Artificial blood vessel as well as preparation method and application thereof

By using a double-layer artificial blood vessel, combined with diselenium-based polyurethane and a support ring, and coated with an anticoagulant layer, the problems of thrombus and leakage during hemodialysis are solved, achieving efficient anticoagulation and anti-proliferation effects, and improving blood vessel health. long-term patency and regeneration capacity.

CN118767210APending Publication Date: 2024-10-15ZHUHAI INST OF ADVANCED TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411011717.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing artificial blood vessels are difficult to avoid thrombosis, vascular stenosis and leakage during hemodialysis, and they lack sufficient anticoagulation and anti-proliferation capabilities, resulting in low long-term patency.

Method used

The artificial blood vessel adopts a double-layer structure, in which the outer layer provides support strength, and the inner layer is composed of diselenium-based polyurethane and a support ring. The anticoagulant layer contains heparin salt to promote endothelial cell maturation and vascular regeneration, and prevent thrombus and leakage.

Benefits of technology

It significantly reduces the risk of thrombosis, increases the long-term patency of blood vessels, prevents leakage after blood vessel puncture, promotes blood vessel regeneration, and improves the mechanical properties and biocompatibility of blood vessels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004964561460000011
    Figure HDA0004964561460000011
  • Figure HDA0004964561460000012
    Figure HDA0004964561460000012
  • Figure HDA0004964561460000021
    Figure HDA0004964561460000021
Patent Text Reader

Abstract

The invention belongs to the technical field of biomedical materials, and provides an artificial blood vessel and a preparation method and application thereof. The artificial blood vessel comprises a vessel wall and a vessel cavity, the vessel wall comprises an outer layer and an inner layer, the inner layer comprises a base body and a supporting ring embedded in the base body, the base body is diselenyl polyurethane, the artificial blood vessel is coated with an anticoagulant layer, and the anticoagulant layer contains heparin. The outer layer can provide enough supporting strength, the high-elasticity inner layer has the effects of preventing leakage and resisting hyperplasia, the supporting ring provides strength, the mechanical property of the blood vessel is guaranteed, the artificial blood vessel has radial supporting performance, and meanwhile fatigue caused by excessive stretching of diselenyl polyurethane of the inner layer is prevented. The artificial blood vessel contains an anticoagulation layer, and has high biocompatibility and long-acting anticoagulation capability. The blood vessel is further used as a blood vessel special for dialysis, the thrombus risk in vivo is reduced, the long-term patency rate of the blood vessel is increased, leakage after blood vessel puncture is prevented, and blood vessel regeneration is accelerated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of biomedical materials, and more specifically, to an artificial blood vessel and a preparation method and application thereof. Background Art

[0002] Chronic kidney disease (CKD) is a major disease that threatens human health worldwide. Hemodialysis (HD) is an important means of treating CKD, and about 90% of patients choose hemodialysis treatment.

[0003] Hemodialysis is one of the renal replacement therapies for patients with acute and chronic renal failure. It drains blood from the body to the outside of the body through a dialyzer composed of countless hollow fibers. The blood and the electrolyte solution (dialysate) containing similar concentrations to the body are exchanged inside and outside the hollow fibers through diffusion, ultrafiltration, adsorption and convection principles to remove metabolic waste from the body, maintain electrolyte and acid-base balance, and remove excess water from the body. The entire process of returning the purified blood is called hemodialysis. During the dialysis operation, the blood vessels need to be punctured to guide the blood to the outside of the body for purification. The frequency of dialysis is generally 2-3 times a week, which means that the blood vessels must withstand repeated punctures. In order to reduce the damage to the blood vessels caused by repeated punctures and ensure the blood flow in the vascular pathway, constructing an arteriovenous fistula is currently the preferred method of hemodialysis.

[0004] The current artificial blood vessels are only suitable for replacing large-sized blood vessels, and there is a lack of blood vessels dedicated to dialysis. Unlike artificial blood vessels for replacement, blood vessels for dialysis are not only required to have good anti-coagulation and anti-proliferation capabilities, but also require the blood vessels to be able to quickly endothelialize and avoid leakage after multiple punctures, which puts higher requirements on the elasticity and biological properties of the blood vessels. Therefore, in response to the current demand for artificial blood vessels dedicated to dialysis, it is urgent to construct an artificial blood vessel that is anti-coagulation, anti-proliferation, highly elastic, can quickly endothelialize, and avoids leakage after multiple punctures. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides an artificial blood vessel and a preparation method and application thereof. The artificial blood vessel provided by the present invention can be used as an artificial blood vessel dedicated to dialysis, combines multiple functions of anticoagulation, antiproliferation and anti-inflammatory, avoids the formation of thrombus, prevents the occurrence of restenosis of blood vessels, and has high elasticity, ensures the anti-leakage performance of blood vessels, and can quickly endothelialize.

[0006] A first aspect of the present invention provides an artificial blood vessel.

[0007] Specifically, an artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, and the artificial blood vessel is coated with an anticoagulant layer, wherein the raw material components of the anticoagulant layer comprise an anticoagulant component, and the anticoagulant component comprises heparin salt.

