Preparation method of hydrophobic anti-ultraviolet microfiber leather
Through dopamine hydrochloride modification and pterostilbene coating technology, combined with the reaction of photoinitiator and hexadecanethiol, the problem of insufficient water resistance of synthetic leather is solved, efficient hydrophobic and UV-resistant performance improvement is achieved, and a stable coating is formed , meeting the waterproof performance requirements in complex environments.
Patent Information
- Application Number
- CN202410995091.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-11
AI Technical Summary
Existing synthetic leather has insufficient water resistance and durability, and it is particularly difficult to meet waterproof performance requirements under complex outdoor climate conditions.
Synthetic leather was modified with dopamine hydrochloride, and ZIF-8 was grown in situ on the fiber through dipping and adsorption to construct a rough surface. It was then coated with an ethanol solution of pterostilbene, and then mixed with a photoinitiator and hexadecanethiol. UV light irradiation is carried out in the solution to promote the thiol-ene reaction and improve the UV resistance and water resistance of the synthetic leather.
Significantly improves the hydrophobicity and UV resistance of synthetic leather, forms a stable coating, and enhances its stability and tolerance in different environments.
Smart Images

Figure CN118756498A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of synthetic leather preparation, and particularly relates to a method for preparing hydrophobic and UV-resistant ultraviolet microfiber leather. Background Art
[0002] Superhydrophobic surfaces have attracted extensive attention in the fields of anti-corrosion, self-cleaning, anti-fogging, oil-water separation, etc. However, the preparation of superhydrophobic surfaces still has many limitations, such as limited service life and the use of toxic fluorine-based substances. Therefore, some strategies for fluorine-free superhydrophobic coatings have been developed by hydrophobic modified nanoparticles. Nevertheless, there is still a need to develop more versatile methods to further promote the application of fluorine-free superhydrophobic surfaces.
[0003] Synthetic leather is widely used in home furnishing, shoes, clothing, automobiles and other fields, and its waterproof performance is particularly important, especially under the conditions of outdoor use, which is inevitably affected by the complex climate of the environment. Superhydrophobic modification is achieved by directly loading MOF onto the fabric. This method of modifying the fabric shows poor fastness properties, which hinders its practical application. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing hydrophobic synthetic leather to solve the problem that the synthetic leather produced by the prior art has insufficient water resistance and durability.
[0005] To achieve the above object, the present invention adopts the following technical solutions: A hydrophobic ultraviolet-resistant microfiber leather comprises the following steps: firstly, dopamine hydrochloride is used to modify synthetic leather to improve the adhesion of the synthetic leather surface; then, ZIF-8 is grown in situ on the fiber by immersion adsorption to construct a rough surface; then, the ZIF-8 is coated by immersion in an ethanol solution of pterostilbene to form a core-shell structure; then, the ZIF-8 is immersed in a mixed solution containing a photoinitiator and hexadecanethiol; ultraviolet light is used to accelerate the thiol-ene reaction between the thiol and the C=C bond on the pterostilbene, so as to improve the ultraviolet-resistant performance and water resistance of the synthetic leather.
[0006] The specific preparation method of the hydrophobic anti-ultraviolet microfiber leather comprises the following steps: (1) After adding tris(hydroxymethyl)aminomethane to deionized water to adjust the pH, dopamine hydrochloride is added and stirred evenly, and then synthetic leather is immersed in the dopamine hydrochloride solution, taken out, washed, and dried to obtain pretreated synthetic leather; (2) immersing the synthetic leather pretreated in step (1) in a zinc acetate solution, then slowly adding a 2-methylimidazole solution, stirring and mixing, and then standing, then taking out the synthetic leather, washing, and drying, to obtain a ZIF-8 modified synthetic leather; (3) soaking the ZIF-8 modified synthetic leather obtained in step (2) in an ethanol solution of pterostilbene, taking it out, washing it, and drying it to obtain a pterostilbene modified synthetic leather; (4) Adding photoinitiator 1173 and hexadecanethiol to ethanol, ultrasonically homogenizing, then immersing the pterostilbene-modified synthetic leather obtained in step (3) in the mixed solution, irradiating it with an ultraviolet lamp under stirring conditions, then taking it out, washing and drying it to obtain the hydrophobic and ultraviolet-resistant ultraviolet leather.
[0007] Furthermore, in step (1), tris(hydroxymethyl)aminomethane is added to adjust the pH to 8.5.
