Plasma processing method
By forming a boron-containing protective film on the sidewall of the mask pattern, plasma etching technology is used to improve the resistance of the protective film, solve the problems of reduced etching selectivity ratio and reduced aperture, and achieve higher processing accuracy and dimensional control.
Patent Information
- Application Number
- CN202410905871.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2019-06-26
- Publication Date
- 2024-10-11
AI Technical Summary
In extreme ultraviolet exposure technology, as the mask pattern becomes miniaturized, the thin film of the resist film continues to develop, resulting in a reduction in the etching selectivity and a reduction in the hole pattern aperture, thereby limiting the processing accuracy, and the protective film has insufficient resistance to plasma. Affects the processing size control of the etched film.
A protective film containing boron is formed on the sidewall of the mask pattern, and the resistance of the protective film is improved through plasma etching technology, thereby improving the processing accuracy of the etched film.
By forming a highly resistant boron protective film on the sidewall of the mask pattern, finer hole pattern processing is achieved, improving the processing accuracy and dimensional control of the etched film.
Smart Images

Figure CN118762989A_ABST
Abstract
Description
[0001] This application is a divisional application of the invention patent application with application number 201980005144.7, invention name “Plasma Treatment Method”, and application date June 26, 2019 (international publication date is May 22, 2020). Technical Field
[0002] The present invention relates to a plasma processing technology, and more particularly to a technology effectively applied to a technology for etching a film to be etched after a protective film is formed on a side wall of a mask pattern. Background Art
[0003] Japanese Patent Application Laid-Open No. 2009-200080 (Patent Document 1) describes an etching technique in which a desired size and shape are obtained by etching using a mixed gas including a gas containing oxygen and a gas containing sulfur and not containing oxygen, thereby protecting the sidewalls.
[0004] Japanese Patent Application Publication No. 2018-56345 (Patent Document 2) describes a technique in which a hard mask having a boron-based film is used as an etching mask when dry etching is performed on a film including a silicon oxide film formed on a substrate to be processed.
[0005] Prior Art Literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2009-200080
[0008] Patent Document 1: Japanese Patent Application Publication No. 2018-56345 Summary of the invention
[0009] -Problems to be solved by the invention-
[0010] In recent years, the miniaturization of semiconductor devices has continued to develop, and as a result, the high-density processing technology has been continuously required. Under such circumstances, in the second-generation photolithography technology represented by extreme ultraviolet exposure technology (EUV technology), along with the miniaturization of the mask pattern, the thin film of the resist film constituting the mask pattern has continued to develop. As a result, the etching selectivity between the mask pattern and the etched film has been reduced, and the aperture of the hole pattern, etc., has been reduced due to the limitation of the photolithography technology, and the limitation has become significant.
[0011] In response to the above-mentioned problems, the following technology is proposed: a protective film is formed on a mask pattern, and the mask pattern and the protective film are used as a mask to etch the etched film. According to this technology, as a result of forming the protective film on the mask pattern, the etched film can be processed with a processing accuracy that is finer than the dimensional accuracy of the mask pattern.
[0012] However, in the technology of forming a protective film with a mask pattern, the protective film functions as a part of the etching mask. Therefore, for example, when the etched film is processed using a plasma etching technology, the protective film constituting a part of the etching mask is required to have resistance to plasma. However, when the material used for the protective film is not sufficiently resistant to plasma, the controllability of the processing size of the etched film is reduced. Therefore, from the viewpoint of improving the controllability of the processing size of the etched film, it is required to improve the resistance to plasma for the protective film formed in the mask pattern. The present invention provides a technology for improving the controllability of the processing size of the etched film by forming a protective film containing boron with high resistance to plasma on the side wall of the mask pattern.
[0013] -Methods for solving the problem-
[0014] A plasma processing method in one embodiment is a plasma processing method for performing plasma etching on an etched film using a mask, and is characterized in that it comprises: a deposition step, providing high-frequency power to a sample table carrying a sample on which the etched film is formed, and depositing a deposited film containing boron elements onto the mask; and an etching step, after the deposition step, etching the etched film using plasma.
[0015] -Effects of the Invention-
[0016] According to the plasma processing method in one embodiment, it is possible to improve processing dimensional accuracy. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a diagram showing the structure of a plasma etching device in an embodiment.
[0018] Figure 2 It is a cross-sectional view showing a plasma etching step in the embodiment.