[0008] The artificial blood vessel provided by the present invention has a double-layer structure, wherein the outer layer can provide sufficient support strength for the artificial blood vessel, and the inner layer plays a role of preventing leakage and anti-proliferation, and also has high elasticity, and the support ring buried in the inner layer can provide sufficient strength for the artificial blood vessel, ensure the mechanical properties of the blood vessel, so that the artificial blood vessel has radial support, and prevent the inner layer of the diselenide polyurethane elastic material from fatigue due to excessive stretching. In addition, the entire surface of the artificial blood vessel is also coated with an anticoagulant layer containing heparin salt, giving the artificial blood vessel a long-term anticoagulant ability. The outer layer and the inner layer jointly ensure that the artificial blood vessel has good mechanical properties. The artificial blood vessel provided by the present invention can also accelerate the maturation of blood vessels. In summary, the artificial blood vessel provided by the present invention can be further used as a dedicated blood vessel for dialysis. Usually, after the construction of an arteriovenous fistula, blood flows rapidly through the blood vessel and contacts the inner wall of the blood vessel, resulting in platelet activation and thus thrombosis, and the damage caused by the operation aggravates the occurrence of thrombosis; in addition, during the service of the artificial blood vessel, the body's immune mechanism causes chronic inflammation at the implantation site, causing stenosis of the blood vessel, which is also the reason why the long-term patency rate of the current artificial blood vessel is not high. After the artificial blood vessel of the present invention is implanted, blood flows through the artificial blood vessel, and the artificial blood vessel expands rapidly. The outer layer and the support ring ensure that the artificial blood vessel does not expand too much and cause fatigue of the diselenide polyurethane material; and the outer surface of the artificial blood vessel also has an anticoagulant layer with an anticoagulant effect to prevent the generation of thrombus; the diselenide on the inner layer of the diselenide polyurethane can react with the NO donor in the body to generate NO to regulate endothelial cells and smooth muscle cells, promote endothelial cell migration, accelerate vascular maturation, and prevent cell proliferation; at the same time, the high elasticity of the diselenide polyurethane can prevent the blood vessel from leaking after multiple punctures. The artificial blood vessel provided by the present invention reduces the risk of thrombosis in the body, increases the long-term patency of the blood vessel, and prevents leakage after blood vessel puncture. At the same time, blood cells are regulated, which can further accelerate the regeneration of blood vessels and prevent the occurrence of complications.

[0009] Preferably, the material of the outer layer is at least one of polytetrafluoroethylene, polyethylene terephthalate, and polyamide.

[0010] Preferably, the raw materials for preparing the diselenyl polyurethane include: a diol compound, a diisocyanate compound, a selenium-containing chain extender and a catalyst.

[0011] Preferably, the molar fraction of the catalyst in the raw materials for preparing the diselenyl polyurethane is 0.1-10%, that is, the amount of the catalyst accounts for 0.1-10 mol% of the total amount of the diol compound, the diisocyanate compound, the selenium-containing chain extender and the catalyst.

[0012] Preferably, the molar ratio of the diol compound, the diisocyanate compound and the chain extender is 1:2:(1-10).

[0013] More preferably, the molar ratio of the diol compound, the diisocyanate compound and the chain extender is 1:2:(1-5).

[0014] More preferably, the molar ratio of the diol compound, the diisocyanate compound and the chain extender is 1:2:1, 1:2:1.1, 1:2:1.3, 1:2:1.5, 1:2:2, 1:2:2.5, 1:2:3, 1:2:3.5, 1:2:4 or 1:2:5.

[0015] Preferably, the diol compound is at least one of dihydroxy organic small molecules, polyethylene glycol, polycaprolactone, and polyether.

[0016] Further preferably, the diol compound is at least one of ethylene glycol, 1,4-butanediol, resorcinol, hydroquinone dihydroxyethyl ether, polyethylene, polypropylene, polysulfone, polyethylene glycol-400, polyethylene glycol-1000, polyethylene glycol-2000, polyethylene glycol-5000, polylactide, polycaprolactone, polyethylene glycol-b-polycaprolactone, and polyethylene glycol-b-polylactide.

[0017] Preferably, the diisocyanate compound is an aliphatic diisocyanate compound and / or an alicyclic diisocyanate compound.

[0018] Further preferably, the diisocyanate compound is at least one of toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), dicyclohexylmethane diisocyanate (HMDI), hexamethylene diisocyanate (HDI), and lysine diisocyanate (LDI).

[0019] Preferably, the selenium-containing chain extender is a selenocystamine chain extender and / or a diselenide bond-containing chain extender.

[0020] More preferably, the selenium-containing chain extender is at least one of selenocystamine, bis(hydroxymethyl) diselenide, bis(hydroxyethyl) diselenide, and bis(aminoethyl) diselenide.

[0021] Preferably, the raw materials for preparing the diselenyl polyurethane further include: an alkane diol chain extender and / or an alkane diamine chain extender.

[0022] Preferably, the alkane diol chain extender is at least one of ethylene glycol (EG), 1,4-butanediol (BDO), hydroquinone dihydroxyethyl ether (HQEE), and resorcinol dihydroxyethyl ether.

[0023] Preferably, the alkane diamine chain extender is at least one of 3,3'-dichloro-4,4'-diaminophenylmethane (MOCA), diethyltoluenediamine (DETDA), 4,4'-methylene-bis(3-chloro-2,6-diethylaniline) (MCDEA), and bis-sec-butylaminodiphenylmethane (MDBA).

[0024] Preferably, the catalyst is at least one of an organic tin catalyst, an organic mercury catalyst, an organic lead catalyst, an organic zinc catalyst, N,N-dimethylcyclohexylamine, N-ethylmorpholine, triethanolamine, and pyridine.

[0025] Further preferably, the catalyst is at least one of stannous octoate, DY-5 (pentamethyldiethylenetriamine), DY-8 (dimethylcyclohexylamine), DY-12 (dibutyltin dilaurate), DY-20 (organic bismuth), DY-41 (triazine trimer), N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl) ether, N,N,N',N'-tetramethylalkylenediamine, triethylamine, N,N-dimethylbenzylamine, solid amine, N-ethylmorpholine, N-methylmorpholine, N,N'-diethylpiperazine, triethanolamine, DMEA, pyridine, and N,N'-lutidine.

