0026] Compared with transferring epitaxial nitride of two-dimensional materials on epitaxial substrates, the process of the present invention is simple, the quality of graphene crystals is stable and reliable, the source of nitride single crystallinity is clear, and the crystal quality is guaranteed. The present invention is stable and compatible with existing semiconductor processes, suitable for large-scale preparation of high-quality self-supporting nitride films, and the prepared high-quality nitride self-supporting films can be used in the fields of vertical structure devices, micro-electromechanical systems and flexible devices. The epitaxial substrate used in the present invention can be recycled and reused multiple times, which greatly reduces the preparation cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 A schematic diagram of a single crystal nitride growth and controllable exfoliation method based on a highly oriented graphene buffer layer according to an embodiment of the present invention;
[0028] Figure 2 The Raman spectra of GaN directly grown, grown, and stripped are shown in the embodiments of the present invention. DETAILED DESCRIPTION
[0029] In order to make the technical solutions and advantages of the present invention more clearly explained, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. The implementation methods not shown or described in the accompanying drawings are forms well known to those skilled in the art. Parameter demonstrations containing specific values are provided herein, but the parameters do not need to be exactly equal to the corresponding values, but are approximated to the corresponding values within an acceptable error tolerance or design constraint.
[0030] Reference Figure 1 As shown in the schematic diagram, the single crystal nitride growth and controllable exfoliation method based on a highly oriented graphene buffer layer includes the following steps:
[0031] 1) Growing highly oriented graphene on an epitaxial substrate;
[0032] 1a) Clean the epitaxial substrate and place it in a vertical cold wall CVD system;
[0033] 1b) introducing methane, argon and hydrogen, with a methane flow rate of 20 to 100 sccm, an argon flow rate of 100 to 1000 sccm, and a hydrogen flow rate of 100 to 1000 sccm;
[0034] 1c) adjusting the reaction chamber pressure to 10-100 mbar and the reaction chamber temperature to 1000-1600° C. to grow highly oriented graphene;
[0035] 1d) Take out the epitaxial substrate / highly oriented graphene and measure the graphene Raman spectrum. Figure 2 shown.
[0036] 2) Annealing pretreatment of epitaxial substrate / highly oriented graphene;
[0037] 2a) placing the sample obtained in step 1) in a metal organic chemical vapor deposition chamber;
[0038] 2b) The annealing atmosphere is ammonia or nitrogen, the annealing temperature is 950-1100° C., and the annealing time is 2-30 minutes.
[0039] 3) growing a nitride epitaxial layer on the epitaxial substrate / highly oriented graphene;
[0040] 3a) after the annealing pretreatment in step 2) is completed, growing an aluminum nitride or gallium nitride nucleation layer on the epitaxial substrate / highly oriented graphene at a growth temperature of 550-1200° C. and a thickness of 5-100 nm;
[0041] 3b) growing a nitride epitaxial layer and an epitaxial structure required for the device, with a growth temperature of 850 to 1200° C. and a thickness of 500 to 10000 nm;
[0042] 3c) After the chamber cools down to room temperature, take out the epitaxial structure and measure its Raman spectrum. Figure 2 shown.
[0043] 4) depositing a metal stress layer of a preset thickness on the surface of the nitride epitaxial layer;
[0044] 4a) placing the sample obtained in step 3) in a magnetron sputtering table and turning on a vacuum pump to clean the chamber;
[0045] 4b) depositing a metal stress layer nickel on the surface of the epitaxial structure, with a sputtering power of 100 to 400 W and a deposition thickness of 500 to 6000 nm.
[0046] 5) Stripping the nitride epitaxial layer and transferring to a new supporting substrate.
[0047] 5a) Paste a thermal release tape on the surface of the sample obtained in step 4), hold a corner of the thermal release tape with tweezers, and slowly peel it off until the entire nitride epitaxial layer is separated from the epitaxial substrate. After peeling, there is no nitride residue on the surface of the epitaxial substrate, but some graphene is still retained. Figure 2 As shown;
[0048] 5b) Spin-coating PI glue on the surface of the PET film, attaching the sample peeled off in step 5a) to the PET film and baking it on a heating table at 100° C. for 5 min, removing it after the thermal release glue loses adhesion and warps, and then placing the nickel stress layer / nitride epitaxial layer / graphene / PET film structure in a ferric chloride solution to corrode the nickel stress layer, completing the transfer of the nitride epitaxial layer;
[0049] 5c) The substrate stripped in step 5a) is placed in a plasma cleaning machine with a plasma power of 30 to 200 W and a cleaning time of 5 to 25 minutes. It is then cleaned in sulfuric acid, a hydrogen peroxide mixed solution, acetone, ethanol and deionized water in sequence, and dried with a nitrogen gun to recover the epitaxial substrate.