[0019] Figure 3 It is a cross-sectional view showing a plasma etching step in the embodiment.
[0020] Figure 4 This is a graph showing the relationship between the film thickness of the protective film formed on the side wall of the resist pattern and the plasma processing time.
[0021] Figure 5 It is a cross-sectional view showing a plasma etching step in the embodiment.
[0022] Figure 6 It is a cross-sectional view showing a plasma etching step in the embodiment.
[0023] Figure 7 It is a cross-sectional view showing a plasma etching step in the embodiment.
[0024] Figure 8 It is a cross-sectional view showing a plasma etching step in the embodiment.
[0025] Fig. 9 It is a cross-sectional view showing a plasma etching step in the embodiment.
[0026] -Explanation of symbols-
[0027] 100 Plasma Etching Device
[0028] 101 Chamber
[0029] 102 processed substrate
[0030] 103 Workbench
[0031] 104 Sprinkler Plate
[0032] 105 Dielectric Window
[0033] 106 Processing Room
[0034] 107 Gas supply device
[0035] 108 Waveguide
[0036] 109 Power supply for generating electromagnetic waves
[0037] 110 Magnetic field generating coil
[0038] 111 Plasma
[0039] 112 DC power supply
[0040] 113 High frequency power supply
[0041] 201 substrate
[0042] 202 Etched film
[0043] 203 Resist pattern
[0044] 204 Protective film
[0045] 205 hole pattern
[0046] 301 substrate
[0047] 302 Etched film
[0048] 303 Resist pattern
[0049] 304 protective film
[0050] 305 hole pattern
[0051] 306 hole pattern. DETAILED DESCRIPTION
[0052] In all the drawings for explaining the embodiments, the same reference numerals are given to the same components in principle, and repeated descriptions thereof are omitted. In addition, hatching may be added even in a top view to make the drawings easier to understand.
[0053] <Plasma Etching Equipment>
[0054] Figure 1 It is a diagram showing a schematic structure of a plasma etching device in this embodiment.
[0055] Figure 1 In the present embodiment, the plasma etching device 100 is constituted by, for example, a microwave ECR (Electron Cyclotron Resonance) discharge etching device.
[0056] The plasma etching device 100 in this embodiment includes: a chamber 101, a wafer arrangement electrode, that is, a workbench (sample table) 103 on which a substrate to be processed 102 is arranged, a shower plate 104 arranged on the upper surface of the chamber and used to introduce etching gas, and a dielectric window 105 that transmits microwaves. In the plasma etching device 100 in this embodiment, the workbench 103, the shower plate 104, and the dielectric window 105 are sealed inside the chamber 101 to form a processing chamber 106. The inside of the processing chamber 106 can be set to a high vacuum state.
[0057] The substrate to be processed 102 is composed of, for example, a silicon substrate, an etched film formed on the silicon substrate, and a mask pattern formed on the etched film. The silicon substrate is, for example, a semiconductor substrate of a planar substantially circular shape called a wafer. In addition, the etched film is, for example, formed of a laminated film of a polycrystalline silicon film and a silicon oxide film formed on the polycrystalline silicon film. In addition, the mask pattern is, for example, composed of a resist film patterned by photolithography.
[0058] A gas supply device 107 for supplying etching gas to the processing chamber 106 is connected to the shower plate 104. In addition, in order to transmit power for generating plasma to the processing chamber 106, a waveguide 108 for radiating high frequency for plasma generation, i.e., electromagnetic waves, is provided above the dielectric window 105. The electromagnetic waves transmitted to the waveguide 108 are oscillated from the electromagnetic wave generating power supply 109. At this time, the frequency of the electromagnetic wave is not particularly limited, but, for example, a microwave of 2.45 GHz can be used.
[0059] In addition, a magnetic field generating coil 110 for generating a magnetic field is arranged at the outer periphery of the processing chamber 106, and the electric power oscillated from the electromagnetic wave generating power supply 109 interacts with the magnetic field generated by the magnetic field generating coil 110, thereby generating a high-density plasma 111 inside the processing chamber 106. In addition, the surface of the workbench 103 is covered with a sprayed film (not shown).
[0060] The substrate 102 to be processed that has been introduced into the processing chamber 106 is attracted to the stage 103 by electrostatic force due to a DC voltage applied from a DC power supply 112, and its temperature is adjusted.
