Electronic device and preparation method thereof, electronic packaging piece and electronic equipment

By setting a laminated structure of a hard substrate and a flexible support plate on a flexible panel-level chip, the problem of low cutting success rate of flexible panels is solved, and the product yield and production efficiency are improved.

CN118763067APending Publication Date: 2024-10-11WUXI BAIROU PHOTOELECTRIC TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410869362.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Due to its flexible nature during the cutting process, flexible panel-level chips have a low cutting success rate, resulting in reduced product yield and are easily damaged during multi-chip packaging.

Method used

After the flexible film layer is placed on the hard substrate to form a conductive circuit layer, it is separated and attached to the flexible support plate to form a laminated structure. The flexible support plate provides tension to protect the conductive circuit layer, and is cut to form multiple circuits. unit.

Benefits of technology

It greatly improves the cutting yield of circuit units, reduces the probability of damage to the flexible film layer and conductive circuit layer, and improves the production efficiency and quality of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763067A_ABST
    Figure CN118763067A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an electronic device, the electronic device and an electronic packaging piece. The method comprises the following steps: arranging a flexible thin film on a hard substrate to form a flexible thin film layer; a conductive circuit layer is formed on the flexible thin film layer, and a conductive circuit is formed; separating the flexible thin film layer from the hard substrate; the flexible thin film layer is attached to a flexible supporting plate to form a laminated structure, the laminated structure is used for being cut into a plurality of circuit units, and the circuit units are used for forming the electronic device. In the manufacturing process of the electronic device, the flexible thin film is separated from the hard substrate and then attached to the flexible supporting plate, and the cutting yield of the circuit unit can be increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a flexible panel-level chip device preparation technology, and in particular to an electronic device and a preparation method thereof, an electronic package, and an electronic device. Background Art

[0002] At present, the preparation process of flexible panel-level chips is to form a circuit functional layer on a glass substrate and form a flexible chip panel through the circuits between the functional layers. However, due to the flexible nature of the flexible chip panel, the chip cutting success rate is quite low when cutting chip particles, resulting in a lower yield of the entire product. Even when the chip panel is packaged in multiple chips, the chip may be seriously damaged when cut by the user. Summary of the invention

[0003] The present application provides an electronic device and a manufacturing method thereof, and an electronic package to at least solve the aforementioned technical problems.

[0004] According to a first aspect of an embodiment of the present application, there is provided a method for preparing an electronic device, comprising:

[0005] Placing a flexible film on a rigid substrate to form a flexible film layer;

[0006] forming a conductive circuit layer on the flexible film layer to form a conductive circuit;

[0007] separating the flexible film layer from the rigid substrate;

[0008] A flexible film layer is attached to a flexible support plate to form a laminated structure, and the laminated structure is used to be cut into a plurality of circuit units, and the circuit units are used to form the electronic device.

[0009] In one embodiment, before separating the flexible film layer from the rigid substrate, or after attaching the flexible film layer to the flexible support plate, the method further comprises:

[0010] forming at least one control element on the flexible film, wherein the control element is used to be electrically connected to the conductive line,

[0011] The electronic device includes a cut circuit unit and at least one control element.

[0012] In one embodiment, before forming the conductive circuit layer on the flexible film layer, the method further includes:

[0013] A waterproof layer is arranged on the flexible film layer, and the waterproof layer is arranged between the flexible film layer and the conductive circuit layer.

[0014] In one embodiment, after forming the conductive circuit layer on the flexible film layer, the method further comprises:

[0015] An insulating layer is formed on the conductive circuit layer.

[0016] According to a second aspect of an embodiment of the present application, there is provided an electronic device, including:

[0017] Flexible support plate;

[0018] A flexible film layer is attached to the surface of the flexible support plate;

[0019] The conductive circuit layer is formed on the flexible film layer, and the conductive circuit layer is used to be bound with at least one control element.

[0020] In one possible implementation, the electronic device further includes:

[0021] At least one control element is formed on the flexible film, and the control element is electrically connected to the conductive circuit.

[0022] In one possible implementation, the electronic device further includes:

[0023] The waterproof layer is arranged on the flexible film layer, and the conductive circuit layer is formed on the waterproof layer.

[0024] In one embodiment, the line width of the conductive circuit in the conductive circuit layer is 0.5 micrometers to 20 micrometers.

[0025] In one embodiment, the Young's modulus of the flexible support plate is greater than the Young's modulus of the flexible film layer.

[0026] In one embodiment, the Young's modulus of the flexible film layer is in the range of: 5×10^9 N / m 2 Up to 10×10^9N / m 2 .

[0027] In one embodiment, the thermal expansion coefficient of the flexible film layer is in the range of 0.5-5 parts per million per degree Celsius.