[0026] Preferably, the weight average molecular weight of the diselenyl polyurethane is 10000-1000000 Da.

[0027] Preferably, the raw material components of the anticoagulant layer include anticoagulant components in an amount of 1% to 50% by mass.

[0028] Further preferably, the raw material components of the anticoagulant layer include an anticoagulant component with a mass fraction of 5%-30%.

[0029] More preferably, the raw material components of the anticoagulant layer include 10%-20% by mass of anticoagulant ingredients.

[0030] More preferably, the raw material components of the anticoagulant layer include anticoagulant components in a mass fraction of 5%, 8%, 10%, 15%, 18% or 20%.

[0031] Preferably, the heparin salt is at least one of heparin sodium, heparin potassium and heparin calcium.

[0032] Preferably, the anticoagulant component also includes at least one of warfarin sodium, Plavix, and Coumarin-6.

[0033] Preferably, the raw material components of the anticoagulation layer also include biocompatible materials.

[0034] Preferably, the biocompatible material is at least one of amino acid polymers, polyphenol polymers, polysaccharide polymers, polyethylene glycol, polyester, polyurethane, and polysulfone.

[0035] Further preferably, the biocompatible material is at least one of gelatin, collagen, polyphenol, polylysine, polydopamine, sodium hyaluronate, bovine glycerin, cellulose, lignin, polysulfone, polyurethane, polyethylene glycol, polyvinyl pyrrolidone, and polyvinyl alcohol. The above biocompatible material can fix the anticoagulant component to the artificial blood vessel.

[0036] Preferably, the thickness of the tube wall is 0.05-0.3 mm.

[0037] Further preferably, the thickness of the tube wall is 0.1-0.2 mm.

[0038] More preferably, the thickness of the tube wall is 0.1 mm, 0.11 mm, 0.12 mm, 0.15 mm or 0.17 mm.

[0039] Preferably, the thickness of the outer layer is 0.01-0.15 mm.

[0040] Preferably, the inner diameter of the artificial blood vessel is 1-10 mm.

[0041] Further preferably, the inner diameter of the artificial blood vessel is 1.5 mm, 1.7 mm, 2 mm, 5 mm, 6 mm or 8 mm.

[0042] Preferably, the support ring is made of polytetrafluoroethylene and / or poly(perfluoroethylene propylene).

[0043] Preferably, the support ring is an integrated spiral structure.

[0044] Preferably, the cross-sectional area of ​​the support ring is 0.1-0.5 mm 2 .

[0045] Further preferably, the cross-sectional area of ​​the support ring is 0.1-0.25 mm 2 .

[0046] Preferably, the ring area of ​​the support ring corresponds to the lumen.

[0047] Preferably, the lumen is a blood passage.

[0048] A second aspect of the present invention provides a method for preparing an artificial blood vessel.

[0049] A method for preparing an artificial blood vessel comprises the following steps:

[0050] (1) taking a diselenyl polyurethane solution, performing electrospinning to obtain a tubular structure and adding a support ring to the outside of the tubular structure, and then continuing electrospinning to obtain an inner layer;

[0051] (2) taking the outer layer solution and performing electrospinning on the outside of the inner layer to obtain a tube containing the inner layer and the outer layer;

[0052] (3) placing the tube of step (3) in a solution containing an anticoagulant component, taking it out and drying it, and then cross-linking it to obtain the artificial blood vessel.

[0053] Preferably, in step (1), the preparation method of the diselenyl polyurethane comprises the following steps: in the presence of a catalyst, a diol compound and a diisocyanate compound undergo a prepolymerization reaction at 60-80° C. for 1-6 hours, and then a chain extension reaction is continued with a chain extender at 100-120° C. for 2-24 hours to obtain the diselenyl polyurethane. The diselenyl polyurethane is obtained by bulk polymerization.

[0054] Preferably, in step (1), the preparation method of the diselenyl polyurethane is to mix the diselenyl polyurethane with a solvent.

[0055] Preferably, in step (1), the solvent of the diselenyl polyurethane solution is at least one of water, dichloromethane, chloroform, ethanol, ethyl acetate, acetonitrile, acetone, N,N-dimethylformamide, hexafluoroisopropanol, toluene, xylene, and acetic acid.

[0056] Preferably, in step (1), the mass concentration of the solute in the diselenyl polyurethane solution is 0.01-10 g / mL.

[0057] Further preferably, in step (1), the mass concentration of the solute in the diselenyl polyurethane solution is 0.01-5 g / mL.

[0058] More preferably, in step (1), the mass concentration of the solute in the diselenyl polyurethane solution is 0.1-5 gm / L.

[0059] More preferably, in step (1), the mass concentration of the solute in the diselenyl polyurethane solution is 0.1 g / mL, 0.5 g / mL, 1 g / mL or 2 g / mL.

[0060] Preferably, in step (1), after electrospinning is performed for 1-3 hours, a support ring is added to the outside of the tubular structure, and then electrospinning is continued for 10-20 minutes to obtain an inner layer.

[0061] Further preferably, in step (1), after electrospinning for 1.5 h, 2 h, 2.5 h or 3 h, a support ring is added to the outside of the tubular structure, and then electrospinning is continued for 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min or 20 min to obtain the inner layer.

