Heterogeneous material joint and intermediate layer design method of heterogeneous material joint
By designing a multi-layer composite intermediate layer in the heterogeneous material joint, and using finite element analysis and machine learning to optimize the material proportions, the thermal expansion coefficient gradient transition is realized, which solves the problem of high thermal stress in the heterogeneous material joint and improves the connection strength.
Patent Information
- Application Number
- CN202410838813.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-11
AI Technical Summary
Due to the difference in elastic modulus and thermal expansion coefficient of heterogeneous material joints, the connection performance is low, and the thermal stress reaches hundreds of megapascals, weakening the connection strength.
The middle layer design method of heterogeneous material joints is adopted, and the proportion of materials corresponding to the minimum thermal stress is determined through finite element analysis and machine learning. The multi-layer composite middle layer is designed to achieve a gradient transition of thermal expansion coefficient and reduce thermal stress.
It effectively reduces the thermal stress of heterogeneous material joints, improves the connection performance, enables the thermal expansion coefficient and other physical properties at the joint to complete a gradient transition, and coordinates deformation, thus improving the connection strength under thermal load.
Smart Images

Figure CN118761267A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite material structure design and optimization, and in particular to a heterogeneous material joint and an intermediate layer design method of the heterogeneous material joint. Background Art
[0002] Due to the differences in elastic modulus and thermal expansion coefficient, the joints of heterogeneous materials often show low connection performance. When the heterogeneous material joints are subjected to thermal loads, the performance difference between the two phase materials at the joint interface will lead to large deformation inconsistency, and then generate large thermal stress, which can reach hundreds of megapascals. This phenomenon greatly weakens the connection strength of heterogeneous material joints under thermal loads. Summary of the invention
[0003] In view of the above problems existing in the prior art, the present invention provides a heterogeneous material joint and an intermediate layer design method of the heterogeneous material joint to improve the connection performance of the heterogeneous material joint.
[0004] The specific content of the invention is as follows:
[0005] In a first aspect, the present invention provides a method for designing an intermediate layer of a heterogeneous material joint, wherein the heterogeneous material joint comprises a first component layer, an intermediate layer and a second component layer stacked in a thickness direction, wherein the intermediate layer is a multilayer composite material phase formed by the first component and the second component, and the method comprises:
[0006] Based on finite element analysis, the thermal stress distribution of the heterogeneous material joint is calculated;
[0007] Based on machine learning, determining the proportion of the first component or the second component corresponding to the minimum thermal stress in the thermal stress distribution in each layer of the composite material phase;
[0008] The thermal stress includes the von-Mises stress σ v , maximum principal stress σ m , transverse normal stress σ x , longitudinal normal stress σ y or shear stress τ xy .
[0009] Optionally, the calculating, based on finite element analysis, the thermal stress distribution of the heterogeneous material joint comprises:
[0010] Performing geometric modeling on the heterogeneous material joint to obtain a geometric model;
[0011] Based on the geometric model, meshing is performed on each region of the heterogeneous material joint, and the proportion of the first component or the second component in each layer of the composite material phase constituting the intermediate layer is set as a boundary condition and a load condition to obtain a finite element thermal stress calculation program;
[0012] Under the condition that only the proportion of the first component or the second component in each layer of the composite material phase constituting the intermediate layer is changed, the thermal stress distribution of the heterogeneous material joint is calculated by the finite element thermal stress calculation program;
[0013] The load condition is that the heterogeneous material joint is heated by 180K from a zero stress state.
[0014] Optionally, determining the proportion of the first component or the second component corresponding to the minimum thermal stress in the thermal stress distribution in each layer of the composite material based on machine learning includes:
[0015] Initializing the proportion of the first component or the second component in each layer of the composite material phase to 0.5, and obtaining the thermal stress peak value of the heterogeneous material joint according to the finite element analysis result;
[0016] By using a machine learning algorithm, the proportion of the first component or the second component in each layer of the composite material is iteratively changed to obtain the proportion of the first component or the second component in each layer of the composite material and the minimum stress value when the thermal stress peak is minimum.