[0061] After the desired etching gas is supplied to the inside of the processing chamber 106 by the gas supply device 107, the pressure inside the processing chamber 106 is set to a given pressure. Then, in this state, plasma 111 is generated inside the processing chamber 106. Here, by applying a high-frequency bias power from a high-frequency power supply 113 connected to the workbench 103, ions are introduced from the plasma 111 into the substrate 102 to be processed, and the substrate 102 to be processed is subjected to plasma processing.
[0062] In addition, as the plasma etching device in this embodiment, a microwave ECR discharge etching device is used as an example, but the plasma etching device in this embodiment is not limited to this, and can be composed of, for example, a spiral wave plasma etching device, an inductively coupled plasma etching device, a capacitively coupled plasma etching device, etc.
[0063] <New insights discovered by the inventors>
[0064] Next, the findings newly discovered by the inventors when a plasma etching method using the above-mentioned plasma etching apparatus is performed will be described.
[0065] For example, the plasma etching method shown below is implemented by the above-mentioned plasma etching device. That is, first, a substrate having an etched film and a mask pattern formed on the etched film is fed into the plasma etching device. Then, in the plasma etching device, a protective film is formed on the side wall of the mask pattern. Thus, if the combination of the mask pattern and the protective film is used as a mask, a high-precision mask pattern can be formed compared to the case where the mask pattern is used alone. This is because, for example, attention is paid to the interval between the first pattern and the second pattern constituting the mask pattern. In this case, if a protective film is formed on the side wall of the first pattern and a protective film is formed on the side wall of the second pattern, the interval between the protective film formed on the side wall of the first pattern and the protective film formed on the side wall of the second pattern is narrower than the interval between the first pattern and the second pattern. As a result, for example, the diameter of the hole pattern formed by processing the etched film exposed between the protective film formed on the side wall of the first pattern and the protective film formed on the side wall of the second pattern is smaller than the diameter of the hole pattern formed by processing the etched film using the first pattern and the second pattern as a mask. This means that by forming a protective film on the sidewalls of the mask pattern, a finer hole pattern can be formed compared to using the mask pattern alone. Therefore, it can be seen that by using a mask with a protective film formed on the sidewalls of the mask pattern, a fine hole pattern that exceeds the limit of the mask pattern alone can be formed. In other words, by using the technology of forming a protective film on the sidewalls of the mask pattern, fine processing that is difficult to achieve using a mask pattern alone can be performed.
[0066] Here, the present inventors studied the technology of forming a protective film on the side wall of the mask pattern, and as a result, obtained the new findings shown below, which will be described below.
[0067] For example, a protective film is formed on the side wall of a mask pattern, and the combination of the mask pattern and the protective film is used as a mask to perform plasma etching on the film to be etched. In this case, not only the mask pattern but also the protective film is exposed to the plasma atmosphere. Therefore, the protective film is required to have resistance to plasma.
[0068] In this regard, for example, if a protective film with insufficient resistance to plasma is used to perform plasma etching of the etched film, the protective film is damaged by the plasma, resulting in, for example, the disappearance of the protective film, and the protective film cannot fully function as a mask. Therefore, if the resistance of the protective film to plasma is low, it becomes difficult to ensure the processing accuracy of the etched film. In other words, even if a mask in which a protective film is formed on the side wall of the mask pattern is used to perform plasma etching of the etched film, if the resistance of the protective film to plasma is low, even if the protective film is used to improve the processing accuracy of the etched film, a sufficient effect cannot be obtained.
[0069] Therefore, as a result of research to achieve a protective film with high plasma resistance, the inventors have newly discovered that by using a film containing boron (B) as a protective film for a mask pattern, the resistance of the protective film to plasma can be improved. That is, the so-called new insight discovered by the inventors refers to the following insight: in order to achieve micro-machining of the etched film based on plasma etching by forming a protective film on the side wall of the mask pattern, it is important to improve the resistance of the protective film to plasma, and on this premise, a film containing boron (B) is used as a protective film. In addition, the inventors have concretized the plasma etching method in the present embodiment shown below by applying this new insight to the plasma etching technology. The plasma etching method in the present embodiment is described below with reference to the accompanying drawings.