[0062] Preferably, in steps (1)-(2), the temperature of the electrospinning is 20-50°C, and / or the receiving distance of the electrospinning is 5-50cm, and / or the injection speed of the electrospinning is 0.1-5mL / h, and / or the voltage of the electrospinning is 5-30kV, and / or the spinning time of the electrospinning is 0.5-3h, and / or the spinning solution flow rate of the electrospinning is 0.5-3mL / h, and / or the rotation speed of the receiver of the electrospinning is 50-1000rpm.

[0063] Further preferably, in steps (1)-(2), the receiving distance of the electrospinning is 3-20 cm, and / or the voltage of the electrospinning is 5-25 kV, and / or the spinning solution flow rate of the electrospinning is 0.5-2 mL / h, and / or the rotation speed of the receiver of the electrospinning is 100-1000 rpm.

[0064] More preferably, in steps (1)-(2), the receiving distance of the electrospinning is 3 cm, 4 cm, 6 cm, 10 cm or 15 cm, and / or the voltage of the electrospinning is 10 kV, 12 kV, 13 kV, 15 kV, 16 kV or 20 kV, and / or the spinning solution flow rate of the electrospinning is 0.5 mL / h, 0.6 mL / h, 0.7 mL / h, 0.8 mL / h, 0.9 mL / h, 1 mL / h or 1.5 mL / h, and / or the rotation speed of the receiver for the electrospinning is 300 rpm, 500 rpm, 600 rpm, 700 rpm or 1000 rpm.

[0065] Preferably, in steps (1)-(2), the electrospinning is performed by solution spinning.

[0066] Preferably, the solvent used in the solution spinning method is at least one of water, dichloromethane, chloroform, ethanol, ethyl acetate, acetonitrile, acetone, N,N-dimethylformamide, toluene, xylene, acetic acid and the like.

[0067] Preferably, in step (2), the solvent of the outer layer solution is at least one of water, dichloromethane, chloroform, ethanol, ethyl acetate, acetonitrile, acetone, N,N-dimethylformamide, toluene, xylene, acetic acid, and tetrahydrofuran.

[0068] Preferably, in step (2), the outer layer solution is prepared by mixing the raw materials of the outer layer with a solvent.

[0069] Preferably, in step (2), the mass fraction of the solute in the outer layer solution is 1%-50%.

[0070] Further preferably, in step (2), the mass fraction of the solute in the outer layer solution is 15%-25%.

[0071] More preferably, in step (2), the mass fraction of the solute in the outer layer solution is 5%, 10%, 15%, 18%, 20%, 25% and 30%.

[0072] Preferably, in step (3), the solvent of the solution containing the anticoagulant component is at least one of water, ethanol, ethyl acetate, acetonitrile, acetone, and N,N-dimethylformamide.

[0073] Preferably, in step (3), the mass fraction of the anticoagulant component in the solution containing the anticoagulant component is 0.1%-50%.

[0074] Further preferably, in step (3), the mass fraction of the anticoagulant component in the solution containing the anticoagulant component is 1%-30%.

[0075] More preferably, in step (3), the mass fraction of the anticoagulant component in the solution containing the anticoagulant component is 10%-20%.

[0076] More preferably, in step (3), the mass fraction of the anticoagulant component in the solution containing the anticoagulant component is 5%, 6%, 8%, 10%, 15%, 18%, 20%, 25% or 30%.

[0077] Preferably, in step (3), the tube in step (3) is placed in a solution containing an anticoagulant component for 1-10 minutes.

[0078] Preferably, in step (3), the cross-linking is carried out in an atmosphere of cross-linking agent vapor, and / or the cross-linking time is 2-6 hours.

[0079] A third aspect of the present invention provides a use of an artificial blood vessel.

[0080] An artificial blood vessel is used in vascular replacement, treatment of blood access diseases, treatment of atherosclerosis, vascular bypass, and preparation of arteriovenous fistula for dialysis.

[0081] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0082] The artificial blood vessel provided by the present invention comprises a tube wall and a lumen, wherein the tube wall comprises an outer layer and an inner layer, wherein the inner layer comprises a matrix and a support ring buried in the matrix, wherein the matrix is ​​a diselenide-based polyurethane, and the entire artificial blood vessel is coated with an anticoagulant layer, wherein the raw material component of the anticoagulant layer comprises an anticoagulant component, wherein the anticoagulant component comprises a heparin salt. The outer layer can provide sufficient support strength, the highly elastic inner layer plays a role in preventing leakage and anti-proliferation, and the support ring can provide strength, ensure the mechanical properties of the blood vessel, so that the artificial blood vessel has radial support, and at the same time prevents the diselenide-based polyurethane elastic material of the inner layer from fatigue due to excessive stretching. In addition, the entire artificial blood vessel contains an anticoagulant layer, which has high biocompatibility and a long-term anticoagulant effect. The artificial blood vessel provided by the present invention can be further used as a dedicated blood vessel for dialysis, reducing the risk of thrombosis in the body, increasing the long-term patency of the blood vessels, and preventing leakage after blood vessel puncture. At the same time, blood cells can be regulated, which can further accelerate the regeneration of blood vessels and prevent the occurrence of complications. It can be used to prepare arteriovenous fistulas for dialysis, vascular replacement, treatment of blood access diseases, treatment of atherosclerosis, vascular bypass, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0083] Figure 1 A schematic diagram of the structure of an artificial blood vessel according to Example 1 of the present invention;

[0084] Figure 2 FIG. 1 is a diagram of the preparation process of the artificial blood vessel according to Example 1 of the present invention;

[0085] Figure 3 This is the stress-strain curve of the diselenyl polyurethane prepared in Example 1 of the present invention;

[0086] Figure 4 is the blood coagulation index (BCI value) of the artificial blood vessel in Example 2 of the present invention;

[0087] Figure 5 is the whole blood coagulation time (BCT value) of the artificial blood vessel in Example 2 of the present invention;