[0017] Optionally, the machine learning algorithm is a genetic algorithm; the machine learning algorithm is used to iteratively change the proportion of the first component or the second component in each layer of the composite material to obtain the proportion of the first component or the second component in each layer of the composite material when the thermal stress peak is minimum, and the minimum stress value, including:
[0018] Set the population size to 20, the crossover rate to 0.5, the elite individual to 2, and each individual in the initial population to 0.5, so that the proportion of the first component or the second component in each layer of the composite material is initialized to 0.5;
[0019] Starting from the initial population, calculate the peak value of thermal stress of each individual in the population and evaluate its fitness function;
[0020] According to the evaluation results, the genetic operator is applied to generate the next generation, and the selection operator is used to select individuals with small peak heat stress in the population;
[0021] The crossover operator is used to combine the information of different individuals to combine the material component values between different individuals;
[0022] Use mutation operators to generate other new individuals to explore the global optimal solution;
[0023] Determine whether the termination condition is met, and if so, obtain the proportion of the first component or the second component in each layer of the composite material when the thermal stress peak is minimum, and the minimum stress value;
[0024] If not reached, the operation is repeated for the next generation population until the thermal stress peak is minimized, and the proportion of the first component or the second component in each layer of the composite material and the minimum stress value are achieved.
[0025] Optionally, the first component is high-strength aluminum, the second component is aluminum-based silicon carbide; the intermediate layer is composed of a first composite material phase, a second composite material phase, a third composite material phase and a fourth composite material phase stacked in layers;
[0026] In the intermediate layer, the proportion of the aluminum-based silicon carbide or high-strength aluminum is, and the von-Mises stress σ of the heterogeneous material joint is v The proportion of the aluminum-based silicon carbide or high-strength aluminum in each layer of the composite material is the minimum; in the first composite material phase, the proportion of the aluminum-based silicon carbide is 21%; in the second composite material phase, the proportion of the aluminum-based silicon carbide is 38%; in the third composite material phase, the proportion of the aluminum-based silicon carbide is 57%; in the fourth composite material phase, the proportion of the aluminum-based silicon carbide is 85%.
[0027] Optionally, the first component is high-strength aluminum, the second component is aluminum-based silicon carbide, and the intermediate layer is composed of a first composite material phase, a second composite material phase, a third composite material phase, and a fourth composite material phase that are stacked;
[0028] In the intermediate layer, the proportion of the aluminum-based silicon carbide or high-strength aluminum is, and the maximum principal stress σ of the heterogeneous material joint is m The proportion of the aluminum-based silicon carbide or high-strength aluminum in each layer of the composite material is minimum; in the first composite material phase, the proportion of the aluminum-based silicon carbide is 40%; in the second composite material phase, the proportion of the aluminum-based silicon carbide is 25%; in the third composite material phase, the proportion of the aluminum-based silicon carbide is 28%; in the fourth composite material phase, the proportion of the aluminum-based silicon carbide is 47%.
[0029] Optionally, the first component is high-strength aluminum, the second component is aluminum-based silicon carbide, and the intermediate layer is composed of a first composite material phase, a second composite material phase, a third composite material phase, and a fourth composite material phase that are stacked;
[0030] In the intermediate layer, the proportion of the aluminum-based silicon carbide or high-strength aluminum is, and the transverse normal stress σ of the heterogeneous material joint x The proportion of the aluminum-based silicon carbide or high-strength aluminum in each layer of the composite material is the minimum; in the first composite material phase, the proportion of the aluminum-based silicon carbide is 15%; in the second composite material phase, the proportion of the aluminum-based silicon carbide is 15%; in the third composite material phase, the proportion of the aluminum-based silicon carbide is 28%; in the fourth composite material phase, the proportion of the aluminum-based silicon carbide is 39%.
[0031] Optionally, the first component is high-strength aluminum, the second component is aluminum-based silicon carbide, and the intermediate layer is composed of a first composite material phase, a second composite material phase, a third composite material phase, and a fourth composite material phase that are stacked;
[0032] In the intermediate layer, the proportion of the aluminum-based silicon carbide or high-strength aluminum is, and the longitudinal normal stress σ of the heterogeneous material joint y The proportion of the aluminum-based silicon carbide or high-strength aluminum in each layer of the composite material is minimum; in the first composite material phase, the proportion of the aluminum-based silicon carbide is 75%; in the second composite material phase, the proportion of the aluminum-based silicon carbide is 75%; in the third composite material phase, the proportion of the aluminum-based silicon carbide is 83%; in the fourth composite material phase, the proportion of the aluminum-based silicon carbide is 56%.
