Bionic ceramic resin composite material and preparation method thereof
By combining hydroxypropyl methylcellulose powder, alumina, nano-zinc oxide and other materials, a bionic ceramic resin composite material with excellent fracture toughness and antibacterial properties is prepared, which solves the problem of fracture toughness and antibacterial properties of traditional ceramic and metal materials. It achieves versatility and simple preparation, and is suitable for dental restoration and other fields.
Patent Information
- Application Number
- CN202410649117.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-23
- Publication Date
- 2024-10-15
AI Technical Summary
Traditional ceramic materials have deficiencies in fracture toughness and antibacterial properties. Metal materials have limited hardness and wear resistance. Resin composites filled with single ceramic particles still have room for improvement in fracture toughness and antibacterial properties, making it difficult to meet the requirements of oral restoration materials. Multifunctional requirements.
Using bionic ceramic resin composite materials, a mixed solution of hydroxypropyl methylcellulose powder, microflake alumina, nano zinc oxide powder, zirconia balls and methanol, deionized water and glacial acetic acid and methacryloyl Oxypropyltrimethoxysilane and methyl methacrylate resin are combined and prepared through ball milling, drying, heat treatment and sintering to form a material with excellent fracture toughness and excellent antibacterial properties.
It achieves the appropriate hardness, excellent fracture toughness and high wear resistance of the material, simplifies the preparation process, reduces costs, and has the ability to flexibly adjust the material ratio, making it suitable for dental restoration and other fields.
Smart Images

Figure CN118766770A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of oral restoration materials, in particular to a bionic ceramic resin composite material and a preparation method thereof. Background Art
[0002] Bionic ceramic resin composite material is a new type of composite material, which combines ceramic particles with resin matrix, through a specific ratio and preparation process, to imitate the performance and structural characteristics of bioceramics; the material has the advantages of superior comprehensive performance, multifunctional performance, simple preparation process and lightweight design; in the bionic ceramic resin composite material, the ceramic particles can be oxide ceramics, nitride ceramics, etc., with the characteristics of high hardness, wear resistance and high temperature stability; these ceramic particles interact with the resin matrix to form a uniformly dispersed composite structure; by optimizing the material ratio and additives, the bionic ceramic resin composite material can be given a variety of functions such as antibacterial properties;
[0003] Traditional ceramic preparation methods have some shortcomings. Traditional ceramic materials usually use dry sintering or wet molding processes, which have long preparation cycles and high energy consumption. In addition, traditional ceramic materials have poor performance in fracture toughness and antibacterial properties, which limits their application range. And the high hardness of traditional ceramics will also cause wear on natural teeth;
[0004] Metal dental restoration materials have advantages in hardness and wear resistance, but they are deficient in fracture toughness and antibacterial properties. Metal materials usually need to go through complex processes such as smelting, casting, and cold working to obtain the desired shape, and the preparation process is complicated. In addition, the aesthetics of metal materials are limited, and the elastic modulus that does not match that of human teeth will cause wear on natural teeth, limiting their application in the field of dental restorations.
[0005] Resin composites filled with single ceramic particles make up for the deficiencies of traditional ceramic and metal materials to a certain extent. However, resin composites filled with single ceramic particles still have limitations in fracture toughness and antibacterial properties. In addition, the preparation process of resin composites filled with single ceramic particles is relatively complicated, and it is necessary to control the uniformity and dispersion of particle filling to ensure the overall performance of the material;
[0006] In terms of bionics, natural shells have a "brick-mud" structure, in which the inorganic calcium carbonate that makes up the shells can be regarded as "bricks" and the organic proteins and polysaccharides in the shells can be regarded as "mud". This constructed microstructure can promote crack deflection, bifurcation, bridging and sheet extraction, blunt cracks, reduce crack tip stress relief and disperse mechanical energy, hinder crack propagation, and achieve material toughening;
[0007] In summary, the traditional ceramic preparation method has deficiencies in fracture toughness and antibacterial properties, metal materials are limited in aesthetics, mechanical properties and antibacterial properties, and resin composites filled with single ceramic particles still have room for improvement in fracture toughness and antibacterial properties. Therefore, it is necessary to develop a bionic ceramic resin composite that can make up for the above deficiencies at the same time. Summary of the invention
[0008] In view of the deficiencies in the prior art, the present invention provides a bionic ceramic resin composite material and a preparation method thereof, which solves the problems of insufficient fracture toughness and antibacterial properties of traditional materials and preparation methods.