[0088] Figure 6 is the daily NO release amount of the artificial blood vessel of Example 3 of the present invention;

[0089] Figure 7 is the number of smooth muscle cells grown in the artificial vascular cell experiment of Example 4 of the present invention;

[0090] Figure 8 This is the number of endothelial cells grown in the artificial vascular cell experiment of Example 4 of the present invention. DETAILED DESCRIPTION

[0091] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0092] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0093] Example 1

[0094] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, wherein the inner layer comprises a matrix and a support ring buried in the matrix, wherein the matrix is ​​diselenide polyurethane, and the artificial blood vessel is coated with an anticoagulant layer, wherein the raw material components of the anticoagulant layer comprise an anticoagulant component, and the anticoagulant component comprises sodium heparin; a schematic diagram of the structure of the artificial blood vessel is shown in Figure 1 As shown, 1 is the anticoagulation layer, 2 is the outer layer, 3 is the inner layer, and 4 is the support ring.

[0095] A method for preparing an artificial blood vessel comprises the following steps:

[0096] (1) Preparation of diselenyl polyurethane: 0.1 g of stannous octoate, 4 g of polytetrahydrofuran-2000, and 1 g of 4,4'-diphenylmethane diisocyanate were added to a reactor, heated to 70°C, and stirred for reaction for 2 h; 0.135 g of 1,4-butanediol and 0.06 g of selenocystamine dihydrochloride were further added to the reactor, heated to 110°C, reacted for 2 h, and cooled to obtain a novel polyurethane.

[0097] The mechanical properties of the diselenide polyurethane prepared above were tested using a universal testing machine to draw a stress-strain curve. The results are as follows: Figure 3 As shown, the results show that diselenide-based polyurethane has good elasticity and tensile strength.

[0098] Preparation of the inner layer: 1.5 g of diselenyl polyurethane was dissolved in 10 g of tetrahydrofuran, and electrospun at a voltage of 15 kV, with a receiving distance of 10 cm and a spinning solution flow rate of 1 mL / h. The receiving speed was 500 rpm for 2 h to obtain an electrospinning tube with a receiver diameter of 2.5 mm. A continuous spiral polyperfluoroethylene propylene support ring was then placed on the electrospinning tube. The support ring had a rotation diameter of about 2.5 mm, a circular cross-section, and a cross-sectional area of ​​0.2 mm. 2 After completion, electrospinning was continued for 10 min to obtain the inner layer.

[0099] (2) Preparation of the outer layer: Replace the spinning solution with a polyethylene terephthalate / xylene solution (the mass fraction of polyethylene terephthalate in the spinning solution is 15%), and continue spinning on the inner layer surface for 1 hour, with a receiving distance of 10 cm, a spinning solution flow rate of 1 mL / h, and a receiving speed of 500 rpm. A tube containing an outer layer and an inner layer is obtained.

[0100] (3) Preparation of anticoagulant layer: After immersing the artificial blood vessel in a mixed solution of 10 mL of ethanol and water (volume ratio of 1:9) containing 1 g of gelatin and 1 g of sodium heparin for 1 min, the blood vessel was freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0101] The preparation process of Example 1 is as follows Figure 2 As shown, 5 is a diselenide polyurethane solution, 6 is a polyethylene terephthalate / xylene solution, and 7 is a heparinized solution.

[0102] Example 2

[0103] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0104] A method for preparing an artificial blood vessel comprises the following steps:

[0105] (1) Preparation of diselenyl polyurethane: 0.1 g of stannous octoate, 4 g of polytetrahydrofuran-5000, and 0.4 g of 4,4'-diphenylmethane diisocyanate were put into a reactor, heated to 70°C, and stirred for reaction for 2 h; 0.054 g of 1,4-butanediol and 0.01 g of selenocystamine were further added to the reactor, heated to 110°C, reacted for 2 h, and cooled to obtain diselenyl polyurethane.

[0106] Preparation of the inner layer: 1.5 g of diselenyl polyurethane was dissolved in 10 g of hexafluoroisopropanol, and electrospun at a voltage of 12 kV, with a receiving distance of 15 cm and a spinning solution flow rate of 1.5 mL / h. The spinning speed was 700 rpm for 2.5 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm 2 , the spinner diameter is about 2.5 mm, and the receiver diameter is 2.5 mm. The electrospinning was continued for 15 min.

[0107] (2) Preparation of outer layer: Replace the spinning solution with a 15% polyethylene terephthalate / xylene solution, continue spinning for 20 min, with a receiving distance of 10 cm, a spinning solution flow rate of 2 mL / h, and a receiving speed of 700 rpm.

[0108] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution of 10 mL of ethanol and water (1:9) containing 3 g of gelatin and 0.6 g of sodium heparin for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0109] Example 3

[0110] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0111] A method for preparing an artificial blood vessel comprises the following steps:

[0112] (1) Preparation of diselenyl polyurethane: 0.1 g of stannous octoate, 4 g of polytetrahydrofuran-5000, and 0.4 g of 4,4'-diphenylmethane diisocyanate were put into a reactor, heated to 70°C, and stirred for reaction for 2 h; 0.054 g of 1,4-butanediol and 0.01 g of selenocystamine were further added to the reactor, heated to 110°C, reacted for 2 h, and cooled to obtain diselenyl polyurethane.

[0113] Preparation of the inner layer: 1.5 g of diselenyl polyurethane was dissolved in 10 g of toluene, and electrospun at a voltage of 12 kV, with a receiving distance of 15 cm and a spinning solution flow rate of 1.5 mL / h. The spinning speed was 700 rpm for 2.5 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm 2 , the spinner diameter is about 2.5 mm, and the receiver diameter is 2.5 mm. The electrospinning was continued for 15 min.