[0033] Optionally, the first component is high-strength aluminum, the second component is aluminum-based silicon carbide, and the intermediate layer is composed of a first composite material phase, a second composite material phase, a third composite material phase, and a fourth composite material phase that are stacked;
[0034] In the intermediate layer, the proportion of the aluminum-based silicon carbide or high-strength aluminum is, and the shear stress τ of the heterogeneous material joint xy The proportion of the aluminum-based silicon carbide or high-strength aluminum in each layer of the composite material is the minimum; in the first composite material phase, the proportion of the aluminum-based silicon carbide is 32%; in the second composite material phase, the proportion of the aluminum-based silicon carbide is 52%; in the third composite material phase, the proportion of the aluminum-based silicon carbide is 47%; in the fourth composite material phase, the proportion of the aluminum-based silicon carbide is 69%.
[0035] In a second aspect, the present invention provides a heterogeneous material joint obtained by the design method described in the first aspect.
[0036] Compared with the prior art, the present invention has the following advantages:
[0037] The heterogeneous material joint provided by the present invention includes a first component layer, an intermediate layer and a second component layer stacked in the thickness direction, the intermediate layer is a multilayer composite material formed by the first component and the second component, and the method includes: calculating the thermal stress distribution of the heterogeneous material joint based on finite element analysis; based on machine learning, determining the proportion of the first component or the second component corresponding to the minimum thermal stress in the thermal stress set in each layer of the composite material.
[0038] The design method of heterogeneous material joints proposed in the present invention designs the number of layers of the intermediate layer and the distribution of material components so that aluminum-based silicon carbide or high-strength aluminum is non-uniformly distributed in the intermediate layer. The thermal expansion coefficient of the intermediate layer has a gradient transition at the interface of the heterogeneous materials (along the thickness direction of the interface), thereby achieving the lowest thermal stress in the heterogeneous material joint. The gradient intermediate layer is prepared with the help of the composite material manufacturing process, which is universal for different types of heterogeneous joints. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0040] Figure 1 A flow chart of a method for designing an intermediate layer of a heterogeneous material joint provided by an embodiment of the present invention is shown;
[0041] Figure 2 A schematic diagram of the composition of a heterogeneous material joint is shown;
[0042] Figure 3 A finite element geometric modeling grid diagram provided by an embodiment of the present invention is shown;
[0043] Figure 4 The embodiment of the present invention provides a method based on shear stress τ xy Finite element analysis stress cloud diagram;
[0044] Figure 5 The thermal stress of the heterogeneous material joint provided by the embodiment of the present invention after the temperature is increased by 180K under zero stress state is shown;
[0045] Figure 6 A flow chart showing the genetic algorithm for calculating the optimal component provided by an embodiment of the present invention is shown;
[0046] Figure 7 The optimized thermal stress optimization result of the gradient intermediate layer joint provided by the embodiment of the present invention is shown. DETAILED DESCRIPTION
[0047] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means a limitation on the present invention and its application or use. Based on the embodiments of the present invention, any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts falls within the scope of protection of the present invention. In addition, all other embodiments obtained by ordinary technicians in this field without carrying out creative work belong to the scope of protection of the present invention.
[0048] In the embodiment, no specific experimental steps or conditions are indicated, and the operation or conditions of the conventional experimental steps described in the prior art in this field can be carried out. The reagents used and other instruments that do not indicate the manufacturer are conventional reagent products that can be obtained commercially. In addition, the accompanying drawings are only schematic diagrams of the embodiments of the present invention and are not necessarily drawn to scale. The same reference numerals in the figures represent the same or similar parts, and thus their repeated description will be omitted. Some block diagrams shown in the accompanying drawings are functional entities and do not necessarily correspond to physically or logically independent entities.
[0049] Technologies, methods, and equipment known to ordinary technicians in the relevant field may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the description of the present invention.
[0050] In the description of the present invention, it should be understood that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.
[0051] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0052] Due to the differences in elastic modulus and thermal expansion coefficient, the joints of heterogeneous materials often show low connection performance. When the heterogeneous material joints are subjected to thermal loads, the performance difference between the two phase materials at the joint interface will lead to large deformation inconsistency, and then generate large thermal stress, which can reach hundreds of megapascals. This phenomenon greatly weakens the connection strength of heterogeneous material joints under thermal loads.