[0070] <Plasma Etching Method in Embodiment>
[0071] first, Figure 2 FIG. 2 is a diagram showing a substrate as an object to be subjected to the plasma etching method according to the present embodiment. Figure 2 As shown in FIG. 1 , the substrate 201 of the present embodiment is, for example, a silicon substrate, and an etched film 202 is formed on the substrate 201. The etched film 202 is formed of, for example, a resist film, a polysilicon film, a silicon oxide film, or a silicon nitride film. In addition, a pre-patterned resist pattern 203 is formed on the etched film 202, for example. The resist pattern 203 is an example of a mask pattern of the present embodiment. The substrate 201 thus constructed is, for example, fed into a Figure 1 The plasma etching apparatus 100 shown in the figure has a processing chamber 106 and is arranged on a workbench 103 arranged inside the processing chamber 106 .
[0072] Next, for the substrate 201 placed on the workbench 103, a protective film 204 containing boron is formed on the sidewalls of the resist pattern 203. That is, in the present embodiment, in a plasma etching apparatus for plasma etching a film to be etched, as shown in FIG. Figure 3 As shown in FIG. 2 , a protective film 204 containing boron is formed on the side walls of the resist pattern 203 .
[0073] Specifically, the temperature of the substrate 201 is maintained at a temperature of more than 10°C and less than 100°C, and plasma is generated in the processing chamber based on a mixed gas containing a gas containing boron and an etching gas, thereby performing a process of forming the protective film 204 of the plasma etching device. For example, the gas containing boron is a deposition gas and becomes a raw material gas for the film containing boron. On the other hand, in the present embodiment, an etching gas is also introduced together with the deposition gas, i.e., the gas containing boron. At this time, the etching gas has the function of removing the deposited film. Therefore, by adjusting the addition ratio of the deposition gas, i.e., the gas containing boron, to the etching gas, the amount of deposit generated can be controlled. Here, as the deposition gas, a gas containing nitrogen can also be added together with the gas containing boron. In this case, boron nitride is also contained in the protective film. On the other hand, as the etching gas, for example, a gas containing fluorine or a gas containing chlorine can be used.
[0074] In addition, at this time, from Figure 1 The high frequency power source 113 connected to the workbench 103 of the plasma etching device 100 shown in FIG. Figure 1 RF bias (high frequency power) is applied to the substrate 102 to be processed. Thus, by sputtering the ions contained in the plasma to the protective film 204 formed on the surface of the etched film 202, the protective film 204 formed on the etched film 202 can be removed, and a protective film containing boron can be selectively formed on the side wall of the resist pattern 203. However, when the RF bias is applied to the substrate 201, the resist pattern 203 will also be damaged. Therefore, in order to suppress the damage to the resist pattern 203 and remove the protective film 204 formed on the surface of the etched film 202, it is desirable to adjust the RF bias applied to the substrate 201 so that the incident energy of the ions is about 50eV to 500eV.
[0075] For example, under the processing conditions shown below, the formation process of the protective film 204 of the present embodiment is implemented. Specifically, as the processing condition, the power of the microwave is set to 500W, and the RF bias is implemented at 30W. In addition, a mixed gas of BCl3 gas introduced into the processing chamber at 50ml / min, N2 gas introduced into the processing chamber at 50ml / min, CF4 gas introduced into the processing chamber at 50ml / min, and Ar gas introduced into the processing chamber at 50ml / min is used. In addition, as a processing condition, the condition of maintaining the internal pressure of the processing chamber at 0.5Pa and maintaining the temperature of the substrate 201 (wafer) at 40°C is used. In this way, a protective film 204 composed of a film containing boron can be formed on the side wall of the resist pattern 203.
[0076] here, Figure 4This is a graph showing the relationship between the film thickness of the protective film 204 formed on the side wall of the resist pattern 203 and the plasma treatment time when the above-mentioned treatment conditions are applied to a hole sample using a multilayer resist structure. Figure 4 In FIG. 1 , the horizontal axis represents the processing time (sec), and the vertical axis represents the film thickness (nm) of the protective film 204. Figure 4 As shown in FIG. 1 , the film thickness of the protective film 204 changes according to the processing time. Specifically, it can be seen that when the processing time is changed within the range of 10 seconds to 40 seconds, the film thickness of the protective film 20 changes from 6 nm to about 13 nm. Figure 4 It is known that if the processing time is extended, the film thickness of the protective film 204 increases. Therefore, it is known that in the process of forming the protective film 204 of the present embodiment, by adjusting the time (processing time) for generating plasma, the film thickness of the protective film 204 can be adjusted. That is, in the process of forming the protective film 204 of the present embodiment, by adjusting the time (processing time) for generating plasma, the film thickness of the protective film 204 can be adjusted. Figure 4 By adjusting the processing time, the thickness of the protective film 204 can be controlled to achieve the desired pore size.