[0009] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0010] A bionic ceramic resin composite material is characterized by comprising the following components: 0.5-1 part of hydroxypropyl methylcellulose powder, 4-5 parts of micro-flaky aluminum oxide, 0.5-1 part of nano zinc oxide powder, 0.1-0.3 part of dispersed ceramic agent, 0.5-1 part of zirconium oxide ball, 4-5 parts of a mixed solution of methanol, deionized water and glacial acetic acid, 0.5-1 part of methacryloxypropyltrimethoxysilane, and 4-5 parts of methyl methacrylate resin.
[0011] Furthermore, the mass ratio of methanol, deionized water and glacial acetic acid in the mixed solution is 9:1:1.
[0012] Furthermore, the diameter of the hydroxypropyl methylcellulose powder is 124-178 μm, the diameter of the micro-flaky aluminum oxide sheet is 5 μm-11 μm, the diameter of the nano zinc oxide powder is 10 nm-50 nm, and the diameter of the zirconium oxide ball is 1.0 mm-3.0 mm.
[0013] Furthermore, the methyl methacrylate resin comprises methyl methacrylate and azobisisobutyronitrile powder, and the mass ratio of the methyl methacrylate to azobisisobutyronitrile powder is 199:1 to 49:1. A method for preparing a bionic ceramic resin composite material comprises the following steps:
[0014] S1. Preliminary material mixing: Pour deionized water into a wide-mouth bottle and put it into a constant temperature water bath at 65°C to 75°C, then add hydroxypropyl methylcellulose powder into the wide-mouth bottle and stir evenly, then add micro-flaky alumina and nano zinc oxide powder into the wide-mouth bottle and stir evenly, then add dispersed ceramic particles and stir evenly to obtain a mixed slurry;
[0015] S2, material drying: adding zirconium oxide balls into the wide-mouth bottle, and then fixing the wide-mouth bottle on a ball mill, ball milling, and then pouring the mixed slurry without the zirconium oxide balls into a glass dish and putting it into a drying oven for drying to obtain ceramics;
[0016] S3, skeleton forming: putting the ceramic into a double-roll rolling mill for cumulative rolling to obtain a ceramic body, placing the ceramic body in an oven to dry, then placing the dried ceramic body into a crucible filled with a sufficient amount of micro-flaky aluminum oxide, placing it in a heat treatment furnace, heating it up to remove organic components, cooling it with the furnace after heat preservation, and placing the crucible containing the ceramic body into a muffle furnace for sintering to form a skeleton;
[0017] S4, skeleton modification: adding glacial acetic acid to the mixed solution to adjust the pH of the mixed solution to 4, then adding γ-methacryloxypropyltrimethoxysilane and mixing evenly to obtain a new mixed solution, and then immersing the skeleton in the new mixed solution to obtain a modified skeleton;
[0018] S5. Material composite: immerse the modified skeleton obtained in step S4 in methyl methacrylate resin, and leave it at room temperature for 7 to 14 days. Then, put the modified skeleton and methyl methacrylate resin into an oven for heat preservation, so that the methyl methacrylate monomer is polymerized and cured. Then, heat is increased and kept warm. Then, the skeleton is taken out, and the resin that has not been immersed in the skeleton is removed to obtain a bionic ceramic resin composite material.
[0019] Furthermore, in the S3 step, the dried ceramic is cumulatively rolled using a double-roll rolling mill, so that the micro-flaky aluminum oxide in the mixed powder is flattened and oriented along the rolling direction to obtain a rolled ceramic sheet, the rolled ceramic sheet is folded in half, rolled again, and repeated multiple times to ensure uniform directional arrangement in the aluminum oxide sheet, and the thickness is gradually reduced to 1±0.2 mm. The ceramic sheet is cut into several thin sheets and then stacked on each other. Every 8 to 12 thin sheets are stacked into a new ceramic body. The new ceramic body has a height of 1±0.1 cm. At room temperature, the body is compressed in a direction perpendicular to the rolling direction. The compressive stress is 6 MPa and the holding time is 1 hour to obtain the desired ceramic body.
[0020] Further, in the S3 step, the muffle furnace heating and cooling rates are: heating to 1000°C at 5°C / min, heating to 1200°C at 2°C / min, heating to 1300°C at 1°C / min, keeping warm for 2h, cooling to 1000°C at 2°C / min, and cooling to room temperature at 5°C / min; heating to 1000°C at 5°C / min, heating to 1250°C at 2°C / min, heating to 1450°C at 1°C / min, keeping warm for 2h, cooling to 1000°C at 2°C / min, and cooling to room temperature at 5°C / min; heating to 1000°C at 5°C / min, heating to 1400°C at 2°C / min, heating to 1600°C at 1°C / min, keeping warm for 2h, cooling to 1000°C at 2°C / min, and cooling to room temperature at 5°C / min.