[0053] In current engineering practice, two methods are generally used to reduce thermal stress at material joints. The first is to set a buffer layer at the joint. The buffer layer generally has greater flexibility and can coordinate the thermal expansion and deformation of heterogeneous materials to reduce structural thermal stress. However, this method is often based on specific engineering practice and is a design that relies on experience. Moreover, the material configuration and morphology design of this buffer layer depends on the material, shape, load, etc. of the joint, and generally there is no universal design specification.
[0054] The second method is to use the heterogeneous materials that make up the joint to make a composite material phase as the interface middle layer of the joint material, thereby reducing the thermal stress of the joint. Therefore, the present invention hopes to optimize the setting of the middle layer on the basis of the existing second method, and perform a multi-layer composite material middle layer setting to obtain a heterogeneous material joint with minimized thermal stress, so that the physical properties such as the thermal expansion coefficient at the joint complete the gradient transition and the thermal deformation is coordinated. The following is a detailed description of some embodiments and their application scenarios in conjunction with the accompanying drawings, and the specific implementation methods are as follows:
[0055] The present invention provides a method for designing an intermediate layer of a heterogeneous material joint. Figure 1 The flowchart of the design method of the heterogeneous material joint provided by the embodiment of the present invention is shown to obtain the heterogeneous material joint with minimized thermal stress, such as Figure 1 As shown in the figure, the design method flow specifically includes:
[0056] S1. Calculate the thermal stress distribution of the heterogeneous material joint based on finite element analysis;
[0057] In specific implementation, the embodiment of the present invention is Figure 2 Taking the schematic diagram of the composition of a heterogeneous material joint as an example, the intermediate layer design method of the heterogeneous material joint is illustrated:
[0058] like Figure 2 As shown in FIG. 1 , the heterogeneous material joint includes a high-strength aluminum layer 1 (material A), an intermediate layer 2, and an aluminum-based silicon carbide layer 3 (material B) stacked in the thickness direction. Since the elastic modulus E of the high-strength aluminum is 70 GPa and the thermal expansion coefficient α is 23.2×10 - 6 K -1 ; The elastic modulus E of aluminum-based silicon carbide is 70GPa, and the thermal expansion coefficient is 6.5×10 -6 K -1 The thermal expansion coefficients of high-strength aluminum and aluminum-based silicon carbide are very different. The middle layer 2 is a composite material formed by high-strength aluminum and aluminum-based silicon carbide; and Figure 1 The intermediate layer 2 shown is composed of 4 layers along the interface thickness direction ( Figure 2The composite material is composed of a stacked arrangement of layers (in the y-axis direction shown); the total thickness is h, the thickness of each layer is h / 4, and they are the first composite material phase 2-1, the second composite material phase 2-2, the third composite material phase 2-3 and the fourth composite material phase 2-4 respectively; the thermal expansion coefficient α of the middle layer 2 is regulated by regulating the ratio of the two materials of high-strength aluminum and aluminum-based silicon carbide in the middle layer 2; the proportion ρ of aluminum-based silicon carbide in the high-strength aluminum layer 1, the middle layer 2 and the aluminum-based silicon carbide layer 3 is used to distinguish the components of the material (0≤ρ≤1), then in the high-strength aluminum layer 1, ρ A =0, thermal expansion coefficient is α A ; In the aluminum-based silicon carbide layer 3, ρ B =1, thermal expansion coefficient is α B If the proportion of aluminum-based silicon carbide in the first composite material phase 2-1 is ρ1, the proportion of aluminum-based silicon carbide in the second composite material phase 2-2 is ρ2, the proportion of aluminum-based silicon carbide in the third composite material phase 2-3 is ρ3, and the proportion of aluminum-based silicon carbide in the fourth composite material phase 2-4 is ρ4, the corresponding thermal expansion coefficients are α1, α2, α3, and α4 respectively; then the thermal expansion coefficient α i =(1-ρ i )α A +ρ i α B It can be seen that by adjusting ρ1, ρ2, ρ3, and ρ4, the thermal expansion coefficient of the joint is made to transition gradually at the interface of heterogeneous materials. When the structure is subjected to thermal load, the thermal displacement and deformation of the middle layer 2 are coordinated, thereby reducing thermal stress.