[0028] In one possible implementation manner, the surface roughness of the flexible film layer is in the range of 0.1 nm-1 nm.

[0029] According to a third aspect of an embodiment of the present application, there is provided an electronic device, including:

[0030] Hard substrate;

[0031] A flexible support plate, arranged on the hard substrate;

[0032] A flexible film layer is attached to the surface of the flexible support plate;

[0033] The conductive circuit layer is formed on the flexible film layer, and the conductive circuit layer is used to be bound with at least one electronic component.

[0034] According to a fourth aspect of an embodiment of the present application, there is provided an electronic package, comprising:

[0035] The packaging shell is provided with a plurality of accommodating cavities, and the packaging shell is in a strip shape;

[0036] A plurality of the aforementioned electronic devices are arranged in the accommodating cavity.

[0037] According to a fifth aspect of the embodiments of the present application, an electronic device is provided, comprising the electronic device as described above.

[0038] The technical solution provided by the embodiments of the present application may have the following beneficial effects:

[0039] In the manufacturing method of the electronic device provided in the present application, after the flexible film layer is separated from the hard substrate, the flexible film layer is attached to the flexible support plate. When the laminated structure is cut, the flexible support plate can provide tension for the flexible film layer to better protect the conductive circuit layer, thereby preventing the flexible film layer from wrinkling during cutting and causing damage to the conductive circuit layer, thereby greatly improving the cutting yield of the circuit unit.

[0040] Furthermore, the electronic device formed by the manufacturing method of the present application includes the flexible support board, and there is no need to remove the flexible support board, which further reduces the probability of damage to the flexible film layer and the conductive circuit layer thereon.

[0041] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0043] Figure 1 A schematic diagram of a process for preparing an electronic device according to an embodiment of the present application;

[0044] Figure 2 A schematic diagram of the preparation process of an electronic device according to an embodiment of the present application;

[0045] Figure 3 A schematic diagram of the structure of a panel-level electronic device according to an embodiment of the present application;

[0046] Figure 4 A schematic diagram of the structure of an electronic device according to an embodiment of the present application;

[0047] Figure 5 This is a schematic diagram of the structure of an electronic seal according to an embodiment of the present application;

[0048] Figure 6 This is a schematic diagram of the structure of an electronic device according to another embodiment of the present application. DETAILED DESCRIPTION

[0049] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated. The implementations described in the following exemplary embodiments do not represent all implementations consistent with the present application. Instead, they are merely examples of devices and methods consistent with some aspects of the present application as detailed in the appended claims.

[0050] Figure 1 FIG. 1 is a flow chart of a method for preparing an electronic device according to an embodiment of the present application. Figure 1 As shown, the method for preparing the electronic device of the embodiment of the present application includes the following steps:

[0051] Step 101 : placing a flexible film on a rigid substrate to form a flexible film layer.

[0052] In the embodiment of the present application, considering the cost and processing convenience, the hard substrate adopts a glass substrate. The embodiment of the present application is described by taking a glass substrate as an example, and other hard materials such as hard plastics can also be used. The flexible film is bonded to the glass substrate. The flexible film mainly adopts a plastic material, which generally has the characteristics of flexibility, transparency, conductivity, insulation, etc. Physical vapor deposition, chemical vapor deposition, sputtering, ion beam and other methods are usually adopted. As an example, the sputtering method and ion beam method can be used to arrange the flexible film on the glass substrate to better control the accuracy and uniformity of the flexible film. In addition, the flexible film can also be a formed film.

[0053] The flexible film here can be at least one of the following materials: polyimide (PI), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), folded ultra-thin glass (UTG), etc. The operating temperature range of the selected flexible film is -60°C to 170°C, and it has high insulation performance. The thickness of the flexible film of the embodiment of the present application is 10 microns to 200 microns. As an example, the thickness of the flexible film can be 12 microns, 15 microns, 20 microns, 30 microns, 50 microns, 80 microns, 100 microns, 120 microns, 150 microns, or 180 microns, etc.

[0054] In this embodiment, the size range of the hard substrate can be greater than or equal to 500 mm in length and greater than or less than 400 mm in width. By selecting a glass substrate of a larger size within this range, more electronic devices can be manufactured, thereby improving the production efficiency of electronic devices. The function of the hard substrate is to serve as a bearing support, so as to facilitate the subsequent production of conductive circuits on the flexible film layer. Without a hard substrate, the flexible film may shrink and wrinkle when the conductive circuit layer is subsequently produced, which is not conducive to the formation of conductive circuits. The hard substrate is preferably a glass substrate.

[0055] Step 102: forming a conductive circuit layer on the flexible film layer to form a conductive circuit.