[0021] The present invention provides a bionic ceramic resin composite material and a preparation method thereof, which has the following beneficial effects:
[0022] 1. The present invention uses multi-material composites to make the bionic ceramic resin composite material have suitable hardness, excellent fracture toughness, excellent antibacterial properties and higher wear resistance, which makes the bionic ceramic resin composite material have wide application potential in the field of oral restoration or other fields.
[0023] 2. Compared with metal materials and traditional ceramic preparation methods, the preparation process of the present invention is simpler and does not require complicated cold processing technology, which reduces the preparation cost. In addition, the material ratio and other functional additives can be flexibly adjusted to make it have antibacterial and anti-corrosive properties to meet different needs. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a scanning electron microscope image of the fracture toughness test of Example 1 of the present invention;
[0025] Figure 2 This is a scanning electron microscope image of the fracture toughness test of Example 2 of the present invention;
[0026] Figure 3 This is a scanning electron microscope image of Example 3 of the present invention when a fracture toughness test was performed. DETAILED DESCRIPTION
[0027] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] A bionic ceramic resin composite material comprises the following components: 0.5-1 part of hydroxypropyl methylcellulose powder, 4-5 parts of micro-flaky aluminum oxide, 0.5-1 part of nano zinc oxide powder, 0.1-0.3 part of dispersed ceramic agent, 0.5-1 part of zirconium oxide ball, 4-5 parts of a mixed solution of methanol, deionized water and glacial acetic acid, 0.5-1 part of methacryloxypropyltrimethoxysilane and 4-5 parts of methyl methacrylate resin.
[0029] The mass ratio of methanol, deionized water and glacial acetic acid in the mixed solution is 9:1:1.
[0030] The diameter of hydroxypropyl methylcellulose powder is 124-178um, the diameter of micro-flaky aluminum oxide sheets is 5μm-11μm, the diameter of nano zinc oxide powder is 10nm-50nm, and the diameter of zirconium oxide balls is 1.0mm-3.0mm.
[0031] The methyl methacrylate resin comprises methyl methacrylate and azobisisobutyronitrile powder, and the added mass ratio of the methyl methacrylate to the azobisisobutyronitrile powder is 199:1 to 49:1.
[0032] A method for preparing a bionic ceramic resin composite material comprises the following steps:
[0033] S1. Preliminary material mixing: Pour deionized water into a wide-mouth bottle and put it into a constant temperature water bath at 65°C to 75°C, then add hydroxypropyl methylcellulose powder into the wide-mouth bottle, use a glass rod to stir at 30r / min for 2min to make it uniform, then add micro-flaky alumina and nano zinc oxide powder into the wide-mouth bottle, use a glass rod to stir at 30r / min for 2min to 5min to make it uniform, add dispersed ceramic particles, and use a glass rod to stir at 30r / min for 15min to 18min to make a mixed slurry;
[0034] S2. Material drying: Add zirconia balls into the wide-mouth bottle, fix the wide-mouth bottle on a ball mill, and mill at 15 r / min for 48 hours. Pour the mixed slurry without the zirconia balls into a glass dish and put it into a drying oven at 40°C to 60°C for 34min to 43min to obtain ceramics.
[0035] S3, skeleton forming: putting the ceramic into a double-roll rolling mill for cumulative rolling to obtain a ceramic body, placing the ceramic body in a 40°C-60°C oven for drying for 24 hours, then placing the dried ceramic body into a crucible filled with a sufficient amount of micro-flaky alumina, placing it in a heat treatment furnace, heating it to 550°C-650°C at 2°C / min to remove organic components, keeping it warm for 3 hours and cooling it with the furnace, placing the crucible containing the ceramic body into a muffle furnace for sintering to form a skeleton;
[0036] S4, skeleton modification: adding glacial acetic acid to the mixed solution to adjust the pH of the mixed solution to 4, then adding γ-methacryloxypropyltrimethoxysilane and mixing evenly to obtain a new mixed solution, and then soaking the skeleton in the new mixed solution for 20 hours to 28 hours to obtain a modified skeleton;
[0037] S5. Material composite: immerse the modified skeleton obtained in step S4 in methyl methacrylate resin, and leave it at room temperature for 7 to 14 days. Then, send the modified skeleton and methyl methacrylate resin into a 40°C to 45°C oven and keep it warm for 20h to 28h to polymerize and solidify the methyl methacrylate monomer. Then, raise the temperature to 90°C and keep it warm for 2h to 3h. Then, take out the skeleton, remove the resin that has not been immersed in the skeleton, and obtain a bionic ceramic resin composite material.