[0059] The embodiment of the present invention uses finite element analysis to analyze the thermal stress generated by heating the heterogeneous material joint from a zero stress state to 180K, and obtains the thermal stress distribution of the heterogeneous material joint. The thermal stress includes the von Mises stress σ v , maximum principal stress σ m , transverse normal stress σ x , longitudinal normal stress σ y or shear stress τ xy ;
[0060] In the embodiment of the present invention, a finite element thermal stress calculation program is written with the help of MATLAB software, and a finite element mesh is established. Figure 3 FIG. 4 shows a finite element geometric modeling grid diagram provided by an embodiment of the present invention, such as Figure 3 As shown, the embodiment of the present invention establishes a finite element mesh of 200*300mm, adopts plane stress 4-node square unit (unit side length is 1mm), and adopts reduced integration. In geometric modeling, the middle layer adopts h=40mm. On both sides of the middle layer, the components ρ of aluminum-based silicon carbide are 0 and 1 respectively, representing a high-strength aluminum layer (ρ A ) and aluminum-based silicon carbide layer (ρ B). In the middle layer (h), the components ρ1, ρ2, ρ3, and ρ4 are between 0 and 1.
[0061] The embodiment of the present invention minimizes the peak value of thermal stress in the joint by adjusting ρ1, ρ2, ρ3, and ρ4. The peak value of thermal stress is obtained by finite element calculation, that is, σ max =f(ρ1,ρ2,ρ3,ρ4), the function calculation is done by finite element. The minimization process is done by machine learning. The optimization problem is described as follows:
[0062] objective:min(σ max )
[0063]
[0064] In the above thermal stress calculation process, the finite element mesh, boundary conditions, and load conditions (temperature rise 180K) are not changed, and only the component distribution ρ1, ρ2, ρ3, ρ4 in the middle layer is changed. Different components will cause different deformations and thermal stress distributions after the structure is subjected to thermal loads. xy Taking as an example, the thermal stress distribution calculated by finite element method is given. Figure 4 The embodiment of the present invention provides a method based on shear stress τ xy Finite element analysis stress contour diagram, where a shows the shear stress τ of the joint without composite material xy Cloud diagram (ρ1=0, ρ2=0, ρ3=1, ρ4=1); b shows the shear stress τ of the uniform gradient intermediate layer joint xy Cloud diagram, uniform gradient middle layer refers to ρ1 = 0.2, ρ2 = 0.4, ρ3 = 0.6, ρ4 = 0.8; c shows the shear stress τ of the optimized gradient middle layer joint xy Cloud map; Figure 4 As shown in the figure, the stress cloud diagrams of the three joints adopt the same scale colorbar (-60, 60) MPa. The black dotted line in the cloud diagram represents the position of the middle layer. The five dotted lines divide the four composite phases, from bottom to top, they are the first composite phase, the second composite phase, the third composite phase and the fourth composite phase, and Figure 1 , 2 Correspondingly, it is obvious that the peak value of thermal stress of the optimized joint is the smallest.
[0065] Figure 5 The maximum thermal stress of the heterogeneous material joint provided by the embodiment of the present invention after heating to 180K under zero stress state is shown. The three types of joints are a joint without composite materials, a uniform gradient intermediate layer joint, and an optimized gradient intermediate layer joint. Each stress is normalized using the stress value of the intermediate layer joint without composite materials, such as Figure 5As shown in Figure 2, even if the maximum value of the five thermal stresses obtained by finite element analysis is taken, it is still not greater than the thermal stress value of the uniform gradient intermediate layer joint. v As an example, the von Mises stress σ of the three joints v The stress value of the non-composite intermediate layer joint is used for normalization, and the von-Mises stress σ of the non-composite joint is v The value is taken as 100%, and the von-Mises stress σ of the uniform gradient intermediate layer joint v The value is about 52.6%, and the von Mises stress σ of the optimized gradient intermediate layer joint v The value is about 52.5%. And, from Figure 5 It can be seen that through finite element analysis, the maximum shear stress τ generated by heating the heterogeneous material joint from zero stress state to 180K xy The von Mises stress σ of the uniform gradient intermediate joint is v The value is about 45%, and the von Mises stress σ of the optimized gradient intermediate layer joint v The value is about 38%. The optimization effect is the most significant.
[0066] S2. Based on machine learning, determine the proportion of aluminum-based silicon carbide or high-strength aluminum in each layer of the composite material corresponding to the minimization of the thermal stress.
[0067] In a specific implementation, the proportion of aluminum-based silicon carbide or high-strength aluminum in the middle layer is determined by the minimum thermal stress in the thermal stress distribution obtained by the heterogeneous material joint when the temperature is increased by 180K from the zero stress state. The thermal stress specifically includes: von Mises stress σ v , maximum principal stress σ m , transverse normal stress σ x , longitudinal normal stress σ y or shear stress τ xy In the embodiment of the present invention, the thermal stress distribution obtained in step S1 is subjected to machine learning to calculate the proportion of aluminum-based silicon carbide or high-strength aluminum in each layer of the composite material when the thermal stress is minimum.