[0077] Then, if Figure 5 As shown, in a plasma etching device, the etching target film 202 is etched using the resist pattern 203 and the protective film 204 as masks. Thus, a hole pattern 205 can be formed in the etching target film 202 in accordance with the protective film 204.
[0078] For example, under the processing conditions shown below, the process of forming the hole pattern 205 of the present embodiment is implemented. Specifically, as the processing condition, the microwave power is set to 900 W, and the RF bias is implemented at 150 W. In addition, a mixed gas of SO2 gas introduced into the processing chamber at 200 ml / min, O2 gas introduced into the processing chamber at 100 ml / min, and He gas introduced into the processing chamber at 500 ml / min is used. In addition, as the processing condition, the condition of maintaining the internal pressure of the processing chamber at 2.4 Pa and maintaining the temperature of the substrate 201 (wafer) at 40°C is used. In this way, the hole pattern 205 can be formed by plasma etching the etched film 202 using the resist pattern 203 and the protective film 204 as a mask.
[0079] Here, in the plasma etching method of the present embodiment, the protective film 204 is formed of a film containing boron, so that, for example, the protective film 204 can be realized with higher resistance to plasma than the resist pattern 203. In addition, compared with any of the carbon-containing film and the silicon-containing film, the film containing boron has higher resistance to plasma. Therefore, according to the present embodiment, by using the film containing boron as the protective film 204, the micro-machining accuracy of the hole diameter of the hole pattern 205 formed using the protective film 204 as a mask can be stably realized.
[0080] In addition, when implementing the plasma etching method in this embodiment, there are no particular restrictions on the type of processing device (plasma etching device) and processing conditions as long as the mask formed by the combination of the resist pattern 203 and the protective film 204 has a selectivity with the etched film 202 and can obtain the desired aperture. However, as in this embodiment, in a case where a structure is adopted in which the process of forming the protective film 204 and the process of plasma etching the etched film 202 are continuously processed together in one plasma etching device, an effect of improving productivity can be obtained.
[0081] <Features of the embodiment>
[0082] Next, the characteristic points of this embodiment will be described.
[0083] The characteristic point of this embodiment is that, in a plasma etching device that performs plasma etching on an etched film formed on a substrate, a protective film containing boron is formed on the side wall of a resist pattern formed on the etched film before the etched film is plasma-etched. In other words, the characteristic point of this embodiment is that a protective film containing boron is formed in a plasma etching device having a function of performing plasma etching.
[0084] Thus, since the protective film containing boron can be formed on the side wall of the resist pattern by plasma processing, the protective film can be formed while maintaining the substrate temperature at 10° C. or higher and 100° C. or lower.
[0085] For example, Patent Document 2 described in "Background Art" describes a technique related to a hard mask having a boron film. In addition, Patent Document 2 describes, for example, using a CVD device to form a hard mask having a boron film. In this regard, paragraph
[0026] of Patent Document 2 states that the temperature when forming a boron film by CVD is preferably in the range of 200°C to 500°C.
[0086] In this regard, since the heat resistance temperature of the hard mask is high, the boron-based film can be formed by the CVD method in the temperature range of 200° C. to 500° C. However, if the presence of a resist pattern is not a hard mask, the heat resistance temperature of the resist film constituting the general resist pattern is about 100° C. to 200° C. Therefore, it is difficult to form a protective film containing boron on the side wall of the resist pattern using the technology described in Patent Document 2.
[0087] This is because the film forming temperature of the boron-based film in the technology described in Patent Document 2 is higher than the heat resistance temperature of the resist film constituting the resist pattern. Therefore, if a film containing boron is formed on the resist pattern by using the CVD method described in Patent Document 2, for example, the resist pattern is thermally decomposed or a solidified layer is formed on the resist pattern, thereby making it difficult to form a film containing boron on the resist pattern while maintaining the original size of the resist pattern.