[0056] In the embodiment of the present application, a conductive material may be sputtered on the flexible film layer by magnetron sputtering to form a conductive circuit layer, and the conductive circuit layer includes a layer structure composed of a metal layer, graphene, metal oxide, etc. The material forming the metal layer in the embodiment of the present application may include at least one of aluminum, molybdenum, silver, chromium, nickel, titanium and copper, or a combination of multiple metals.

[0057] After forming the conductive material layer, the embodiment of the present application also needs to make a conductive circuit on the conductive material layer, that is, to arrange the circuit to form the conductive circuit required by the electronic device. As an implementation method, the yellow light process of the panel thin film transistor (Thin Film Transistor, TFT) can be used, and then the conductive material layer is formed into a conductive circuit layer through cleaning, photoresist coating, exposure, development, etching, film stripping and other manufacturing processes to generate various conductive circuits that can be used for circuit conduction. The line width (line width) and line spacing (line spacing or line-to-line distance) of the conductive circuit are two more important parameters of the conductive circuit. These two parameters can be set independently according to the design requirements and the limitations of the manufacturing process. The line width usually refers to the width of the conductor line, and the line spacing refers to the distance between the centers of adjacent conductor lines. During the design, in order to achieve the desired electrical performance, reduce crosstalk, increase integration density, optimize the manufacturing process and other factors, the line width and line spacing will be optimized separately.

[0058] The conductive circuit processing and manufacturing line width range of the embodiment of the present application is 0.5 micron to 20 microns, preferably 1-5 microns. As an example, the line width of the conductive circuit can be 1 micron, 2 microns, 3 microns, 5 microns, 7 microns, 10 microns, 13 microns, 15 microns, or 19 microns. The line spacing range is 0.5 microns to 25 microns. By first attaching the flexible film to the hard substrate in the present application, and then using the above-mentioned process method, a line width of 0.5 microns to 20 microns and a line spacing of 0.5 microns to 25 microns can be formed. Compared with the conventional method of forming a conductive circuit on a flexible film, the above method can significantly reduce the line width and line spacing between the conductive circuits.

[0059] The thickness of the conductive material layer of the embodiment of the present application ranges from 200 nanometers to 3000 nanometers. As an example, the thickness of the conductive material layer can be 250 nanometers, 300 nanometers, 500 nanometers, 800 nanometers, 1000 nanometers, 1200 nanometers, 1500 nanometers, 1600 nanometers, 1900 nanometers, 2000 nanometers, 2300 nanometers, 2500 nanometers, 2700 nanometers, or 2900 nanometers.

[0060] After being etched, the conductive layer in this embodiment will form a plurality of conductive line units arranged in a matrix. When the conductive layer is subsequently cut into a plurality of circuit units, each circuit unit will have one conductive line unit.

[0061] Step 103 , separating the flexible film layer from the rigid substrate.

[0062] In the embodiment of the present application, after the conductive circuit layer is formed on the flexible film layer, the flexible film layer is removed from the glass substrate to prepare for further manufacturing of the electronic device with a flexible support board according to the embodiment of the present application.

[0063] Step 104 , attaching the flexible film layer to a flexible support plate to form a laminated structure.

[0064] The stacked structure is used to be cut into a plurality of circuit units, and the circuit units are used to form the electronic device.

[0065] In an embodiment of the present application, after the flexible film layer is separated from the glass substrate, a corresponding flexible support plate is prepared, and the flexible film layer is attached to the flexible support plate to form a laminated structure, so that the flexible film layer and the conductive circuit layer thereon are supported by the flexible support plate, thereby facilitating subsequent cutting operations.

[0066] The flexible support plate of the embodiment of the present application can be made of polyethylene or polyurethane, which has the characteristics of good flexibility, high strength, and wear resistance while ensuring the supporting performance of the flexible support plate. The thickness of the flexible support plate is generally 0.1mm to 0.8mm. As an example, the thickness of the flexible support plate is 0.18mm, 0.2mm, 0.22mm, 0.25mm, 0.3mm, 0.35mm, or 0.4mm.

[0067] The Young's modulus range of the flexible film layer 10 in the embodiment of the present application is: 5×10^9 N / m 2 Up to 10×10^9N / m 2 As an example, the Young's modulus of the flexible film layer 10 is 5.1×10^9 N / m 2 , 5.3×10^9N / m 2 , 5.5×10^9N / m 2 , 5.8×10^9N / m 2 、6×10^9N / m 2 、6.2×10^9N / m 2 、6.5×10^9N / m 2 、6.7×10^9N / m 2 , or 7×10^9N / m 2 、7.4×10^9N / m 2 、7.8×10^9N / m 2 , 8×10^9N / m 2 、8.3×10^9N / m 2 、8.5×10^9N / m 2 , 9×10^9N / m 2 , 9.5×10^9N / m 2, 9.8×10^9N / m 2 wait.