[0008] Furthermore, the synthetic leather in step (1) is specifically PA6 / PU type ultrafine fiber synthetic leather.
[0009] Furthermore, the mass concentration of the dopamine hydrochloride solution in step (1) is 1% to 1.5%.
[0010] Furthermore, the soaking time in step (1) is 24 h.
[0011] Furthermore, the volume ratio of the zinc acetate solution to the 2-methylimidazole solution used in step (2) is 2.5:1, wherein the mass ratio of the zinc acetate dihydrate to the 2-methylimidazole used is 1:3.
[0012] Furthermore, the standing time in step (2) is 24 h.
[0013] Furthermore, the mass concentration of the pterostilbene ethanol solution in step (3) is 1.5%.
[0014] Furthermore, the soaking time in step (3) is 30 min.
[0015] Furthermore, in the mixed solution of step (4), the mass concentration of the photoinitiator is 0.02%, and the mass concentration of hexadecanethiol is 1% to 2%.
[0016] Furthermore, the stirring speed in step (4) is 30 r / min.
[0017] Furthermore, the UV lamp used in step (4) is specifically a 365 nm UV LED lamp with an irradiation power of 500 mW·cm −2 The irradiation time is 30 min.
[0018] The present invention utilizes the strong adhesion of dopamine (DA) to improve the interfacial activity and adhesion of the fiber surface, so that the MOF particles can be fixed on the fiber surface to produce a rough surface. Hexadecenethiol is a long-chain alkyl with low surface free energy, and the -SH contained in it can produce a thiol-ene click chemical reaction with the C=C bond to introduce a long alkane chain. This rough surface structure and the introduction of the long alkane chain together give the synthetic leather a superhydrophobic surface. Pterostilbene, as a phenolic derivative, can be firmly attached to the surface of MOF to form a core-shell structure, and the C=C bond contained in it can provide a reaction site to achieve a thiol-ene click chemical reaction with hexadecenethiol; at the same time, the benzene ring structure, methoxy group and conjugated π electrons contained in pterostilbene give it an outstanding ultraviolet shielding function, and ultraviolet irradiation will not significantly affect the stability of pterostilbene, so it can effectively improve the anti-ultraviolet ability of synthetic leather.
[0019] The beneficial effects of the present invention are: The present invention provides a method for preparing a hydrophobic anti-ultraviolet ultra-fiber leather, which first utilizes dopamine to self-polymerize to form polydopamine (PDA) to form a thin adhesive film on the surface of the material, and then uses it as a multifunctional secondary reaction platform so that metal ions can be absorbed onto the PDA layer, thereby growing a metal organic framework (MOF) on the fiber surface to construct a micro-nano rough surface; then, pterostilbene is used to coat the generated ZIF-8, and the characteristic that phenolic derivatives can firmly adhere to the surface of the MOF material to form a core-shell structure is utilized to form a stable coating on the surface of the synthetic leather. At the same time, the benzene ring and specific methylated groups contained in pterostilbene have excellent antioxidant, scattering and ultraviolet absorption properties, so that the obtained material can have excellent anti-ultraviolet properties. In addition, by utilizing the C=C bond contained in pterostilbene to covalently bond with the -SH group contained in hexamethylenethiol, and introducing a long alkane chain, the prepared hydrophobic anti-ultraviolet coating can have excellent stability and tolerance, and can meet the use requirements of the modified synthetic leather in different environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a scanning electron microscope image of the initial synthetic leather.
[0021] Figure 2 This is a scanning electron microscope image of the hydrophobic and UV-resistant microfiber leather prepared in Example 1 and its partial magnified image.
[0022] Figure 3 This is the infrared spectrum of the hydrophobic and UV-resistant microfiber leather obtained in Example 1.
[0023] Figure 4 is the contact angle of the initial synthetic leather.