[0114] (2) Preparation of outer layer: Replace the spinning solution with a 15% polyethylene terephthalate / xylene solution, continue spinning for 20 min, with a receiving distance of 10 cm, a spinning solution flow rate of 2 mL / h, and a receiving speed of 700 rpm.

[0115] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution of 10 mL of ethanol and water (1:9) containing 3 g of gelatin and 0.6 g of sodium heparin for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0116] Example 4

[0117] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0118] A method for preparing an artificial blood vessel comprises the following steps:

[0119] (1) Preparation of diselenyl polyurethane: 0.1 g of stannous octoate, 4 g of polytetrahydrofuran-5000, and 0.4 g of 4,4'-diphenylmethane diisocyanate were put into a reactor, heated to 70°C, and stirred for reaction for 2 h; 0.054 g of 1,4-butanediol and 0.01 g of selenocystamine were further added to the reactor, heated to 110°C, reacted for 2 h, and cooled to obtain diselenyl polyurethane.

[0120] Preparation of the inner layer: 1 g of diselenyl polyurethane was dissolved in 10 mL of xylene, and electrospun at a voltage of 20 kV, with a receiving distance of 3 cm and a spinning solution flow rate of 0.5 mL / h. The spinning speed was 1000 rpm for 3 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm 2 , the spinner diameter is about 2.5 mm, and the receiver diameter is 2.5 mm. The electrospinning was continued for 20 min.

[0121] (2) Preparation of outer layer: Replace the spinning solution with a 10% polyethylene terephthalate / xylene solution, continue spinning for 20 min, with a receiving distance of 10 cm, a spinning solution flow rate of 2 mL / h, and a receiving speed of 700 rpm.

[0122] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution of 10 mL of ethanol and water (1:9) containing 3 g of hyaluronic acid and 0.15 g of sodium heparin for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0123] Example 5

[0124] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0125] A method for preparing an artificial blood vessel comprises the following steps:

[0126] (1) Preparation of diselenyl polyurethane: 0.1 g of stannous octoate, 4 g of polytetrahydrofuran-5000, and 0.4 g of 4,4'-diphenylmethane diisocyanate were put into a reactor, heated to 70°C, and stirred for reaction for 2 h; 0.054 g of 1,4-butanediol and 0.01 g of selenocystamine were further added to the reactor, heated to 110°C, reacted for 2 h, and cooled to obtain diselenyl polyurethane.

[0127] Preparation of the inner layer: 2 g of diselenyl polyurethane was dissolved in 10 g of dichloromethane, and electrospun at a voltage of 10 kV, with a receiving distance of 20 cm and a spinning solution flow rate of 1.5 mL / h. The spinning speed was 700 rpm for 2.5 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm 2 , the spinner diameter is about 6 mm, and the receiver diameter is 6 mm. The electrospinning was continued for 15 min.

[0128] (2) Preparation of outer layer: Replace the spinning solution with a 15% polyethylene terephthalate / tetrahydrofuran solution, continue spinning for 11 min, the receiving distance is 10 cm, the spinning solution flow rate is 2 mL / h, and the receiving speed is 500 rpm.

[0129] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution of 20 mL of ethanol and water (1:9) containing 7.5 g of cellulose and 0.6 g of sodium heparin for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0130] Example 6

[0131] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0132] A method for preparing an artificial blood vessel comprises the following steps:

[0133] (1) Preparation of diselenyl polyurethane: 0.1 g of stannous octoate, 4 g of polytetrahydrofuran-5000, and 0.4 g of 4,4'-diphenylmethane diisocyanate were put into a reactor, heated to 70°C, and stirred for reaction for 2 h; 0.054 g of 1,4-butanediol and 0.01 g of selenocystamine were further added to the reactor, heated to 110°C, reacted for 2 h, and cooled to obtain diselenyl polyurethane.

[0134] Preparation of the inner layer: 2 g of diselenyl polyurethane was dissolved in 8 g of acetone, and electrospun at a voltage of 13 kV, with a receiving distance of 15 cm and a spinning solution flow rate of 0.6 mL / h. The spinning speed was 600 rpm for 1.5 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm 2 , the spinner diameter is about 6 mm, and the receiver diameter is 6 mm. The electrospinning was continued for 12 min.

[0135] (2) Preparation of outer layer: Replace the spinning solution with a 20% polyethylene terephthalate / N,N-dimethylformamide solution, continue spinning for 20 min, with a receiving distance of 10 cm, a spinning solution flow rate of 2 mL / h, and a receiving speed of 500 rpm.

[0136] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution containing 3 g lignin, 0.6 g sodium heparin and 10 mL water for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0137] Example 7

[0138] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0139] A method for preparing an artificial blood vessel comprises the following steps:

[0140] (1) Preparation of diselenyl polyurethane: 0.1 g of stannous octoate, 4 g of polytetrahydrofuran-5000, and 0.4 g of 4,4'-diphenylmethane diisocyanate were put into a reactor, heated to 70°C, and stirred for reaction for 2 h; 0.054 g of 1,4-butanediol and 0.01 g of selenocystamine were further added to the reactor, heated to 110°C, reacted for 2 h, and cooled to obtain diselenyl polyurethane.

[0141] Preparation of the inner layer: 2 g of diselenyl polyurethane was dissolved in 10 g of hexafluoroisopropanol, and electrospun at a voltage of 16 kV, with a receiving distance of 6 cm and a spinning solution flow rate of 1 mL / h. The spinning speed was 700 rpm for 1 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm 2 , the spinner diameter is about 8 mm, and the receiver diameter is 8 mm. The electrospinning was continued for 18 min.