[0068] In the embodiment of the present application, the Young's modulus of the flexible support plate is greater than the Young's modulus of the flexible film layer, and the Young's modulus of the flexible support plate may be in the range of 6×10^9 N / m 2 Up to 20×10^9N / m 2 By selecting a flexible support plate with a suitable Young's modulus, when the electronic device of the embodiment of the present application is deformed (eg folded), it can be ensured that the flexible support plate has sufficient elasticity to deform, making the structure of the electronic device more stable.

[0069] The thermal expansion coefficient of the flexible film layer of the embodiment of the present application is in the range of 0.5-5 parts per million per degree Celsius. As an example, the thermal expansion coefficient of the flexible film layer is 0.6 parts per million per degree Celsius, 0.8 parts per million per degree Celsius, 1 parts per million per degree Celsius, 1.2 parts per million per degree Celsius, 1.5 parts per million per degree Celsius, 1.7 parts per million per degree Celsius, 2 parts per million per degree Celsius, 2.2 parts per million per degree Celsius, 2.5 parts per million per degree Celsius, 2.8 parts per million per degree Celsius, 3 parts per million per degree Celsius, 3.3 parts per million per degree Celsius, 3.5 parts per million per degree Celsius, 3.9 parts per million per degree Celsius, 4.2 parts per million per degree Celsius, 4.6 parts per million per degree Celsius, or 4.8 parts per million per degree Celsius.

[0070] To ensure that other structural layers can be better formed on the flexible film layer, the surface roughness of the flexible film layer is in the range of 0.1nm-1nm. As an example, the surface roughness of the flexible film layer is 0.2nm, 0.3nm, 0.4nm, 0.5nm, 0.6nm, 0.7nm, 0.8nm, or 0.9nm.

[0071] Step 105 , cutting the laminated structure to form a plurality of circuit units.

[0072] The flexible film is separated from the glass, and the flexible film layer is attached to the flexible support plate to form a laminated structure, so as to cut the laminated structure into circuit units. In the embodiment of the present application, the flexible film is mechanically separated from the glass as a whole, the flexible film layer is attached to the flexible support plate, and then cut into corresponding circuit units, for example, by laser cutting. By attaching the flexible film layer to the flexible support plate, when the laminated structure is cut, the flexible support plate can provide tension for the flexible film layer to better protect the conductive circuit layer, prevent the flexible film layer from wrinkling during cutting and thus damage the conductive circuit layer, thereby greatly improving its yield rate.

[0073] The embodiment of the present application can support the flexible film layer and the conductive circuit layer by setting a flexible support plate. In this way, multiple electronic devices can be arranged on the flexible support plate in various set ways, so that multiple electronic devices can be packaged as a packaging unit, which not only facilitates the transportation of electronic devices, but also protects the electronic devices. In this way, the control components can be bound in units of the entire packaging unit, thereby improving the binding efficiency. After the user obtains the electronic device in the packaging unit, the corresponding electronic device can be cut out from the packaging unit according to the needs of use. And it can be determined whether to detach the flexible support plate from the electronic device as needed. The embodiment of the present application supports the detachment of the flexible support plate in units of the entire packaging unit, and the detachment efficiency of the flexible support plate is higher.

[0074] In the embodiment of the present application, before forming the conductive circuit layer on the flexible film layer, the preparation method further includes: forming a waterproof layer on the flexible film layer. The thickness of the waterproof layer is generally 20 nanometers to 500 nanometers, and it is coated on the flexible film layer by a sputtering process. The material of the waterproof layer is generally a silicon nitride film (SiNx) material, or a gate-silicon nitride (G-SiNx) material. In another embodiment, the waterproof layer can also be a waterproof film layer, which is directly attached to the flexible film layer to avoid the above-mentioned sputtering process.

[0075] In an embodiment of the present application, after forming a conductive circuit layer on the flexible film layer, the preparation method further includes: forming an insulating layer on the conductive circuit layer. Insulating ink is applied on the conductive circuit layer to form an insulating layer, which is applied to conductive circuits, control components and glass substrates that do not require welding, in order to protect the conductive circuit patterns formed on the glass substrate for a long time. The insulating ink is applied to the conductive circuit layer by ink printing, screen printing and other manufacturing processes to form an insulating layer. As an example, the main components of the insulating ink in an embodiment of the present application include: epoxy denatured resin, thermosetting epoxy resin, photoinitiator, body pigment, coloring pigment, additive, solvent. The body pigment is mainly composed of a mixture of at least one of salts of barium, calcium, magnesium, or aluminum, oxides of silicon or aluminum, and the like.