[0024] Figure 5This is the contact angle of the hydrophobic and UV-resistant microfiber leather fiber prepared in Example 1. DETAILED DESCRIPTION
[0025] A hydrophobic and UV-resistant microfiber leather, the preparation method of which comprises the following steps: (1) Adding tris(hydroxymethyl)aminomethane to deionized water to adjust the pH to 8.5, then adding dopamine hydrochloride and stirring evenly to obtain a dopamine hydrochloride solution with a mass concentration of 1% to 1.5%, then soaking synthetic leather in the dopamine hydrochloride solution for 24 hours, taking it out, washing it, and drying it to obtain a pretreated synthetic leather; (2) immersing the synthetic leather pretreated in step (1) in a zinc acetate solution, and then slowly adding a 2-methylimidazole solution at a volume ratio of zinc acetate solution to 2-methylimidazole solution of 2.5:1 (the mass ratio of zinc acetate dihydrate to 2-methylimidazole used is 1:3), stirring and mixing, and then standing for 24 hours, then taking out the synthetic leather, washing and drying, to obtain a ZIF-8 modified synthetic leather; (3) soaking the ZIF-8 modified synthetic leather obtained in step (2) in a 1.5 wt % pterostilbene ethanol solution for 30 min, taking it out, washing it, and drying it to obtain a pterostilbene modified synthetic leather; (4) Adding photoinitiator 1173 and hexadecanethiol to ethanol, and ultrasonically homogenizing to obtain a mixed solution containing 0.02 wt% of photoinitiator and 1 wt% to 2 wt% of hexadecanethiol; immersing the pterostilbene modified synthetic leather obtained in step (3) in the mixed solution, and using a 365 nm ultraviolet LED lamp (power of 500 mW·cm) under stirring at a speed of 30 r / min; −2 ) is irradiated for 30 minutes, then taken out, washed and dried to obtain the hydrophobic and UV-resistant microfiber leather.
[0026] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.
[0027] The synthetic leather used is PA6 / PU type ultrafine fiber synthetic leather.
[0028] Example 1 Step 1: Preparation of polydopamine modified synthetic leather: add 1 mmol of tris(hydroxymethyl)aminomethane to 100 mL of deionized water, adjust the pH to 8.5, and stir for 5 min; then add 0.1 g of dopamine hydrochloride and stir for 5 min; then add synthetic leather, let stand for 24 h, take out, wash with deionized water, and dry to obtain polydopamine modified synthetic leather; Step 2: Preparation of ZIF-8 modified synthetic leather: Dissolve 6 g zinc acetate dihydrate in 100 mL deionized water and stir for 5 min to obtain a zinc acetate solution; dissolve 17.95 g 2-methylimidazole in 40 mL deionized water and stir for 10 min to obtain a 2-methylimidazole solution; place polydopamine modified synthetic leather in the obtained zinc acetate solution, then slowly add the 2-methylimidazole solution, slowly stir at room temperature for 24 h, then take out, wash with deionized water, and dry to obtain ZIF-8 modified synthetic leather (Z-MSL); Step 3: Preparation of pterostilbene modified synthetic leather: 1.5 g of pterostilbene was added to 100 mL of ethanol and stirred for 10 min to obtain an ethanol solution of pterostilbene; ZIF-8 modified synthetic leather was placed in the ethanol solution of pterostilbene, allowed to stand at room temperature for 15 min, then taken out, washed with deionized water, and dried to obtain pterostilbene modified synthetic leather (PZ-MSL); Step 4: Preparation of hexadecanethiol-modified synthetic leather: 1.5 g hexadecanethiol and 0.02 g photoinitiator 1173 were added to 100 mL ethanol and ultrasonicated for 15 min to make it uniform; then the pterostilbene-modified synthetic leather was added to the mixed solution and the mixture was stirred at 30 r / min using a 365 nm UV LED lamp (power of 500 mW·cm −2 ) for 30 min, washed with deionized water and dried to obtain the hydrophobic and UV-resistant microfiber leather (SPZ-MSL).
[0029] Figure 1 , 2 They are scanning electron microscope images of the initial synthetic leather material and the hydrophobic anti-ultraviolet microfiber leather prepared in Example 1. From the figure, it can be seen that ZIF-8 is well adsorbed on the surface of the synthetic leather fiber, increasing the surface roughness of the material.
[0030] Figure 3 This is the infrared spectrum of the hydrophobic and UV-resistant microfiber leather prepared in Example 1. In the figure, 3623 cm -1 The peak at 3201 cm -1 The stretching vibration peaks of -OH and -NH groups are at 2969 cm -1 and 2925 cm -1 The peaks at 1700 cm-1 are the PZ-stretching vibration peaks of polyurethane and hexadecanethiol. -1 The peak at 1581 cm is the stretching vibration peak of amide. -1 and 1423 cm -1 The characteristic peak of benzene ring, 761cm -1 The peak at the center is the stretching vibration peak of 2-methylimidazole in ZIF-8, which indicates that the hydrophobic and UV-resistant microfiber leather was successfully synthesized.