[0142] (2) Preparation of outer layer: Replace the spinning solution with a 15% polyethylene terephthalate / xylene solution, continue spinning for 30 min, with a receiving distance of 10 cm, a spinning solution flow rate of 2 mL / h, and a receiving speed of 500 rpm.

[0143] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution of 10 mL of ethanol and water (1:9) containing 3 g of gelatin and 0.6 g of sodium heparin for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0144] Example 8

[0145] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0146] A method for preparing an artificial blood vessel comprises the following steps:

[0147] (1) Preparation of diselenyl polyurethane: 0.1 g of dibutyltin dilaurate, 4 g of 1,4-butanediol, and 4 g of toluene diisocyanate were put into a reactor, the temperature was raised to 70°C, and the reaction was stirred for 2 h; 0.054 g of resorcinol dihydroxyethyl ether and 0.02 g of selenocystamine were further added to the reactor, the temperature was raised to 110°C, the reaction was carried out for 2 h, and the temperature was lowered to obtain diselenyl polyurethane.

[0148] Preparation of the inner layer: 1.5 g of diselenyl polyurethane was dissolved in 10 g of hexafluoroisopropanol, and electrospun at a voltage of 12 kV, with a receiving distance of 15 cm and a spinning solution flow rate of 1.5 mL / h. The spinning speed was 700 rpm for 2.5 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm 2 , the spinner diameter is about 2.5 mm, and the receiver diameter is 2.5 mm. The electrospinning was continued for 15 min.

[0149] (2) Preparation of outer layer: Replace the spinning solution with a 15% polyethylene terephthalate / xylene solution, continue spinning for 20 min, with a receiving distance of 10 cm, a spinning solution flow rate of 2 mL / h, and a receiving speed of 700 rpm.

[0150] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution of 10 mL of ethanol and water (1:9) containing 3 g of gelatin and 0.6 g of sodium heparin for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0151] Example 9

[0152] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0153] A method for preparing an artificial blood vessel comprises the following steps:

[0154] (1) Preparation of diselenyl polyurethane: 0.1 g of dibutyltin dilaurate, 4 g of polylactide, and 0.4 g of isophorone diisocyanate were put into a reactor, heated to 70°C, and stirred for reaction for 2 h; 0.054 g of diethyltoluenediamine and 0.01 g of bis(hydroxymethyl) diselenide were further added to the reactor, heated to 110°C, reacted for 2 h, and cooled to obtain diselenyl polyurethane.

[0155] Preparation of the inner layer: 1.5 g of diselenyl polyurethane was dissolved in 10 g of hexafluoroisopropanol, and electrospun at a voltage of 12 kV, with a receiving distance of 15 cm and a spinning solution flow rate of 1.5 mL / h. The spinning speed was 700 rpm for 2.5 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm 2 , the spinner diameter is about 2.5 mm, and the receiver diameter is 2.5 mm. The electrospinning was continued for 15 min.

[0156] (2) Preparation of outer layer: Replace the spinning solution with a 15% polyethylene terephthalate / xylene solution, continue spinning for 20 min, with a receiving distance of 10 cm, a spinning solution flow rate of 2 mL / h, and a receiving speed of 700 rpm.

[0157] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution of 10 mL of ethanol and water (1:9) containing 3 g of gelatin and 0.6 g of sodium heparin for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0158] Example 10

[0159] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0160] A method for preparing an artificial blood vessel comprises the following steps:

[0161] (1) Preparation of diselenyl polyurethane: 0.1 g of pentamethyldiethylenetriamine, 4 g of polyethylene glycol-b-polylactide, and 0.5 g of lysine diisocyanate were put into a reactor, heated to 70°C, and stirred for reaction for 2 h; 0.054 g of hydroquinone dihydroxyethyl ether and 0.01 g of bis(aminoethyl) diselenide were further added to the reactor, the temperature was raised to 110°C, reacted for 2 h, and the temperature was lowered to obtain diselenyl polyurethane.

[0162] Preparation of the inner layer: 1.5 g of diselenyl polyurethane was dissolved in 10 g of hexafluoroisopropanol, and electrospun at a voltage of 12 kV, with a receiving distance of 15 cm and a spinning solution flow rate of 1.5 mL / h. The spinning speed was 700 rpm for 2.5 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm 2 , the spinner diameter is about 2.5 mm, and the receiver diameter is 2.5 mm. The electrospinning was continued for 15 min.

[0163] (2) Preparation of outer layer: Replace the spinning solution with a 15% polyethylene terephthalate / xylene solution, continue spinning for 20 min, with a receiving distance of 10 cm, a spinning solution flow rate of 2 mL / h, and a receiving speed of 700 rpm.

[0164] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution of 10 mL of ethanol and water (1:9) containing 3 g of gelatin and 0.6 g of sodium heparin for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0165] Embodiment 11

[0166] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0167] A method for preparing an artificial blood vessel comprises the following steps:

[0168] (1) Preparation of diselenyl polyurethane: 0.1 g of N,N-dimethylcyclohexylamine, 4 g of polytetrahydrofuran-5000, and 0.4 g of isophorone diisocyanate were put into a reactor, heated to 70°C, and stirred for reaction for 2 h; 0.054 g of ethylene glycol and 0.01 g of selenocystamine were further added to the reactor, the temperature was raised to 110°C, the reaction was carried out for 2 h, and the temperature was lowered to obtain diselenyl polyurethane.