[0076] Figure 2 FIG. 1 is a schematic diagram of a manufacturing process of an electronic device according to an embodiment of the present application. Figure 2As shown, the preparation process of the electronic device of the embodiment of the present application includes: cleaning the glass substrate 15, coating PI on one side of the glass substrate to form a flexible film layer 10; checking the coating effect of the flexible film layer 10 by visual inspection to determine whether re-coating is required. The coated flexible film layer 10 is cleaned and then baked. The cleaning can be carried out by rolling a brush on the surface of the flexible film layer 10 to remove particles, and then the fine particles on the surface of the flexible film layer are removed again by liquid spraying to ensure the cleanliness of the surface of the flexible film layer 10. After the surface of the flexible film layer 10 is dried, a silicon nitride film or a gate-silicon nitride is coated on the flexible film layer by a sputtering process to form a waterproof layer. The thickness of the waterproof layer is generally 20 nanometers to 500 nanometers. A conductive material is sputtered on the waterproof layer to form a conductive material layer 11. The material of the conductive material layer 11 can be at least one of aluminum, molybdenum, silver, chromium, nickel, titanium and copper, or a superposition of several of them, or other conductive materials such as graphene, metal oxides, etc. The thickness of the conductive material layer 11 is between 200 and 3000 nanometers. The corresponding conductive circuit is made on the conductive material layer 11, that is, the wiring is carried out. Specifically, it is made by using the panel TFT yellow light process, and then processed into a conductive circuit with a line width of 1.5 to 20 through processes such as cleaning, photoresist coating, exposure, development, etching, and film stripping. After the circuit is made, a full electrical inspection is carried out to determine whether the conductive circuit of the conductive material layer is normal. Insulating ink is applied to the conductive circuit layer through a silk screen process, etc., so as to form an insulating layer, which is applied to the conductive circuit, control element and glass substrate 15 that do not require welding, in order to protect the conductive circuit pattern formed on the glass substrate 15 for a long time. Inspection is carried out by visual inspection of the appearance to determine whether the insulating layer covers all areas of the conductive circuit layer. At least one control element 13 such as an IC is bound to a flexible film so that the control element such as the IC is electrically connected to the conductive circuit of the conductive circuit layer 11. The conductive circuit layer 11 bound to the IC is treated with glue for protection, that is, protective glue is applied to the surface of the conductive circuit layer to solidify and form a protective film to protect the circuit board from damage such as scratches, improve its water resistance, shock resistance, corrosion resistance and other capabilities, and increase the mechanical strength and connection stability of the circuit board. The conductive circuit layer 11 after the glue protection treatment is fully electrically inspected to ensure that the conductive circuit can work normally. The flexible film layer 10 and the glass substrate 15 are separated, and the flexible film layer 10 is attached to a flexible support plate 14 to form a laminated structure to support the flexible film layer. Then, the flexible film layer 10 provided with the flexible support plate 14 is cut to form a plurality of corresponding electronic devices to achieve panel-level packaging, which can be transported and sold after packaging.

[0077] The method for preparing the electronic device in the embodiment of the present application further includes the following processing steps before separating the flexible film layer from the glass substrate:

[0078] At least one control element is disposed on the flexible film, and the control element is used to be electrically connected to the conductive circuit, wherein the cut circuit unit includes the control element. The control element here includes various control chips, control circuits, field programmable gate arrays (FPGA), micro controller units (MCU) and other elements. As an example, the control element can be bound to the conductive circuit layer by anisotropic conductive film (ACF) process; or the control element can be bound to the conductive circuit layer by ACF pressure-leading process, or the control element can be bound to the conductive circuit layer by inner lead bonding (ILB).

[0079] As another implementation method, after the flexible film layer is attached to the flexible support board, at least one control element can be arranged on the flexible film, and the control element is used to be electrically connected to the conductive circuit. The electronic device of the embodiment of the present application includes a cut circuit unit and at least one control element.

[0080] As a third implementation manner, after the stacked structure is cut into a plurality of circuit units, the control element may be arranged on the circuit unit.

[0081] In the embodiment of the present application, the control element is disposed on the flexible film before the flexible film layer is separated from the glass substrate. Since a plurality of matrix-type conductive circuit units have been formed on the flexible film, one conductive circuit unit can be electrically connected to one control element, or can be connected to a plurality of control elements to form an independent circuit entity, and the plurality of independent circuit entities are arranged in a matrix on the flexible film layer. Figure 3 As shown, it shows a schematic diagram of the structure of the panel-level electronic device of the embodiment of the present application. After the multiple control elements 13 are bound to the conductive circuit layer 11, the panel-level electronic device is formed. Cutting and packaging can be performed based on the panel-level electronic device. Figure 5 As shown, the cut electronic devices can be packaged in a packaging strip to facilitate subsequent processing or use. Those skilled in the art should understand that the cutting and packaging of the electronic devices can also be completed in other ways.