[0031] Figure 4 , 5 They are the contact angles of the initial synthetic leather material and the hydrophobic anti-ultraviolet microfiber leather prepared in Example 1. As can be seen from the figure, the contact angle of the initial synthetic leather is 58°, while the water contact angle of the hydrophobic anti-ultraviolet microfiber leather is 155°, proving that its hydrophobicity is significantly increased.
[0032] Example 2 Step 1: Preparation of polydopamine modified synthetic leather: add 1 mmol of tris(hydroxymethyl)aminomethane to 100 mL of deionized water, adjust the pH to 8.5, and stir for 5 min; then add 0.1 g of dopamine hydrochloride and stir for 5 min; then add synthetic leather, let stand for 24 h, take out, wash with deionized water, and dry to obtain polydopamine modified synthetic leather; Step 2: Preparation of ZIF-8 modified synthetic leather: Dissolve 6 g zinc acetate dihydrate in 100 mL deionized water and stir for 5 min to obtain a zinc acetate solution; dissolve 17.95 g 2-methylimidazole in 40 mL deionized water and stir for 10 min to obtain a 2-methylimidazole solution; place polydopamine modified synthetic leather in the obtained zinc acetate solution, then slowly add the 2-methylimidazole solution, slowly stir at room temperature for 24 h, then take out, wash with deionized water, and dry to obtain ZIF-8 modified synthetic leather (Z-MSL); Step 3: Preparation of pterostilbene modified synthetic leather: 1.5 g of pterostilbene was added to 100 mL of ethanol and stirred for 10 min to obtain an ethanol solution of pterostilbene; ZIF-8 modified synthetic leather was placed in the ethanol solution of pterostilbene, allowed to stand at room temperature for 15 min, then taken out, washed with deionized water, and dried to obtain pterostilbene modified synthetic leather (PZ-MSL); Step 4: Preparation of hexadecanethiol-modified synthetic leather: 1.0 g hexadecanethiol and 0.02 g photoinitiator 1173 were added to 100 mL ethanol and ultrasonicated for 15 min to make it uniform; then the pterostilbene-modified synthetic leather was added to the mixed solution and the mixture was stirred at 30 r / min using a 365 nm UV LED lamp (power of 500 mW·cm −2 ) for 30 min, washed with deionized water and dried to obtain the hydrophobic and UV-resistant microfiber leather (SPZ-MSL).
[0033] Example 3 Step 1: Preparation of polydopamine modified synthetic leather: add 1 mmol of tris(hydroxymethyl)aminomethane to 100 mL of deionized water, adjust the pH to 8.5, and stir for 5 min; then add 0.1 g of dopamine hydrochloride and stir for 5 min; then add synthetic leather, let stand for 24 h, take out, wash with deionized water, and dry to obtain polydopamine modified synthetic leather; Step 2: Preparation of ZIF-8 modified synthetic leather: Dissolve 6 g zinc acetate dihydrate in 100 mL deionized water and stir for 5 min to obtain a zinc acetate solution; dissolve 17.95 g 2-methylimidazole in 40 mL deionized water and stir for 10 min to obtain a 2-methylimidazole solution; place polydopamine modified synthetic leather in the obtained zinc acetate solution, then slowly add the 2-methylimidazole solution, slowly stir at room temperature for 24 h, then take out, wash with deionized water, and dry to obtain ZIF-8 modified synthetic leather (Z-MSL); Step 3: Preparation of pterostilbene modified synthetic leather: 1.5 g of pterostilbene was added to 100 mL of ethanol and stirred for 10 min to obtain an ethanol solution of pterostilbene; ZIF-8 modified synthetic leather was placed in the ethanol solution of pterostilbene, allowed to stand at room temperature for 15 min, then taken out, washed with deionized water, and dried to obtain pterostilbene modified synthetic leather (PZ-MSL); Step 4: Preparation of hexadecanethiol-modified synthetic leather: 2.0 g hexadecanethiol and 0.02 g photoinitiator 1173 were added to 100 mL ethanol and ultrasonicated for 15 min to make it uniform; then the pterostilbene-modified synthetic leather was added to the mixed solution and the mixture was stirred at 30 r / min using a 365 nm UV LED lamp (power of 500 mW·cm −2 ) for 30 min, washed with deionized water and dried to obtain the hydrophobic and UV-resistant microfiber leather (SPZ-MSL).