[0038] In step S3, the dried ceramic is cumulatively rolled using a double-roll rolling mill to orient the micro-flaky aluminum oxide in the mixed powder along the rolling direction to obtain a rolled ceramic sheet. The rolled ceramic sheet is folded in half and rolled again. This process is repeated multiple times to ensure uniform orientation in the aluminum oxide sheet. The thickness of the ceramic sheet is gradually reduced to 1±0.2 mm. The ceramic sheet is cut into several thin sheets and then stacked on each other. Every 8 to 12 thin sheets are stacked into a new ceramic body. The new ceramic body has a height of 1±0.1 cm. At room temperature, the body is compressed in a direction perpendicular to the rolling direction. The compressive stress is 6 MPa and the holding time is 1 hour to obtain the desired ceramic body.
[0039] In step S3, the heating and cooling rates of the muffle furnace are as follows: heating to 1000°C at 5°C / min, heating to 1200°C at 2°C / min, heating to 1300°C at 1°C / min, keeping warm for 2h, cooling to 1000°C at 2°C / min, and cooling to room temperature at 5°C / min; heating to 1000°C at 5°C / min, heating to 1250°C at 2°C / min, heating to 1450°C at 1°C / min, and keeping warm for 2h, cooling to 1000°C at 2°C / min, and cooling to room temperature at 5°C / min; heating to 1000°C at 5°C / min, heating to 1400°C at 2°C / min, heating to 1600°C at 1°C / min, and keeping warm for 2h, cooling to 1000°C at 2°C / min, and cooling to room temperature at 5°C / min.
[0040] In the step S4:
[0041] The chemical reaction formula of the mixed solution and glacial acetic acid is:
[0042] CH3COOH+CH3OH→CH3COOCH3+H2O;
[0043] Among them, CH3COOH is acetic acid, CH3OH is methanol, and the formula is the esterification reaction produced by the two.
[0044] The chemical reaction formula produced by the mixed solution and γ-methacryloxypropyltrimethoxysilane is:
[0045] γ-MPS+H2O→γ-MPS-OH+CH3Si(OH)3;
[0046] Among them, γ-MPS represents γ-methacryloxypropyltrimethoxysilane, which is a silane coupling agent, MPS-OH represents the hydroxyl-containing γ-MPS product formed by the reaction of γ-MPS with hydroxyl groups in water, and CH3Si(OH)3 represents methyltrihydroxysilane, which reflects the compound of silane combined with hydroxyl groups in water.
[0047] In the step S5, the reaction formula for the polymerization and curing of methyl methacrylate monomer is:
[0048] nMMA→[-MMA-]n;
[0049] Here n represents the number of repeating units in the polymer, i.e., the degree of polymerization, MMA represents methyl methacrylate, and [-MMA-] represents the structural unit of the polymer chain, wherein [-MMA-]n represents a polymer chain composed of n MMA monomers, and n represents the number of repeating units in the polymer chain or the degree of polymerization.
[0050] Example 1: Bionic ceramic resin composite material example 1
[0051] Prepare materials: including the following components: 0.5 parts of hydroxypropyl methylcellulose powder, 4 parts of flaky aluminum oxide with a diameter of 5μm to 11μm, 0.5 parts of nano zinc oxide powder with a diameter of 10nm to 50nm, 0.1 parts of dispersed ceramic particles, 0.5 parts of zirconium oxide balls with a diameter of 1.0mm to 3.0mm, 4 parts of a mixed solution including methanol, deionized water, and glacial acetic acid, 0.5 parts of methacryloxypropyltrimethoxysilane, and 4 parts of methyl methacrylate resin.