[0082] According to the technical solution of the embodiment of the present application, during the preparation process of the electronic device, a flexible support plate is firstly bonded to a glass substrate, and after the flexible film layer is separated from the hard substrate, the flexible film layer is attached to the flexible support plate. When the laminated structure is cut, the flexible support plate can provide tension for the flexible film layer to better protect the conductive circuit layer, thereby preventing the flexible film layer from wrinkling during cutting and causing damage to the conductive circuit layer, thereby greatly improving its yield rate.

[0083] The line width of the conductive circuit in the conductive circuit layer of the embodiment of the present application can be between 1.5 microns and 20 microns, thereby reducing the area of ​​COF (short for Chip On Film) and saving costs.

[0084] Figure 4 FIG. 1 is a schematic diagram of the structure of an electronic device according to an embodiment of the present application. Figure 4 As shown, the electronic device of the embodiment of the present application includes:

[0085] Flexible support plate 14: The flexible support plate 14 of the embodiment of the present application can be made of polyethylene or polyurethane, which has the characteristics of good flexibility, high strength, and wear resistance while ensuring the supporting performance of the flexible support plate 14. The thickness of the flexible support plate is generally 0.1mm to 0.8mm. As an example, the thickness of the flexible support plate is 0.18mm, 0.2mm, 0.22mm, 0.25mm, 0.3mm, 0.35mm, or 0.4mm.

[0086] The flexible film layer 10 is attached to the surface of the flexible support plate 14; the flexible film can be at least one of the following materials: polyimide (PI), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), folded ultra-thin glass (UTG), etc. The operating temperature range of the selected flexible film is -60°C to 170°C, and it has high insulation performance. The thickness of the flexible film of the embodiment of the present application is 10 microns to 200 microns. As an example, the thickness of the flexible film can be 12 microns, 15 microns, 20 microns, 30 microns, 50 microns, 80 microns, 100 microns, 120 microns, 150 microns, or 180 microns, etc.

[0087] The conductive circuit layer 11 is formed on the flexible film layer 10, and the conductive circuit layer 11 is used to bind with at least one control element. The thickness of the conductive material layer 11 ranges from 200 nanometers to 3000 nanometers. As an example, the thickness of the conductive material layer 11 can be 250 nanometers, 300 nanometers, 500 nanometers, 800 nanometers, 1000 nanometers, 1200 nanometers, 1500 nanometers, 1600 nanometers, 1900 nanometers, 2000 nanometers, 2300 nanometers, 2500 nanometers, 2700 nanometers, or 2900 nanometers.

[0088] like Figure 4 As shown, the electronic device of the embodiment of the present application further includes:

[0089] At least one control element is formed on the flexible film, and the control element is electrically connected to the conductive circuit. The control element includes an IC circuit 13. As an example, the control element of the embodiment of the present application includes various control chips, control circuits, FPGAs, MCUs and other elements. As an example, the control element can be bound to the conductive circuit layer by an ACF process; or the control element can be bound to the conductive circuit layer by an ACF compression process.

[0090] like Figure 4 As shown, the electronic device of the embodiment of the present application further includes:

[0091] Waterproof layer( Figure 4 The waterproof layer is disposed on the flexible film layer 10, and the waterproof layer is disposed between the flexible film layer 10 and the conductive circuit layer 11. The waterproof layer of the embodiment of the present application generally has a thickness of 20 nanometers to 500 nanometers, and is coated on the flexible film layer by a sputtering process. The material of the waterproof layer is generally a silicon nitride film (SiNx) material, or a gate-silicon nitride (G-SiNx) material, etc.

[0092] like Figure 4 As shown, the electronic device of the embodiment of the present application further includes: an insulating layer ( Figure 4 Insulating ink is coated on the conductive circuit layer 11 to form an insulating layer, which is coated on the conductive circuits, control components and flexible film layer 10 that do not require welding to protect the conductive circuit patterns formed on the flexible film layer 10. The insulating ink as the insulating layer is coated on the conductive circuit layer 11 by a manufacturing process such as ink printing or screen printing. In other embodiments, the insulating layer can also be other materials.

[0093] The Young's modulus of the flexible film layer of the embodiment of the present application is in the range of: 5×10^9N / m 2 Up to 10×10^9N / m 2 As an example, the Young's modulus of the flexible film layer is 5.1×10^9 N / m 2, 5.3×10^9N / m 2 , 5.5×10^9N / m 2 , 5.8×10^9N / m 2 、6×10^9N / m 2 、6.2×10^9N / m 2 、6.5×10^9N / m 2 、6.7×10^9N / m 2 , or 7×10^9N / m 2 、7.4×10^9N / m 2 、7.8×10^9N / m 2 , 8×10^9N / m 2 、8.3×10^9N / m 2 、8.5×10^9N / m 2 , 9×10^9N / m 2 , 9.5×10^9N / m 2 , 9.8×10^9N / m 2 wait..