[0068] Machine learning methods can adopt genetic algorithms, particle swarm optimization, simulated annealing, ant colony algorithms, etc. Taking genetic algorithms as an example, genetic algorithm optimization can be implemented with the help of matlab software or python language. The population size is 20, the crossover rate is 0.5, and the number of elite individuals is 2. Each individual in the initial population is set to ρ1=ρ2=ρ3=ρ4=0.5. After iteration, the genetic algorithm obtains the component distribution with the minimum thermal stress (the proportion of aluminum-based silicon carbide or high-strength aluminum in each layer of composite material phase) and the minimum stress value.
[0069] The genetic algorithm process calculates the optimal component process. Figure 6, starting from the initial population (generation 0), calculate the peak value of thermal stress of each individual in the population and evaluate its fitness function. According to the evaluation results, apply genetic operators to produce the next generation. The selection operator selects excellent individuals in the population (i.e., individuals with small thermal stress). The crossover operator combines the information of different individuals (i.e., combines the material component values between different individuals); the mutation operator generates other new individuals to explore the global optimal solution. Determine whether the termination condition is met (function tolerance, maximum number of generations, etc. can be selected as the termination condition). If it is met, the optimal component that minimizes thermal stress is obtained; if it is not met, repeat the operation for the next generation population until the optimal component is produced.
[0070] Figure 7 The optimized thermal stress optimization result of the gradient intermediate layer joint provided by the embodiment of the present invention is shown as follows: Figure 7 As shown in Figure 2, machine learning calculates the von Mises stress σ of the heterogeneous material joint v , maximum principal stress σ m , transverse normal stress σ x , longitudinal normal stress σ y and the shear stress τ xy At the minimum, the proportion of aluminum-based silicon carbide in each layer of composite material. Figure 7 It can be seen that the von-Mises stress σ of the heterogeneous material joint v In the first composite phase determined by minimization, the proportion of aluminum-based silicon carbide is 21%; in the second composite phase, the proportion of aluminum-based silicon carbide is 38%; in the third composite phase, the proportion of aluminum-based silicon carbide is 57%; in the fourth composite phase, the proportion of aluminum-based silicon carbide is 85%; the maximum principal stress σ of the heterogeneous material joint is m In the first composite phase determined by minimization, the proportion of aluminum-based silicon carbide is 40%; in the second composite phase, the proportion of aluminum-based silicon carbide is 25%; in the third composite phase, the proportion of aluminum-based silicon carbide is 28%; in the fourth composite phase, the proportion of aluminum-based silicon carbide is 47%; the transverse normal stress σ of the heterogeneous material joint is x In the first composite phase determined by minimization, the proportion of aluminum-based silicon carbide is 15%; in the second composite phase, the proportion of aluminum-based silicon carbide is 15%; in the third composite phase, the proportion of aluminum-based silicon carbide is 28%; in the fourth composite phase, the proportion of aluminum-based silicon carbide is 39%; the longitudinal normal stress σ of the heterogeneous material joint is y In the first composite phase determined by minimization, the proportion of aluminum-based silicon carbide is 75%; in the second composite phase, the proportion of aluminum-based silicon carbide is 75%; in the third composite phase, the proportion of aluminum-based silicon carbide is 83%; in the fourth composite phase, the proportion of aluminum-based silicon carbide is 56%; the shear stress τ of the heterogeneous material joint xyIn the first composite material phase determined by minimization, the proportion of aluminum-based silicon carbide is 32%; in the second composite material phase, the proportion of aluminum-based silicon carbide is 52%; in the third composite material phase, the proportion of aluminum-based silicon carbide is 47%; in the fourth composite material phase, the proportion of aluminum-based silicon carbide is 69%.
[0071] In specific implementation, the composite material phase can use traditional manufacturing processes, such as particle reinforcement or fiber reinforcement, etc.; it can also be prepared using a "two-step manufacturing" method such as liquid phase sintering and melt infiltration.
[0072] It should be noted that, based on the heterogeneous material joint and design method provided by the present invention, the number of layers, layer thickness, and type of thermal stress of the intermediate layer can be flexibly selected according to the manufacturing process constraints and structural load conditions. The present invention does not limit this.