[0052] step:
[0053] S1. Preliminary material mixing: Pour deionized water into a wide-mouth bottle and put it into a constant temperature water bath at 65°C to 75°C, then add hydroxypropyl methylcellulose powder into the wide-mouth bottle and stir it at 30r / min for 2min using a glass rod, then add micro-flaky alumina with a diameter of 5μm to 11μm and nano zinc oxide powder with a diameter of 10nm to 50nm into the wide-mouth bottle and stir them at 30r / min for 2min to 5min using a glass rod, add dispersed ceramic particles and stir them at 30r / min for 15min to 18min to obtain a mixed slurry;
[0054] S2, material drying: 1.0mm-3.0mm zirconia balls are added into a wide-mouth bottle, and then the wide-mouth bottle is fixed on a ball mill, and ball milled at 15r / min for 48h, and then the mixed slurry without the zirconia balls is poured into a glass dish and placed in a drying oven at 40℃-60℃ for 34min-43min to obtain ceramics;
[0055] S3, skeleton forming: putting the ceramic into a double-roll rolling mill for cumulative rolling to obtain a ceramic body, placing the ceramic body in a 40°C-60°C oven for drying for 24 hours, then placing the dried ceramic body into a crucible filled with a sufficient amount of micro-flaky alumina, placing it in a heat treatment furnace, heating it to 550°C-650°C at 2°C / min to remove organic components, keeping it warm for 3 hours and then cooling it with the furnace, finally placing the crucible containing the ceramic body into a muffle furnace for sintering to form a skeleton;
[0056] S4, skeleton modification: adding glacial acetic acid to the mixed solution to adjust the pH of the mixed solution to 4, then adding γ-methacryloxypropyltrimethoxysilane and mixing evenly to obtain a new mixed solution, and then soaking the skeleton in the new mixed solution for 20 hours to 28 hours to obtain a modified skeleton;
[0057] S5. Material composite: immerse the modified skeleton obtained in step S4 in methyl methacrylate resin, and leave it at room temperature for 7 to 14 days. Then, send the modified skeleton and methyl methacrylate resin into a 40°C to 45°C oven and keep it warm for 20h to 28h to polymerize and solidify the methyl methacrylate monomer. Then, raise the temperature to 90°C and keep it warm for 2h to 3h. Then, take out the skeleton, remove the resin that has not been immersed in the skeleton, and obtain a bionic ceramic resin composite material.
[0058] Figure 1 This is a scanning electron microscope image of the fracture toughness test of Example 1. There is a zigzag deflection of the crack in the image, which will dissipate the energy of the crack expansion, extend the expansion path, and increase the toughness of the ceramic.
[0059] Example 2: Bionic ceramic resin composite material example 2
[0060] Prepare materials: including the following components: 0.8 parts of hydroxypropyl methylcellulose powder, 4 parts of flaky aluminum oxide with a diameter of 5μm to 11μm, 0.8 parts of nano zinc oxide powder with a diameter of 10nm to 50nm, 0.3 parts of dispersed ceramic particles, 1 part of zirconium oxide balls with a diameter of 1.0mm to 3.0mm, 4 parts of a mixed solution including methanol, deionized water, and glacial acetic acid, 1 part of methacryloxypropyltrimethoxysilane, and 5 parts of methyl methacrylate resin.
[0061] step:
[0062] S1. Preliminary material mixing: Pour deionized water into a wide-mouth bottle and put it into a constant temperature water bath at 65°C to 75°C, then add hydroxypropyl methylcellulose powder into the wide-mouth bottle and stir it at 30r / min for 2min using a glass rod, then add micro-flaky alumina with a diameter of 5μm to 11μm and nano zinc oxide powder with a diameter of 10nm to 50nm into the wide-mouth bottle and stir them at 30r / min for 2min to 5min using a glass rod, add dispersed ceramic particles and stir them at 30r / min for 15min to 18min to obtain a mixed slurry;
[0063] S2, material drying: 1.0mm-3.0mm zirconia balls are added into a wide-mouth bottle, and then the wide-mouth bottle is fixed on a ball mill, and ball milled at 15r / min for 48h, and then the mixed slurry without the zirconia balls is poured into a glass dish and placed in a drying oven at 40℃-60℃ for 34min-43min to obtain ceramics;
[0064] S3, skeleton forming: putting the ceramic into a double-roll rolling mill for cumulative rolling to obtain a ceramic body, placing the ceramic body in a 40°C-60°C oven for drying for 24 hours, then placing the dried ceramic body into a crucible filled with a sufficient amount of micro-flaky alumina, placing it in a heat treatment furnace, heating it to 550°C-650°C at 2°C / min to remove organic components, keeping it warm for 3 hours and then cooling it with the furnace, finally placing the crucible containing the ceramic body into a muffle furnace for sintering to form a skeleton;
[0065] S4, skeleton modification: adding glacial acetic acid to the mixed solution to adjust the pH of the mixed solution to 4, then adding γ-methacryloxypropyltrimethoxysilane and mixing evenly to obtain a new mixed solution, and then soaking the skeleton in the new mixed solution for 20 hours to 28 hours to obtain a modified skeleton;
[0066] S5. Material composite: immerse the modified skeleton obtained in step S4 in methyl methacrylate resin, and leave it at room temperature for 7 to 14 days. Then, send the modified skeleton and methyl methacrylate resin into a 40°C to 45°C oven and keep it warm for 20h to 28h to polymerize and solidify the methyl methacrylate monomer. Then, raise the temperature to 90°C and keep it warm for 2h to 3h. Then, take out the skeleton, remove the resin that has not been immersed in the skeleton, and obtain a bionic ceramic resin composite material.