[0094] The thermal expansion coefficient of the flexible film layer of the embodiment of the present application is in the range of 0.5-5 parts per million per degree Celsius. As an example, the thermal expansion coefficient of the flexible film layer is 0.6 parts per million per degree Celsius, 0.8 parts per million per degree Celsius, 1 parts per million per degree Celsius, 1.2 parts per million per degree Celsius, 1.5 parts per million per degree Celsius, 1.7 parts per million per degree Celsius, 2 parts per million per degree Celsius, 2.2 parts per million per degree Celsius, 2.5 parts per million per degree Celsius, 2.8 parts per million per degree Celsius, 3 parts per million per degree Celsius, 3.3 parts per million per degree Celsius, 3.5 parts per million per degree Celsius, 3.9 parts per million per degree Celsius, 4.2 parts per million per degree Celsius, 4.6 parts per million per degree Celsius, or 4.8 parts per million per degree Celsius. Selecting a flexible film layer with a suitable thermal expansion coefficient is conducive to the formation of a conductive circuit layer on the flexible film layer, and can further prevent damage to the flexible film layer during the process of photolithography of forming a conductive circuit on the conductive circuit layer.

[0095] The surface roughness of the flexible film layer of the embodiment of the present application is in the range of 0.1 nm to 1 nm. As an example, the surface roughness of the flexible film layer is 0.2 nm, 0.3 nm, 0.4 nm, 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, or 0.9 nm.

[0096] The line width of the conductive circuit in the conductive circuit layer 11 of the embodiment of the present application is 1.5 microns to 20 microns. As an example, the line width of the conductive circuit can be 1.8 microns, 2 microns, 3 microns, 5 microns, 7 microns, 10 microns, 13 microns, 15 microns, or 19 microns. The line spacing of the conductive circuit can range from 2 to 30 microns.

[0097] Figure 6 FIG. 1 is another schematic diagram of the structure of an electronic device according to an embodiment of the present application. Figure 6 As shown, the electronic device of the embodiment of the present application includes:

[0098] Glass substrate 15;

[0099] A flexible support plate 14, disposed on the glass substrate;

[0100] A flexible film layer 10 is attached to the surface of the flexible support plate;

[0101] The conductive circuit layer 11 is formed on the flexible film layer 10 , and the conductive circuit layer 11 is used to be bound with at least one electronic component.

[0102] The electronic device and Figure 4 Compared with the structure of the electronic device shown in FIG. 1 , a glass substrate 15 is further provided on the other surface of the flexible support plate 14. That is, the electronic device of the embodiment of the present application may also be an electronic device having a glass substrate 15, and the other structures are the same as those of FIG. Figure 4 The structure shown is exactly the same. When the glass substrate 15 needs to be removed, the glass substrate 15 is separated from the flexible support plate 14. Figure 4 Compared with the structure shown in FIG. 1 , the electronic device of this structure can omit the step of separating the flexible film layer 10 from the glass substrate 15, thereby preventing the flexible film layer 10 from being damaged when peeling off the glass substrate 15. The structure can directly remove the glass substrate 15 when necessary. Figure 6 The electronic device shown can also be packaged at the panel level to be suitable for different electronic product processing processes.

[0103] In the electronic device of the embodiment of the present application, the IC chip and the wiring structure are electrically connected to the conductive circuit of the conductive circuit layer 11. By setting the flexible support board 14, the IC chip and the wiring structure can be set at the end of the conductive circuit layer 11, and the end can be bent to adapt to the frame size of the subsequent packaging of the electronic device of the embodiment of the present application.

[0104] In the electronic device of the embodiment of the present application, the traditional production method is to bind the IC chip to the conductive circuit layer 11, carry the glass substrate for cutting, and then separate the flexible film layer 10 from the glass substrate, which will result in low production efficiency. In the embodiment of the present application, the flexible film layer 10 is first separated from the glass substrate, and then the flexible film layer 10 is attached to the surface of the flexible support plate 14. By attaching the flexible support plate 14 to the back of the flexible film, when the laminated structure is cut, the flexible support plate 14 can provide tension for the flexible film layer 10 to better protect the conductive circuit layer, prevent the flexible film layer 10 from wrinkling during cutting and then damaging the conductive circuit layer 11, and greatly improve its yield rate.

[0105] It can be understood that the circuit unit provided in the embodiment of the present application is a single product after cutting, and the electronic device includes the circuit unit and at least one control element. The electronic device is a semi-finished product, which is part of a terminal product (such as an electronic device).