[0034] Comparative Example 1 (microfiber leather with only ZIF-8 attached) Step 1: Preparation of polydopamine modified synthetic leather: add 1 mmol of tris(hydroxymethyl)aminomethane to 100 mL of deionized water, adjust the pH to 8.5, and stir for 5 min; then add 0.1 g of dopamine hydrochloride and stir for 5 min; then add synthetic leather, let stand for 24 h, take out, wash with deionized water, and dry to obtain polydopamine modified synthetic leather; Step 2: Preparation of ZIF-8 modified synthetic leather: Dissolve 6 g of zinc acetate dihydrate in 100 mL of deionized water and stir for 5 min to obtain a zinc acetate solution; dissolve 17.95 g of 2-methylimidazole in 40 mL of deionized water and stir for 10 min to obtain a 2-methylimidazole solution; place the polydopamine modified synthetic leather in the obtained zinc acetate solution, then slowly add the 2-methylimidazole solution, slowly stir at room temperature for 24 h, then take out, wash with deionized water, and dry to obtain ZIF-8 modified synthetic leather (Z-MSL).
[0035] Comparative Example 2 (ZIF-8 modified microfiber leather coated with pterostilbene) Preparation of polydopamine modified synthetic leather: 1 mmol of tris(hydroxymethyl)aminomethane was added to 100 mL of deionized water, the pH was adjusted to 8.5, and stirred for 5 min; then 0.1 g of dopamine hydrochloride was added and stirred for 5 min; then synthetic leather was added, and the mixture was taken out after standing for 24 h, washed with deionized water, and dried to obtain polydopamine modified synthetic leather; Step 2: Preparation of ZIF-8 modified synthetic leather: Dissolve 6 g zinc acetate dihydrate in 100 mL deionized water and stir for 5 min to obtain a zinc acetate solution; dissolve 17.95 g 2-methylimidazole in 40 mL deionized water and stir for 10 min to obtain a 2-methylimidazole solution; place polydopamine modified synthetic leather in the obtained zinc acetate solution, then slowly add the 2-methylimidazole solution, slowly stir at room temperature for 24 h, then take out, wash with deionized water, and dry to obtain ZIF-8 modified synthetic leather (Z-MSL); Step 3: Preparation of pterostilbene modified synthetic leather: Add 1.5 g of pterostilbene into 100 mL of ethanol and stir for 10 min to obtain an ethanol solution of pterostilbene; place the ZIF-8 modified synthetic leather in the ethanol solution of pterostilbene, let it stand at room temperature for 15 min, then take it out, wash it with deionized water, and dry it to obtain pterostilbene modified synthetic leather (PZ-MSL).
[0036] Comparative Example 3 (microfiber leather without pterostilbene modification) Step 1: Preparation of polydopamine modified synthetic leather: add 1 mmol of tris(hydroxymethyl)aminomethane to 100 mL of deionized water, adjust the pH to 8.5, and stir for 5 min; then add 0.1 g of dopamine hydrochloride and stir for 5 min; then add synthetic leather, let stand for 24 h, take out, wash with deionized water, and dry to obtain polydopamine modified synthetic leather; Step 2: Preparation of ZIF-8 modified synthetic leather: Dissolve 6 g zinc acetate dihydrate in 100 mL deionized water and stir for 5 min to obtain a zinc acetate solution; dissolve 17.95 g 2-methylimidazole in 40 mL deionized water and stir for 10 min to obtain a 2-methylimidazole solution; place polydopamine modified synthetic leather in the obtained zinc acetate solution, then slowly add the 2-methylimidazole solution, slowly stir at room temperature for 24 h, then take out, wash with deionized water, and dry to obtain ZIF-8 modified synthetic leather (Z-MSL); Step 3: Preparation of hexadecanethiol-modified synthetic leather: 1.5 g hexadecanethiol and 0.02 g photoinitiator 1173 were added to 100 mL ethanol and ultrasonicated for 15 min to make it uniform; then the ZIF-8-modified synthetic leather obtained in step 2 was added to the mixed solution, and a 365 nm ultraviolet LED lamp (power of 500 mW·cm) was used under stirring at a speed of 30 r / min. −2 ) for 30 min, washed with deionized water and dried to obtain the hydrophobic and UV-resistant microfiber leather (ZH-MSL).