[0067] Figure 2 This is a scanning electron microscope image of the fracture toughness test of Example 2. The image shows crack bifurcation and sheet pullout during the fracture process. The artificial 'mud-brick' structure that imitates the natural structure of shells enhances the fracture toughness and bending strength of the composite material.
[0068] Example 3: Bionic ceramic resin composite material example 3
[0069] Prepare materials: including the following components: 1 part of hydroxypropyl methylcellulose powder, 5 parts of flaky aluminum oxide with a diameter of 5μm to 11μm, 1 part of nano zinc oxide powder with a diameter of 10nm to 50nm, 0.3 parts of dispersed ceramic particles, 1 part of zirconium oxide balls with a diameter of 1.0mm to 3.0mm, 5 parts of a mixed solution including methanol, deionized water, and glacial acetic acid, 1 part of methacryloxypropyltrimethoxysilane, and 5 parts of methyl methacrylate resin.
[0070] step:
[0071] S1. Preliminary material mixing: Pour deionized water into a wide-mouth bottle and put it into a constant temperature water bath at 65°C to 75°C, then add hydroxypropyl methylcellulose powder into the wide-mouth bottle and stir it at 30r / min for 2min using a glass rod, then add micro-flaky alumina with a diameter of 5μm to 11μm and nano zinc oxide powder with a diameter of 10nm to 50nm into the wide-mouth bottle and stir them at 30r / min for 2min to 5min using a glass rod, add dispersed ceramic particles and stir them at 30r / min for 15min to 18min to obtain a mixed slurry;
[0072] S2, material drying: 1.0mm-3.0mm zirconia balls are added into a wide-mouth bottle, and then the wide-mouth bottle is fixed on a ball mill, and ball milled at 15r / min for 48h, and then the mixed slurry without the zirconia balls is poured into a glass dish and placed in a drying oven at 40℃-60℃ for 34min-43min to obtain ceramics;
[0073] S3, skeleton forming: putting the ceramic into a double-roll rolling mill for cumulative rolling to obtain a ceramic body, placing the ceramic body in a 40°C-60°C oven for drying for 24 hours, then placing the dried ceramic body into a crucible filled with a sufficient amount of micro-flaky alumina, placing it in a heat treatment furnace, heating it to 550°C-650°C at 2°C / min to remove organic components, keeping it warm for 3 hours and then cooling it with the furnace, finally placing the crucible containing the ceramic body into a muffle furnace for sintering to form a skeleton;
[0074] S4, skeleton modification: adding glacial acetic acid to the mixed solution to adjust the pH of the mixed solution to 4, then adding γ-methacryloxypropyltrimethoxysilane and mixing evenly to obtain a new mixed solution, and then soaking the skeleton in the new mixed solution for 20 hours to 28 hours to obtain a modified skeleton;
[0075] S5. Material composite: immerse the modified skeleton obtained in step S4 in methyl methacrylate resin, and leave it at room temperature for 7 to 14 days. Then, send the modified skeleton and methyl methacrylate resin into a 40°C to 45°C oven and keep it warm for 20h to 28h to polymerize and solidify the methyl methacrylate monomer. Then, raise the temperature to 90°C and keep it warm for 2h to 3h. Then, take out the skeleton, remove the resin that has not been immersed in the skeleton, and obtain a bionic ceramic resin composite material.
[0076] Summary: Through the above three examples, we can prepare bionic ceramic resin composite materials with similar properties by adjusting the material ratio. These examples demonstrate the flexibility of bionic ceramic resin composite materials, and the appropriate preparation method can be selected according to specific needs.
[0077] Figure 3This is a scanning electron microscope image of the fracture toughness test of Example 3. As shown in the image, during the fracture process, the inorganic part of the alumina and the organic resin structure in the ceramic break into step-like cracks, dissipating the fracture energy and effectively increasing the fracture toughness of the material.
[0078] Test experiment 1: Performance test of bionic ceramic resin composite material example 1
[0079] Test objectives: Test the hardness and fracture toughness of bionic ceramic resin composite material example 1, focusing on its ability to resist unstable crack propagation in a plane state, i.e. K IC Value; antibacterial properties.
[0080] Test process:
[0081] a. Prepare samples: sample 1 of biomimetic ceramic resin composite material;
[0082] b. Test hardness: Use MH-5L microhardness tester to test the hardness of the sample. According to the normal operation, place the sample on the hardness tester, apply a load of 1kgf, hold the load for 15s, and measure the hardness value of the sample;
[0083] c. K IC Value test: Use ASTME1820-18 standard to test the K value of the sample. IC The value test is carried out to evaluate its plane strain fracture toughness; the loading force is adjusted to 1N, the test displacement rate is 3μm / min, the load loading direction is perpendicular to the layer direction, and the scanning electron microscope monitors the crack extension length in real time, and records the corresponding load and displacement at the same time;
[0084] d. Antibacterial test: Use the standard antibacterial test, i.e., plate count method, to evaluate the antibacterial properties of the samples. Incubate the bacteria on the samples for 24 hours, observe the growth of the bacteria, and calculate the antibacterial rate;
[0085] e. Record data: record the hardness, fracture toughness and antibacterial properties of each sample.