[0073] The present invention provides a composite material intermediate layer stress discretization (optimized gradient intermediate layer) heterogeneous material joint and design method, by designing the material component distribution of the intermediate layer, aluminum-based silicon carbide or high-strength aluminum is non-uniformly distributed in the intermediate layer, so that the thermal expansion coefficient of the intermediate layer is gradiently transitioned at the heterogeneous material interface (along the interface thickness direction), thereby achieving the lowest thermal mismatch stress of the heterogeneous material joint. The design method can also be applied to other heterogeneous material joints with different materials and different interface morphologies to achieve the purpose of minimizing the thermal stress of the joint.
[0074] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification.
[0075] For the method embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the order of the actions described, because according to the present invention, some steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and components involved are not necessarily required by the present invention.
[0076] The above is a detailed introduction to a heterogeneous material joint and an intermediate layer design method for a heterogeneous material joint provided by the present invention. Specific examples are used in this article to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea; at the same time, for general technical personnel in this field, according to the idea of the present invention, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.
Claims
1. A method for designing an intermediate layer of a heterogeneous material joint, characterized in that: The heterogeneous material joint comprises a first component layer, an intermediate layer and a second component layer stacked in a thickness direction, wherein the intermediate layer is a multilayer composite material phase formed by the first component and the second component, and the method comprises: Based on finite element analysis, the thermal stress distribution of the heterogeneous material joint is calculated; Based on machine learning, determining the proportion of the first component or the second component corresponding to the minimum thermal stress in the thermal stress distribution in each layer of the composite material phase; The thermal stress includes the von-Mises stress σ v , maximum principal stress σ m , transverse normal stress σ x , longitudinal normal stress σ y or shear stress τ xy .
2. The design method according to claim 1, characterized in that: The thermal stress distribution of the heterogeneous material joint is calculated based on the finite element analysis, including: Performing geometric modeling on the heterogeneous material joint to obtain a geometric model; Based on the geometric model, meshing is performed on each region of the heterogeneous material joint, and the proportion of the first component or the second component in each layer of the composite material phase constituting the intermediate layer is set as a boundary condition and a load condition to obtain a finite element thermal stress calculation program; Under the condition that only the proportion of the first component or the second component in each layer of the composite material phase constituting the intermediate layer is changed, the thermal stress distribution of the heterogeneous material joint is calculated by the finite element thermal stress calculation program; The load condition is that the heterogeneous material joint is heated by 180K from a zero stress state.
3. The design method according to claim 1, characterized in that: The determining, based on machine learning, the proportion of the first component or the second component corresponding to the minimum thermal stress in the thermal stress distribution in each layer of the composite material comprises: Initializing the proportion of the first component or the second component in each layer of the composite material phase to 0.5, and obtaining the thermal stress peak value of the heterogeneous material joint according to the finite element analysis result; By using a machine learning algorithm, the proportion of the first component or the second component in each layer of the composite material is iteratively changed to obtain the proportion of the first component or the second component in each layer of the composite material and the minimum stress value when the thermal stress peak is minimum.
4. The design method according to claim 1, characterized in that: The machine learning algorithm is a genetic algorithm; the machine learning algorithm is used to iteratively change the proportion of the first component or the second component in each layer of the composite material to obtain the proportion of the first component or the second component in each layer of the composite material when the thermal stress peak is minimum, and the minimum stress value, including: Set the population size to 20, the crossover rate to 0.5, the elite individual to 2, and each individual in the initial population to 0.5, so that the proportion of the first component or the second component in each layer of the composite material is initialized to 0.5; Starting from the initial population, calculate the peak value of thermal stress of each individual in the population and evaluate its fitness function; According to the evaluation results, the genetic operator is applied to generate the next generation, and the selection operator is used to select individuals with small peak heat stress in the population; The crossover operator is used to combine the information of different individuals to combine the material component values between different individuals; Use mutation operators to generate other new individuals to explore the global optimal solution; Determine whether the termination condition is met, and if so, obtain the proportion of the first component or the second component in each layer of the composite material when the thermal stress peak is minimum, and the minimum stress value; If not reached, the operation is repeated for the next generation population until the thermal stress peak is minimized, and the proportion of the first component or the second component in each layer of the composite material and the minimum stress value are achieved.