[0050] The above specific embodiments further illustrate the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for the growth and controlled exfoliation of single crystal nitrides based on a highly oriented graphene buffer layer, characterized in that: include: Step 1) growing a highly oriented graphene buffer layer on an epitaxial substrate; Step 2) performing annealing pretreatment on the epitaxial substrate and the highly oriented graphene buffer layer; Step 3) growing a nitride epitaxial layer on the epitaxial substrate and the highly oriented graphene buffer layer; Step 4) depositing a metal stress layer of a preset thickness on the surface of the nitride epitaxial layer; Step 5) Stripping the nitride epitaxial layer and transferring it to a new supporting substrate. 5a) adding a sticky support layer on the surface of the metal stress layer; 5b) fixing the structure of adding a sticky support layer on the surface of the metal stress layer and peeling off the nitride epitaxial layer; 5c) transferring the stripped nitride epitaxial layer to a new supporting substrate; 5d) Cleaning and recovering the epitaxial substrate.
2. The method for growth and controllable exfoliation of single crystal nitride based on a highly oriented graphene buffer layer according to claim 1, characterized in that: In step 1), highly oriented graphene is grown on an epitaxial substrate, wherein the epitaxial substrate comprises one of the following substrates: sapphire, aluminum nitride, gallium oxide, silicon carbide, and diamond; the highly oriented graphene has graphene domains with consistent in-plane orientation and a thickness of 2-5 layers.
3. The method for growth and controllable exfoliation of single crystal nitride based on a highly oriented graphene buffer layer according to claim 1, characterized in that: In step 2), the epitaxial substrate / graphene is pre-annealed, and the gas environment of the annealing treatment includes ammonia, hydrogen or nitrogen; the annealing time is 1 to 120 minutes; and the annealing temperature is 100 to 1500°C.
4. The method for growth and controllable exfoliation of single crystal nitride based on a highly oriented graphene buffer layer according to claim 1, characterized in that: In step 3), a nitride epitaxial layer is grown on the epitaxial substrate / graphene, and the nitride epitaxial layer includes one or more of the following epitaxial layers: AlN, GaN, AlGaN, InGaN.
5. The method for growth and controllable exfoliation of single crystal nitride based on a highly oriented graphene buffer layer according to claim 1, characterized in that: In step 4), a metal stress layer of a preset thickness is deposited on the surface of the nitride epitaxial layer, and the deposition method includes sputtering, evaporation or electroplating; the type of the metal stress layer includes nickel or cadmium; the preset thickness is 200 to 6000 nm.
6. The method for growth and controllable exfoliation of single crystal nitride based on a highly oriented graphene buffer layer according to claim 1, characterized in that: In step 5a), a sticky support layer is added on the surface of the metal stress layer, including sticking a thermal release tape and spin coating a polyimide PI support layer.
7. The method for growth and controllable exfoliation of single crystal nitride based on a highly oriented graphene buffer layer according to claim 1, characterized in that: In step 5b), the structure of adding a sticky support layer to the surface of the metal stress layer is fixed, and the nitride epitaxial layer is peeled off. The fixing method is to use tape or a vacuum pump to suck the substrate; the peeling method is to clamp a corner of the support layer and lift it upward to separate the nitride epitaxial layer from the epitaxial substrate.
8. The method for growth and controllable exfoliation of single crystal nitride based on a highly oriented graphene buffer layer according to claim 1, characterized in that: In step 5c), the stripped nitride epitaxial layer is transferred to a new supporting substrate. After spin coating PI sticky organic matter on the surface of the new supporting substrate, the nitride epitaxial layer is transferred to the surface of the new supporting substrate; the new supporting substrate includes one of the following substrates: polyethylene terephthalate PET film and copper foil flexible substrate or diamond rigid substrate; the sticky supporting layer is removed by heating, organic solvent or etching liquid; the metal stress layer is removed by using the corresponding metal etching liquid to complete the transfer of the nitride epitaxial layer.
9. The method for growth and controllable exfoliation of single crystal nitride based on a highly oriented graphene buffer layer according to claim 1, characterized in that: In step 5d), the epitaxial substrate is cleaned and recovered, and the graphene remaining on the surface of the epitaxial substrate is removed by plasma, and then the residual metal and organic matter are removed by a mixture of sulfuric acid and hydrogen peroxide, followed by ultrasonic cleaning with acetone, ethanol and deionized water, and finally the epitaxial substrate is blown dry with a nitrogen gun.