[0088] In this regard, according to the characteristic point of the present embodiment, a protective film containing boron is formed on the side wall of the resist pattern by using plasma processing in a plasma etching device instead of a CVD device, so that the substrate temperature can be lower than the heat resistance temperature of the resist pattern. That is, according to the characteristic point of the present embodiment, a protective film containing boron can be formed on the side wall of the resist pattern while maintaining the substrate temperature at a temperature lower than the heat resistance temperature of the resist pattern. Therefore, if the characteristic point of the present embodiment is adopted, a protective film containing boron can be used not only in a hard mask but also in a mask composed of a resist pattern. That is to say, according to the characteristic point of the present embodiment, regardless of the type of mask, a protective film containing boron can be formed on the side wall of the mask pattern over a wide range of types of masks as a whole without degenerating the mask material. In this way, the characteristic point of the present embodiment is that it is possible to provide a technical idea with high versatility regardless of the type of mask.
[0089] For example, a hard mask improves the etching selectivity ratio with respect to the etched film compared to a mask composed of a resist pattern, and is therefore used, for example, when forming a hole pattern with a high aspect ratio, while a mask composed of a resist pattern is used in patterning technology for the entire microfabrication. Therefore, it can be said that the use of a mask composed of a resist pattern is greater than that of a hard mask.
[0090] In addition, in the process of etching the etched film using a hard mask, first, after forming a resist pattern, the hard mask is formed using the resist pattern. Thereafter, the etched film is etched using the hard mask. Therefore, in the process of etching the etched film using a hard mask, a resist pattern forming process, a hard mask forming process, and an etched film etching process are required. In contrast, in the process of etching the etched film using a resist pattern, after forming the resist pattern, the etched film is etched using the resist pattern as a mask. That is, the process of etching the etched film using the resist pattern only requires a resist pattern forming process and an etched film etching process. Therefore, the process of etching the etched film using the resist pattern can reduce the number of processes compared to the process of etching the etched film using the hard mask.
[0091] Based on the above, compared with the technology described in Patent Document 2 which can only be applied to hard masks, the plasma etching method in this embodiment can be applied not only to hard masks but also to resist patterns, and can also be applied to resist patterns with high versatility. In this regard, it can have a very excellent advantage.
[0092] In addition, in this embodiment, a protective film containing boron is formed on the side wall of the resist pattern by using a plasma etching device that is usually used only for etching the etched film, which is very excellent. In particular, in the plasma etching device, by using a mixed gas containing a deposition gas and an etching gas, it is possible to adjust so that a protective film containing boron can be selectively formed on the side wall of the resist pattern, which is advantageous.
[0093] For example, when forming a protective film containing boron on the sidewalls of a mask pattern, for example, using a CVD device, after first forming the protective film so as to cover the mask pattern, it is necessary to perform anisotropic etching so that the protective film remains only on the sidewalls of the mask pattern. In this regard, in a plasma etching device, by adjusting the ratio of a deposition gas to an etching gas, and the incident energy of ions obtained from the plasma, a protective film containing boron can be formed only on the sidewalls of the mask pattern. This means that the process of forming a protective film containing boron on the sidewalls of a mask pattern using a plasma etching device can be simplified compared to the process of forming a protective film containing boron on the sidewalls of a mask pattern using a CVD device.
[0094] In addition, in a structure in which a protective film containing boron is formed on the side wall of a mask pattern using a plasma etching device, after the protective film containing boron is formed on the side wall of the mask pattern, the plasma etching of the etched film can be continuously performed using the mask pattern and the protective film as a mask without opening the processing chamber. In particular, if the protective film containing boron is exposed to the atmosphere, the protective film may react with oxygen and moisture in the atmosphere and deteriorate. In this regard, according to the present embodiment, as described above, in a processing chamber of a plasma etching device, the processing chamber is not opened to the atmosphere, and the process of forming a protective film containing boron on the side wall of the mask pattern and the plasma etching process of the etched film using the mask pattern and the protective film as a mask are continuously performed. Therefore, according to the present embodiment, the plasma etching of the etched film can be performed while maintaining the quality of the protective film with high resistance to plasma, which is a useful technical idea in this regard.
[0095] <Further research content>
[0096] In the plasma etching method of the present embodiment described above, in the plasma generated by the mixed gas of the deposition gas containing the gas containing boron and the etching gas, by adjusting the ratio of the deposition gas to the etching gas and the incident energy of the ions obtained from the plasma, a protective film containing boron is formed only on the side walls of the mask pattern. In this regard, for example, when the mask pattern has a region with a high pattern density and a region with a low pattern density, and the density difference of the pattern density is large, the following situation occurs: in the region with a high pattern density, a protective film containing boron is formed only on the side walls of the mask pattern, and on the other hand, in the region with a low pattern density, a protective film is formed not only on the side walls of the mask pattern but also on the surface of the etched film. This is because the surface area of the region with a low pattern density is relatively small compared to the surface area of the region with a high pattern density, and as a result, the film thickness of the deposition film per unit surface area in the region with a low pattern density is thicker than the film thickness of the deposition film per unit surface area in the region with a high pattern density.