[0037] Comparative Example 4 (Resveratrol-modified hydrophobic anti-ultraviolet microfiber leather) Step 1: Preparation of polydopamine modified synthetic leather: add 1 mmol of tris(hydroxymethyl)aminomethane to 100 mL of deionized water, adjust the pH to 8.5, and stir for 5 min; then add 0.1 g of dopamine hydrochloride and stir for 5 min; then add synthetic leather, let stand for 24 h, take out, wash with deionized water, and dry to obtain polydopamine modified synthetic leather; Step 2: Preparation of ZIF-8 modified synthetic leather: Dissolve 6 g zinc acetate dihydrate in 100 mL deionized water and stir for 5 min to obtain a zinc acetate solution; dissolve 17.95 g 2-methylimidazole in 40 mL deionized water and stir for 10 min to obtain a 2-methylimidazole solution; place polydopamine modified synthetic leather in the obtained zinc acetate solution, then slowly add the 2-methylimidazole solution, slowly stir at room temperature for 24 h, then take out, wash with deionized water, and dry to obtain ZIF-8 modified synthetic leather (Z-MSL); Step 3: Preparation of resveratrol-modified synthetic leather: 1.5 g of resveratrol was added to 100 mL of ethanol and stirred for 10 min to obtain an ethanol solution of resveratrol; ZIF-8-modified synthetic leather was placed in the ethanol solution of resveratrol, allowed to stand at room temperature for 15 min, then taken out, washed with deionized water, and dried to obtain resveratrol-modified synthetic leather (PZ-MSL); Step 4: Preparation of hexadecanethiol-modified synthetic leather: 1.5 g hexadecanethiol and 0.02 g photoinitiator 1173 were added to 100 mL ethanol and ultrasonicated for 15 min to make it uniform; then resveratrol-modified synthetic leather was added to the mixed solution and the mixture was stirred at 30 r / min using a 365 nm UV LED lamp (power of 500 mW·cm −2 ) for 30 min, washed with deionized water and dried to obtain the hydrophobic and UV-resistant microfiber leather (SPZ-MSL).
[0038] Comparative Example 5 (2,4-hydroxycinnamic acid modified hydrophobic anti-ultraviolet microfiber leather) Step 1: Preparation of polydopamine modified synthetic leather: add 1 mmol of tris(hydroxymethyl)aminomethane to 100 mL of deionized water, adjust the pH to 8.5, and stir for 5 min; then add 0.1 g of dopamine hydrochloride and stir for 5 min; then add synthetic leather, let stand for 24 h, take out, wash with deionized water, and dry to obtain polydopamine modified synthetic leather; Step 2: Preparation of ZIF-8 modified synthetic leather: Dissolve 6 g zinc acetate dihydrate in 100 mL deionized water and stir for 5 min to obtain a zinc acetate solution; dissolve 17.95 g 2-methylimidazole in 40 mL deionized water and stir for 10 min to obtain a 2-methylimidazole solution; place polydopamine modified synthetic leather in the obtained zinc acetate solution, then slowly add the 2-methylimidazole solution, slowly stir at room temperature for 24 h, then take out, wash with deionized water, and dry to obtain ZIF-8 modified synthetic leather (Z-MSL); Step 3: Preparation of 2,4-hydroxycinnamic acid modified synthetic leather: 1.5 g of 2,4-hydroxycinnamic acid was added to 100 mL of ethanol and stirred for 10 min to obtain an ethanol solution of 2,4-hydroxycinnamic acid; ZIF-8 modified synthetic leather was placed in the ethanol solution of 2,4-hydroxycinnamic acid, allowed to stand at room temperature for 15 min, then taken out, washed with deionized water, and dried to obtain 2,4-hydroxycinnamic acid modified synthetic leather (PZ-MSL); Step 4: Preparation of hexadecanethiol-modified synthetic leather: 1.5 g hexadecanethiol and 0.02 g photoinitiator 1173 were added to 100 mL ethanol and ultrasonicated for 15 min to make it uniform; then 2,4-hydroxycinnamic acid-modified synthetic leather was added to the mixed solution and the mixture was stirred at 30 r / min using a 365 nm UV LED lamp (power of 500 mW·cm −2 ) for 30 min, washed with deionized water and dried to obtain the hydrophobic and UV-resistant microfiber leather (SPZ-MSL).