[0106] The present application also describes an electronic device, which includes the electronic device described in the above embodiment. The electronic device includes but is not limited to a mobile phone, a PAD, a game console, a laptop computer, a television, etc.

[0107] Figure 5 FIG. 1 is a schematic diagram of the structure of an electronic seal according to an embodiment of the present application. Figure 5 As shown, the embodiment of the present application also describes an electronic package, including:

[0108] The packaging shell 20 is provided with a plurality of accommodating cavities 21, and the packaging shell 20 is in a strip shape;

[0109] The electronic devices of the aforementioned embodiments are arranged in the accommodating cavity 21. It is understandable that the entire electronic device can be arranged in the accommodating cavity 21, or a part of the electronic device can be accommodated in the accommodating cavity 21 to match the subsequent processing of the electronic device.

[0110] The electronic package of the embodiment of the present application supports packaging a plurality of electronic devices into corresponding packaging shells 20 as units.

[0111] It should be understood that the various forms of processes shown above can be used to reorder, add or delete steps. For example, the steps recorded in this disclosure can be executed in parallel, sequentially or in different orders, as long as the desired results of the technical solution disclosed in this application can be achieved, and this document is not limited here.

[0112] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0113] Furthermore, the term “formed on” in the present application may mean “directly” formed on, or “indirectly” formed on. That is, for example, if A is formed on B, it may be that A is directly formed on B, or there may be other structures between A and B. Therefore, the term “formed on” in the present application does not only mean directly formed on.

[0114] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any person skilled in the art who is familiar with the present technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing an electronic device, characterized in that: The method comprises: Placing a flexible film on a rigid substrate to form a flexible film layer; forming a conductive circuit layer on the flexible film layer to form a conductive circuit; separating the flexible film layer from the rigid substrate; A flexible film layer is attached to a flexible support plate to form a laminated structure, and the laminated structure is used to be cut into a plurality of circuit units, and the circuit units are used to form the electronic device.

2. The preparation method according to claim 1, characterized in that: Before separating the flexible film layer from the rigid substrate, or after attaching the flexible film layer to the flexible support plate, the method further comprises: forming at least one control element on the flexible film, wherein the control element is used to be electrically connected to the conductive line, The electronic device includes a cut circuit unit and at least one control element.

3. The preparation method according to claim 1, characterized in that: Before forming the conductive circuit layer on the flexible film layer, the method further comprises: A waterproof layer is arranged on the flexible film layer, and the waterproof layer is arranged between the flexible film layer and the conductive circuit layer.

4. The preparation method according to claim 1, characterized in that: After forming a conductive circuit layer on the flexible film layer, the method further comprises: An insulating layer is formed on the conductive circuit layer.

5. An electronic device, characterized in that: The electronic device comprises: Flexible support plate; A flexible film layer is attached to the surface of the flexible support plate; The conductive circuit layer is formed on the flexible film layer, and the conductive circuit layer is used to be bound with at least one control element.

6. The electronic device according to claim 5, characterized in that: The electronic device further comprises: At least one control element is formed on the flexible film, and the control element is electrically connected to the conductive circuit.

7. The electronic device according to claim 5, characterized in that: The electronic device further comprises: The waterproof layer is arranged on the flexible film layer, and the conductive circuit layer is formed on the waterproof layer.

8. The electronic device according to claim 5, characterized in that: The line width of the conductive circuit in the conductive circuit layer ranges from 0.5 micrometers to 20 micrometers.

9. The electronic device according to claim 5, characterized in that: The Young's modulus of the flexible support plate is greater than the Young's modulus of the flexible film layer.

10. The electronic device according to claim 5 or 9, characterized in that: The Young's modulus of the flexible film layer is in the range of: 5×10^9N / m 2 Up to 10×10^9N / m 2 .

11. The electronic device according to any one of claims 5 to 9, characterized in that: The thermal expansion coefficient of the flexible film layer is in the range of 0.5-5 parts per million per degree Celsius.

12. The electronic device according to claim 11, characterized in that: The surface roughness of the flexible film layer is in the range of 0.1 nm to 1 nm.

13. An electronic device, characterized in that: The electronic device comprises: Hard substrate; A flexible support plate, arranged on the hard substrate; A flexible film layer is attached to the surface of the flexible support plate; The conductive circuit layer is formed on the flexible film layer, and the conductive circuit layer is used to be bound with at least one electronic component.

14. An electronic package, comprising: The packaging shell is provided with a plurality of accommodating cavities, and the packaging shell is in a strip shape; A plurality of electronic devices as described in any one of claims 5 to 13, wherein the electronic devices are arranged in the accommodating cavity.

15. An electronic device, comprising the electronic device according to any one of claims 5 to 13.

Citation Information

Cited By

  • Chip manufacturing method, chip and electronic equipment

    CN119786351A