5. The design method according to claim 1, characterized in that: The first component is high-strength aluminum, and the second component is aluminum-based silicon carbide; the intermediate layer is composed of a first composite material phase, a second composite material phase, a third composite material phase, and a fourth composite material phase that are stacked; In the intermediate layer, the proportion of the aluminum-based silicon carbide or high-strength aluminum is, and the von-Mises stress σ of the heterogeneous material joint is v The proportion of the aluminum-based silicon carbide or high-strength aluminum in each layer of the composite material is the minimum; in the first composite material phase, the proportion of the aluminum-based silicon carbide is 21%; in the second composite material phase, the proportion of the aluminum-based silicon carbide is 38%; in the third composite material phase, the proportion of the aluminum-based silicon carbide is 57%; in the fourth composite material phase, the proportion of the aluminum-based silicon carbide is 85%.
6. The design method according to claim 1, characterized in that: The first component is high-strength aluminum, the second component is aluminum-based silicon carbide, and the intermediate layer is composed of a first composite material phase, a second composite material phase, a third composite material phase, and a fourth composite material phase that are stacked; In the intermediate layer, the proportion of the aluminum-based silicon carbide or high-strength aluminum is, and the maximum principal stress σ of the heterogeneous material joint is m The proportion of the aluminum-based silicon carbide or high-strength aluminum in each layer of the composite material is minimum; in the first composite material phase, the proportion of the aluminum-based silicon carbide is 40%; in the second composite material phase, the proportion of the aluminum-based silicon carbide is 25%; in the third composite material phase, the proportion of the aluminum-based silicon carbide is 28%; in the fourth composite material phase, the proportion of the aluminum-based silicon carbide is 47%.
7. The design method according to claim 1, characterized in that: The first component is high-strength aluminum, the second component is aluminum-based silicon carbide, and the intermediate layer is composed of a first composite material phase, a second composite material phase, a third composite material phase, and a fourth composite material phase that are stacked; In the intermediate layer, the proportion of the aluminum-based silicon carbide or high-strength aluminum is, and the transverse normal stress σ of the heterogeneous material joint x The proportion of the aluminum-based silicon carbide or high-strength aluminum in each layer of the composite material is the minimum; in the first composite material phase, the proportion of the aluminum-based silicon carbide is 15%; in the second composite material phase, the proportion of the aluminum-based silicon carbide is 15%; in the third composite material phase, the proportion of the aluminum-based silicon carbide is 28%; in the fourth composite material phase, the proportion of the aluminum-based silicon carbide is 39%.
8. The design method according to claim 1, characterized in that: The first component is high-strength aluminum, the second component is aluminum-based silicon carbide, and the intermediate layer is composed of a first composite material phase, a second composite material phase, a third composite material phase, and a fourth composite material phase that are stacked; In the intermediate layer, the proportion of the aluminum-based silicon carbide or high-strength aluminum is, and the longitudinal normal stress σ of the heterogeneous material joint y The proportion of the aluminum-based silicon carbide or high-strength aluminum in each layer of the composite material is minimum; in the first composite material phase, the proportion of the aluminum-based silicon carbide is 75%; in the second composite material phase, the proportion of the aluminum-based silicon carbide is 75%; in the third composite material phase, the proportion of the aluminum-based silicon carbide is 83%; in the fourth composite material phase, the proportion of the aluminum-based silicon carbide is 56%.
9. The design method according to claim 1, characterized in that: The first component is high-strength aluminum, the second component is aluminum-based silicon carbide, and the intermediate layer is composed of a first composite material phase, a second composite material phase, a third composite material phase, and a fourth composite material phase that are stacked; In the intermediate layer, the proportion of the aluminum-based silicon carbide or high-strength aluminum is, and the shear stress τ of the heterogeneous material joint xy The proportion of the aluminum-based silicon carbide or high-strength aluminum in each layer of the composite material is the minimum; in the first composite material phase, the proportion of the aluminum-based silicon carbide is 32%; in the second composite material phase, the proportion of the aluminum-based silicon carbide is 52%; in the third composite material phase, the proportion of the aluminum-based silicon carbide is 47%; in the fourth composite material phase, the proportion of the aluminum-based silicon carbide is 69%.
10. A heterogeneous material joint, characterized in that: A heterogeneous material joint obtained by the intermediate layer design method described in any one of claims 1-9.
Citation Information
Cited By
Bluetooth earphone cabin shell gradient injection molding method
CN120245353A