[0097] Therefore, in the plasma etching method of this embodiment, when the mask pattern has a region with high pattern density and a region with low pattern density, and the density difference of the pattern density is large, the protective film containing boron may not be completely removed and may remain on the etched film in the region with low pattern density. In this case, in the region with low pattern density, plasma etching of the etched film may not be performed due to the protective film containing boron remaining on the etched film.
[0098] Therefore, in the present embodiment, further studies were conducted assuming that the mask pattern has a region with a high pattern density and a region with a low pattern density and that the difference in the density of the pattern is large. The contents of the studies are described below.
[0099] Figure 6 The figure schematically shows a substrate having a film to be etched and a resist pattern formed on the film to be etched, that is, a substrate having a region with a high pattern density and a region with a low pattern density in the resist pattern.
[0100] Here, if Figure 6 As shown in FIG. 1 , an etched film 302 is formed on a substrate 301, and a resist pattern 303 is formed on the etched film 302. Figure 6 As shown in FIG. 1 , in region RA, the pattern density of the resist pattern 303 formed on the etched film 302 is high. On the other hand, in region RB, the pattern density of the resist pattern 303 formed on the etched film 302 is low. In other words, the resist pattern 303 formed on the etched film 302 has a difference in pattern density. The substrate 301 thus constructed is fed, for example, to Figure 1 The processing chamber 106 of the plasma etching apparatus 100 is shown as being arranged inside the processing chamber 106 and on the workbench 103 .
[0101] Next, if Figure 7 As shown, for the substrate 301 placed on the stage 103, a protective film 304 containing boron is formed on the side walls of the resist pattern 303. That is, in this embodiment, the protective film 304 containing boron is formed on the side walls of the resist pattern 303.
[0102] At this time, the temperature of the substrate 301 is maintained at 10°C or higher and 100°C or lower, and plasma is generated in the processing chamber based on a mixed gas containing a gas (deposition gas) containing boron and an etching gas, thereby performing a process of forming the protective film 304 of the plasma etching device. In addition, in this embodiment, the addition ratio of the deposition gas, i.e., the gas containing boron, to the etching gas is adjusted. In addition, in the process of forming the protective film 304, for example, the addition ratio of the deposition gas, i.e., the gas containing boron, to the etching gas is adjusted. Figure 1 The high frequency power source 113 connected to the workbench 103 of the plasma etching device 100 shown in FIG. Figure 1 RF bias (high frequency power) is applied to the substrate to be processed 102). Thus, the incident energy of the ions obtained from the plasma is adjusted. In this way, the addition ratio of the deposition gas, i.e., the gas containing boron, and the etching gas, and the incident energy of the ions obtained from the plasma are adjusted. As a result, Figure 7 As shown in FIG. 1 , in the region RA, ions contained in the plasma are sputtered to the protective film 304 formed on the surface of the etched film 302, thereby removing the protective film 304 formed on the etched film 302. Figure 7 As shown, in the region RB, the protective film 304 formed on the surface of the etched film 302 is thicker than that in the region RA, so the protective film 304 formed on the etched film 302 remains.
[0103] That is, Figure 7 As shown in FIG. 1 , in the region RA where the pattern density of the resist pattern 303 is high, a protective film 304 containing boron is selectively formed on the sidewall of the resist pattern 303. Figure 7 As shown in the figure, in the region RB of the resist pattern 303 with low pattern density, the protective film 304 containing boron is formed not only on the sidewalls of the resist pattern 303, but also on the surface (upper surface) of the exposed etched film 302. This is because the surface area of the region RB with low pattern density is relatively small compared to the surface area of the region RA with high pattern density, and as a result, the film thickness of the protective film 304 per unit surface area of the region RB with low pattern density is thicker than the film thickness of the protective film 304 per unit surface area of the region RA with high pattern density.
[0104] Then, if Figure 8As shown in FIG. 1 , the protective film 304 formed on the etched film 302 in the region RB where the pattern density is low is removed. This step is a further development of the plasma etching step in this embodiment.