[0039] Comparative Example 6 (Curcumin-modified hydrophobic anti-ultraviolet microfiber leather) Step 1: Preparation of polydopamine modified synthetic leather: add 1 mmol of tris(hydroxymethyl)aminomethane to 100 mL of deionized water, adjust the pH to 8.5, and stir for 5 min; then add 0.1 g of dopamine hydrochloride and stir for 5 min; then add synthetic leather, let stand for 24 h, take out, wash with deionized water, and dry to obtain polydopamine modified synthetic leather; Step 2: Preparation of ZIF-8 modified synthetic leather: Dissolve 6 g zinc acetate dihydrate in 100 mL deionized water and stir for 5 min to obtain a zinc acetate solution; dissolve 17.95 g 2-methylimidazole in 40 mL deionized water and stir for 10 min to obtain a 2-methylimidazole solution; place polydopamine modified synthetic leather in the obtained zinc acetate solution, then slowly add the 2-methylimidazole solution, slowly stir at room temperature for 24 h, then take out, wash with deionized water, and dry to obtain ZIF-8 modified synthetic leather (Z-MSL); Step 3: Preparation of curcumin-modified synthetic leather: 1.5 g of curcumin was added to 100 mL of ethanol and stirred for 10 min to obtain an ethanol solution of curcumin; ZIF-8-modified synthetic leather was placed in the ethanol solution of curcumin, allowed to stand at room temperature for 15 min, then taken out, washed with deionized water, and dried to obtain curcumin-modified synthetic leather (PZ-MSL); Step 4: Preparation of hexadecanethiol-modified synthetic leather: 1.5 g hexadecanethiol and 0.02 g photoinitiator 1173 were added to 100 mL ethanol and ultrasonicated for 15 min to make it uniform; then curcumin-modified synthetic leather was added to the mixed solution and the mixture was stirred at 30 r / min using a 365 nm UV LED lamp (power of 500 mW·cm −2 ) for 30 min, washed with deionized water and dried to obtain the hydrophobic and UV-resistant microfiber leather (SPZ-MSL).
[0040] 1. Coating stability test Wear stability test: Place the synthetic leather to be tested on 1000-grit sandpaper, and then place a 100-g weight on it. Use external force to move the sample 10 cm on the sandpaper. One back-and-forth movement is one cycle, and each cycle is recorded as one wear test. A total of 30 wears are performed. After washing and drying, the contact angle of the sample is tested using a contact angle meter.
[0041] Washing stability test: Place the sample in a soap solution and wash for 45 min, with a washing speed of 40 r / min and a washing temperature of 40°C. The mass ratio of the sample to the mass of the washing liquid is 1:50. Wash it with water, dry it, and then use a contact angle meter to test the contact angle of the sample.
[0042] Acid, alkali and salt solution resistance test: The synthetic leather to be tested is immersed in acidic solution (pH=1, 3, 5), alkaline solution (pH=9, 11, 13) and salt solution (3.5 wt% NaCl solution) for 24 h. After immersion, it is washed and dried, and the contact angle of the sample is tested using a contact angle meter.
[0043] Table 1 Coating stability test results
[0044] As can be seen from Table 1, the hydrophobic anti-ultraviolet ultra-fine leather prepared in the embodiment still retains the ability of super-hydrophobicity after the wear test and the washing test, and except that low pH and high pH have a certain influence on the material, its hydrophobic performance is basically stable and can meet the general use environment. And it can be found from the comparative example that the synthetic leather modified by only ZIF-8 (Comparative Example 1) or modified by pterostilbene coating (Comparative Example 2) does not have hydrophobicity, and the hydrophobic performance of the hexamercaptan modified synthetic leather (Comparative Example 3) without pterostilbene modification is slightly improved, but because the hexamercaptan is simply attached to the surface of the synthetic leather, the firmness is insufficient. The hydrophobic anti-ultraviolet ultra-fine leather prepared by modification with other phenolic compounds (Comparative Examples 4-6) is not as good as the hydrophobic anti-ultraviolet ultra-fine leather prepared by coating with pterostilbene.
[0045] 2. Synthetic leather anti-ultraviolet performance test The anti-ultraviolet properties of different synthetic leather samples were tested using a textile anti-ultraviolet performance tester.