[0086] Experimental data and test results:
[0087]
[0088]
[0089] According to the test results, the hardness of the sample of Example 1 of the bionic ceramic resin composite material is adapted to natural teeth, which will reduce their wear; it has excellent fracture toughness and can effectively prevent breakage during use; and it has antibacterial properties that general materials do not have.
[0090] Test experiment 2: Performance test of bionic ceramic resin composite material example 2
[0091] Test objectives: Test the hardness performance of bionic ceramic resin composite material Example 2; fracture toughness, focusing on its ability to resist unstable crack propagation in a planar state, namely, KIC value; antibacterial properties.
[0092] Test process:
[0093] a. Prepare samples: sample 2 of biomimetic ceramic resin composite material;
[0094] b. Test hardness: Use MH-5L microhardness tester to test the hardness of the sample. According to the normal operation, place the sample on the hardness tester, apply a load of 1kgf, hold the load for 15s, and measure the hardness value of the sample;
[0095] c. KIC value test: Use ASTME1820-18 standard to test the KIC value of the sample to evaluate its plane strain fracture toughness; the load force is adjusted to 1N, the test displacement rate is 3μm / min, the load direction is perpendicular to the layer direction, and the scanning electron microscope monitors the crack extension length in real time, and records the corresponding load and displacement at the same time;
[0096] d. Antibacterial test: Use the standard antibacterial test, i.e., plate count method, to evaluate the antibacterial properties of the samples. Incubate the bacteria on the samples for 24 hours, observe the growth of the bacteria, and calculate the antibacterial rate;
[0097] e. Record data: record the hardness, fracture toughness and antibacterial properties of each sample.
[0098] Experimental data and test results:
[0099]
[0100] According to the test results, the hardness of bionic ceramic resin composite material Example 2 is adapted to natural teeth and will reduce their wear; its fracture toughness is higher than other materials; and it has antibacterial properties that general materials do not have.
[0101] Test experiment 3: Performance test of bionic ceramic resin composite material example 3
[0102] Test objectives: Test the hardness performance of bionic ceramic resin composite material Example 3; fracture toughness, focusing on its ability to resist unstable crack propagation in a planar state, namely, KIC value; antibacterial properties.
[0103] Test process:
[0104] a. Prepare samples: sample 3 of biomimetic ceramic resin composite material;
[0105] b. Test hardness: Use MH-5L microhardness tester to test the hardness of the sample. According to the normal operation, place the sample on the hardness tester, apply a load of 1kgf, hold the load for 15s, and measure the hardness value of the sample;
[0106] c. KIC value test: Use ASTME1820-18 standard to test the KIC value of the sample to evaluate its plane strain fracture toughness; the load force is adjusted to 1N, the test displacement rate is 3μm / min, the load direction is perpendicular to the layer direction, and the scanning electron microscope monitors the crack extension length in real time, and records the corresponding load and displacement at the same time;
[0107] d. Antibacterial test: Use the standard antibacterial test, i.e., plate count method, to evaluate the antibacterial properties of the samples. Incubate the bacteria on the samples for 24 hours, observe the growth of the bacteria, and calculate the antibacterial rate;
[0108] e. Record data: record the hardness, fracture toughness and antibacterial properties of each sample.
[0109] Experimental data and test results:
[0110]
[0111] According to the test results, the hardness of bionic ceramic resin composite material Example 3 is adapted to natural teeth and will reduce their wear; its fracture toughness is higher than other materials; and it has antibacterial properties that general materials do not have.
[0112] Obviously, the above-mentioned embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the embodiments of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made on the basis of the above description. It is impossible to list all the embodiments here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A bionic ceramic resin composite material, characterized in that: The invention comprises the following components: 0.5-1 part of hydroxypropyl methylcellulose powder, 4-5 parts of micro-flaky aluminum oxide, 0.5-1 part of nano zinc oxide powder, 0.1-0.3 part of dispersed ceramic agent, 0.5-1 part of zirconium oxide ball, 4-5 parts of a mixed solution of methanol, deionized water and glacial acetic acid, 0.5-1 part of methacryloxypropyltrimethoxysilane and 4-5 parts of methyl methacrylate resin.