[0105] As a further research content, in order to remove the protective film 304 formed on the etched film 302 in the area RB with low pattern density, the plasma etching process shown below is adopted. Specifically, plasma etching is implemented under the processing conditions shown below. For example, as the processing condition, the power of the microwave is set to 500W, and the RF bias is implemented at 10W, and a mixed gas of CF4 gas introduced into the processing chamber at 100ml / min, HBr gas introduced into the processing chamber at 50ml / min, and Ar gas introduced into the processing chamber at 50ml / min is used. In addition, as the processing condition, the internal pressure of the processing chamber is maintained at 0.5Pa, and the temperature of the substrate 201 (wafer) is maintained at 40°C. In this way, as Figure 8 As shown, in the region RB where the pattern density is low, the protective film 304 formed on the surface of the film to be etched 302 can be removed.
[0106] Here, for example, after implementing Figure 7 After the step of forming the protective film 304 shown in FIG. 1 , if the surface of the substrate 301 is exposed to the atmosphere, the oxygen and moisture contained in the atmosphere may react with the protective film 304, and the surface of the protective film may be deteriorated. Figure 7 The steps of forming the protective film 304 and Figure 8 The step of removing the protective film 304 formed on the etched film 302 in the region RB with low pattern density shown in FIG. 1 is continuously performed without opening the processing room (chamber).
[0107] As described above, by adopting the further research contents of the plasma etching process in this embodiment, the protective film 304 formed on the etched film 302 in the region RB with low pattern density can be removed. Fig. 9 As shown in the figure, in the plasma etching device, in the region RA with high pattern density, the resist pattern 303 and the protective film 304 are used as masks to etch the etched film 302. As a result, the hole pattern 305 can be formed in the etched film 302 in accordance with the protective film 304. On the other hand, in the region RB with low pattern density, since the protective film 304 formed on the surface of the etched film 302 is removed, the resist pattern 303 and the protective film 304 can be used as masks to etch the etched film 302 in the region RB. As a result, the hole pattern 306 can be formed in the etched film 302 in accordance with the protective film 304 in the region RB.
[0108] As mentioned above, the invention made by the present inventors has been specifically described based on the embodiment. However, the present invention is not limited to the above-mentioned embodiment, and various modifications can be made without departing from the scope of the invention.
[0109] For example, in the above-mentioned embodiment, an example of using BCl 3 gas as the gas containing the boron element is described, but the present invention is not limited to this, and BF 3 gas, BBr 3 gas, etc. can be used.
[0110] Furthermore, in the above-described embodiment, an example of using N 2 gas as the gas containing nitrogen element is described, but the present invention is not limited to this, and NH 3 gas, NF 3 gas, etc. can be used.
[0111] In addition, in the above-mentioned embodiment, an example of using CF4 gas as the gas containing fluorine element is described, but it is not limited to this, and CHF3 gas, CH2F2 gas, CH3F gas, C4F8 gas, etc. can be used.
Claims
1. A plasma processing method, wherein a mask is used to perform plasma etching on an etched film, the plasma processing method comprising: A deposition step of supplying high frequency power to a sample stage on which a sample having the film to be etched is placed, and simultaneously using plasma generated by a mixed gas of a boron-containing gas and a nitrogen-containing gas to deposit a deposited film containing the boron element on the mask; a removal step of removing the deposited film deposited on the etched film in the second region by plasma while leaving the deposited film on the side wall of the mask in the first region and the second region after the deposition step; and an etching step, after the removal step, etching the film to be etched using plasma, The pattern density of the first region is higher than the pattern density of the second region.
2. The plasma processing method according to claim 1, wherein: The plasma in the removal step is generated using a mixed gas of hydrogen bromide gas and fluorine-containing element gas.
3. The plasma processing method according to claim 1, wherein: The boron-containing gas is boron trichloride gas. The nitrogen-containing gas is nitrogen.
4. The plasma processing method according to claim 1, wherein: The deposition process is performed using plasma generated using a mixed gas containing BCl 3 gas, N 2 gas, CF 4 gas and Ar gas.
5. The plasma processing method according to claim 2, wherein: The fluorine-containing gas is CF4 gas.
6. The plasma processing method according to claim 1, wherein: The plasma in the removal step is generated using a mixed gas containing CF 4 gas, HBr gas, and Ar gas.