[0046] Table 2 Ultraviolet (UV) protection test results
[0047] As can be seen from Table 2, when the amount of hexadecyl mercaptan is greater than 1.5g, the obtained hydrophobic anti-ultraviolet ultraviolet leather (Example 1 and Example 3) has the best ultraviolet protection performance. At the same time, by comparing with the comparative example, it can be seen that the synthetic leather modified with only ZIF-8 (Comparative Example 1) or only introducing a long alkane chain (Comparative Example 3) basically has no anti-ultraviolet performance; after being coated with pterostilbene (Comparative Example 2), the anti-ultraviolet performance of the modified synthetic leather is significantly improved. This is because the methoxy, phenolic hydroxyl and conjugated unsaturated CC structure contained in pterostilbene enable it to absorb free radicals generated by ultraviolet radiation, reduce oxidative stress, reflect and absorb part of the ultraviolet rays, thereby effectively increasing the ultraviolet protection ability of the material. In addition, the anti-ultraviolet performance of the hydrophobic anti-ultraviolet ultraviolet leather prepared by replacing pterostilbene with resveratrol, 2,4-hydroxycinnamic acid and curcumin is not as good as that of pterostilbene. This may be because the benzene ring and specific methylated groups in the molecular structure of pterostilbene enable it to absorb and disperse ultraviolet energy more effectively and resist the invasion of ultraviolet rays.
[0048] From the above data, it can be seen that the hydrophobic anti-UV microfiber leather prepared by thiol-ene reaction of pterostilbene and hexadecyl mercaptan has better anti-UV performance.
[0049] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A method for preparing a hydrophobic and UV-resistant microfiber leather, characterized in that: The following steps are involved: (1) After adding tris(hydroxymethyl)aminomethane to deionized water to adjust the pH, dopamine hydrochloride is added and stirred evenly, and then synthetic leather is immersed in the dopamine hydrochloride solution, taken out, washed, and dried to obtain pretreated synthetic leather; (2) immersing the synthetic leather pretreated in step (1) in a zinc acetate solution, then slowly adding a 2-methylimidazole solution, stirring and mixing, and then allowing to stand. Then, the synthetic leather is taken out, washed, and dried to obtain a ZIF-8 modified synthetic leather; (3) soaking the ZIF-8 modified synthetic leather obtained in step (2) in an ethanol solution of pterostilbene, taking it out, washing it, and drying it to obtain a pterostilbene modified synthetic leather; (4) Add photoinitiator 1173 and hexadecanethiol to ethanol, ultrasonically homogenize, and then immerse the pterostilbene-modified synthetic leather obtained in step (3) in the mixed solution, irradiate with an ultraviolet lamp under stirring conditions, then take out, wash, and dry to obtain the hydrophobic and ultraviolet-resistant microfiber leather.
2. The method for preparing the hydrophobic anti-ultraviolet microfiber leather according to claim 1, wherein In step (1), tris(hydroxymethyl)aminomethane was added to adjust the pH to 8.
5.
3. The method for preparing the hydrophobic anti-ultraviolet microfiber leather according to claim 1, wherein The synthetic leather described in step (1) is specifically PA6 / PU type microfiber synthetic leather.
4. The method for preparing the hydrophobic anti-ultraviolet microfiber leather according to claim 1, wherein The mass concentration of the dopamine hydrochloride solution in step (1) is 1% to 1.5%; the soaking time is 24 hours.
5. The method for preparing the hydrophobic and UV-resistant microfiber leather according to claim 1, wherein: The volume ratio of the zinc acetate solution to the 2-methylimidazole solution used in step (2) is 2.5:1, wherein the mass ratio of the zinc acetate dihydrate to the 2-methylimidazole used is 1:
3.
6. The method for preparing the hydrophobic and UV-resistant microfiber leather according to claim 1, wherein: The standing time in step (2) is 24 hours.
7. The method for preparing the hydrophobic and UV-resistant microfiber leather according to claim 1, wherein: The mass concentration of the pterostilbene ethanol solution in step (3) is 1.5%; the soaking time is 30 minutes.
8. The method for preparing the hydrophobic and UV-resistant microfiber leather according to claim 1, wherein: The mass concentration of the photoinitiator in the mixed solution of step (4) is 0.02%, and the mass concentration of hexadecanethiol is 1% to 2%.
9. The method for preparing the hydrophobic anti-ultraviolet microfiber leather according to claim 1, wherein The stirring speed in step (4) is 30 r / min; the UV lamp used is a 365 nm UV LED lamp with an irradiation power of 500 mW·cm −2 , the irradiation time is 30 min.
10. A hydrophobic, UV-resistant microfiber leather prepared by the method according to any one of claims 1 to 9.