2. The bionic ceramic resin composite material according to claim 1, characterized in that: The mass ratio of methanol, deionized water and glacial acetic acid in the mixed solution is 9:1:
1.
3. The bionic ceramic resin composite material according to claim 1, characterized in that: The diameter of the hydroxypropyl methylcellulose powder is 124-178 μm, the diameter of the micro-flaky aluminum oxide sheet is 5 μm-11 μm, the diameter of the nano zinc oxide powder is 10 nm-50 nm, and the diameter of the zirconium oxide ball is 1.0 mm-3.0 mm.
4. The bionic ceramic resin composite material according to claim 1, characterized in that: The methyl methacrylate resin comprises methyl methacrylate and azobisisobutyronitrile powder, and the added mass ratio of the methyl methacrylate to the azobisisobutyronitrile powder is 199:1 to 49:
1.
5. The method for preparing a bionic ceramic resin composite material according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Preliminary material mixing: Pour deionized water into a wide-mouth bottle and put it into a constant temperature water bath at 65°C to 75°C, then add hydroxypropyl methylcellulose powder into the wide-mouth bottle and stir evenly, then add micro-flaky alumina and nano zinc oxide powder into the wide-mouth bottle and stir evenly, then add dispersed ceramic particles and stir evenly to obtain a mixed slurry; S2, material drying: adding zirconium oxide balls into the wide-mouth bottle, and then fixing the wide-mouth bottle on a ball mill, ball milling, and then pouring the mixed slurry without the zirconium oxide balls into a glass dish and putting it into a drying oven for drying to obtain ceramics; S3, skeleton forming: putting the ceramic into a double-roll rolling mill for cumulative rolling to obtain a ceramic body, placing the ceramic body in an oven to dry, then placing the dried ceramic body into a crucible filled with a sufficient amount of micro-flaky aluminum oxide, placing it in a heat treatment furnace, heating it up to remove organic components, cooling it with the furnace after heat preservation, and placing the crucible containing the ceramic body into a muffle furnace for sintering to form a skeleton; S4, skeleton modification: adding glacial acetic acid to the mixed solution to adjust the pH of the mixed solution to 4, then adding γ-methacryloxypropyltrimethoxysilane and mixing evenly to obtain a new mixed solution, and then immersing the skeleton in the new mixed solution to obtain a modified skeleton; S5. Material composite: immerse the modified skeleton obtained in step S4 in methyl methacrylate resin, and leave it at room temperature for 7 to 14 days. Then, put the modified skeleton and methyl methacrylate resin into an oven for heat preservation, so that the methyl methacrylate monomer is polymerized and cured. Then, heat is increased and kept warm. Then, the skeleton is taken out, and the resin that has not been immersed in the skeleton is removed to obtain a bionic ceramic resin composite material.
6. The method for preparing a bionic ceramic resin composite material according to claim 5, characterized in that: In the S3 step, the dried ceramic is cumulatively rolled using a double-roll rolling mill, so that the micro-flaky aluminum oxide in the mixed powder is flattened and oriented along the rolling direction to obtain a rolled ceramic sheet, the rolled ceramic sheet is folded in half, rolled again, and the process is repeated multiple times to ensure uniform directional arrangement in the aluminum oxide sheet, and the thickness of the ceramic sheet is gradually reduced to 1±0.2 mm. The ceramic sheet is cut into several thin sheets, which are then stacked on each other, with every 8 to 12 thin sheets stacked into a new ceramic body, the new ceramic body having a height of 1±0.1 cm, and at room temperature, the body is compressed in a direction perpendicular to the rolling direction, the compressive stress is 6 MPa, and the holding time is 1 hour to obtain the desired ceramic body.
7. The method for preparing a bionic ceramic resin composite material according to claim 5, characterized in that: In the step S3, the heating and cooling rates of the muffle furnace are: heating to 1000°C at 5°C / min, heating to 1200°C at 2°C / min, heating to 1300°C at 1°C / min, keeping warm for 2h, cooling to 1000°C at 2°C / min, and cooling to room temperature at 5°C / min; heating to 1000°C at 5°C / min, heating to 1250°C at 2°C / min, heating to 1450°C at 1°C / min, keeping warm for 2h, cooling to 1000°C at 2°C / min, and cooling to room temperature at 5°C / min; heating to 1000°C at 5°C / min, heating to 1400°C at 2°C / min, heating to 1600°C at 1°C / min, keeping warm for 2h, cooling to 1000°C at 2°C / min, and cooling to room temperature at 5°C / min.
Citation Information
Cited By
Honeycomb ceramic and preparation method thereof
CN120081678A
A honeycomb ceramic and method of making the same
CN120081678B