[0169] Preparation of the inner layer: 1.5 g of diselenyl polyurethane was dissolved in 10 g of hexafluoroisopropanol, and electrospun at a voltage of 12 kV, with a receiving distance of 15 cm and a spinning solution flow rate of 1.5 mL / h. The spinning speed was 700 rpm for 2.5 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm 2 , the spinner diameter is about 2.5 mm, and the receiver diameter is 2.5 mm. The electrospinning was continued for 15 min.

[0170] (2) Preparation of outer layer: Replace the spinning solution with a 15% polyethylene terephthalate / xylene solution, continue spinning for 20 min, with a receiving distance of 10 cm, a spinning solution flow rate of 2 mL / h, and a receiving speed of 700 rpm.

[0171] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution of 10 mL of ethanol and water (1:9) containing 3 g of gelatin and 0.6 g of sodium heparin for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0172] Example 12

[0173] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0174] A method for preparing an artificial blood vessel comprises the following steps:

[0175] (1) Preparation of diselenyl polyurethane: 0.1 g of DY-20, 4 g of hydroquinone dihydroxyethyl ether, and 4 g of dicyclohexylmethane diisocyanate were put into a reactor, heated to 70°C, and stirred for reaction for 2 h; 0.054 g of bis-sec-butylaminodiphenylmethane and 0.01 g of bis(hydroxyethyl) diselenide were further added to the reactor, the temperature was raised to 110°C, the reaction was carried out for 2 h, and the temperature was lowered to obtain diselenyl polyurethane.

[0176] Preparation of the inner layer: 1.5 g of diselenyl polyurethane was dissolved in 10 g of hexafluoroisopropanol, and electrospun at a voltage of 12 kV, with a receiving distance of 15 cm and a spinning solution flow rate of 1.5 mL / h. The spinning speed was 700 rpm for 2.5 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm 2 , the spinner diameter is about 2.5 mm, and the receiver diameter is 2.5 mm. The electrospinning was continued for 15 min.

[0177] (2) Preparation of outer layer: Replace the spinning solution with a 15% polyethylene terephthalate / xylene solution, continue spinning for 20 min, with a receiving distance of 10 cm, a spinning solution flow rate of 2 mL / h, and a receiving speed of 700 rpm.

[0178] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution of 10 mL of ethanol and water (1:9) containing 3 g of gelatin and 0.6 g of sodium heparin for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0179] Example 13

[0180] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0181] A method for preparing an artificial blood vessel comprises the following steps:

[0182] (1) Preparation of diselenyl polyurethane: 0.1 g of N,N'-diethylpiperazine, 4 g of polycaprolactone, and 0.4 g of 4,4'-diphenylmethane diisocyanate were put into a reactor, heated to 70°C, and stirred for reaction for 2 h; 0.054 g of 1,4-butanediol and 0.01 g of selenocystamine were further added to the reactor, heated to 110°C, reacted for 2 h, and cooled to obtain diselenyl polyurethane.

[0183] Preparation of the inner layer: 1.5 g of diselenyl polyurethane was dissolved in 10 g of hexafluoroisopropanol, and electrospun at a voltage of 12 kV, with a receiving distance of 15 cm and a spinning solution flow rate of 1.5 mL / h. The spinning speed was 700 rpm for 2.5 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm 2 , the spinner diameter is about 2.5 mm, and the receiver diameter is 2.5 mm. The electrospinning was continued for 15 min.

[0184] (2) Preparation of outer layer: Replace the spinning solution with a 15% polyethylene terephthalate / xylene solution, continue spinning for 20 min, with a receiving distance of 10 cm, a spinning solution flow rate of 2 mL / h, and a receiving speed of 700 rpm.

[0185] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution of 10 mL of ethanol and water (1:9) containing 3 g of gelatin and 0.6 g of sodium heparin for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0186] Embodiment 14

[0187] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0188] A method for preparing an artificial blood vessel comprises the following steps:

[0189] (1) Preparation of diselenyl polyurethane: 0.1 g of dibutyltin dilaurate, 4 g of polytetrahydrofuran-5000, and 0.4 g of 4,4'-diphenylmethane diisocyanate were put into a reactor, heated to 70°C, and stirred for reaction for 2 h; 0.054 g of bis-sec-butylaminodiphenylmethane and 0.01 g of bis(hydroxymethyl) diselenide were further added to the reactor, heated to 110°C, reacted for 2 h, and cooled to obtain diselenyl polyurethane.

[0190] Preparation of the inner layer: 1.5 g of diselenyl polyurethane was dissolved in 10 g of hexafluoroisopropanol, and electrospun at a voltage of 12 kV, with a receiving distance of 15 cm and a spinning solution flow rate of 1.5 mL / h. The spinning speed was 700 rpm for 2.5 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm 2 , the spinner diameter is about 2.5 mm, and the receiver diameter is 2.5 mm. The electrospinning was continued for 15 min.

[0191] (2) Preparation of outer layer: Replace the spinning solution with a 15% polyethylene terephthalate / xylene solution, continue spinning for 20 min, with a receiving distance of 10 cm, a spinning solution flow rate of 2 mL / h, and a receiving speed of 700 rpm.

[0192] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution of 10 mL of ethanol and water (1:9) containing 3 g of gelatin and 0.6 g of sodium heparin for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0193] Embodiment 15

[0194] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0195] A method for preparing an artificial blood vessel comprises the following steps:

[0196] (1) Preparation of diselenyl polyurethane: 0.1 g of N,N,N',N'-tetramethylalkylenediamine, 1 g of polyethylene glycol-1000, and 0.4 g of 4'-diphenylmethane diisocyanate were put into a reactor, the temperature was raised to 70°C, and the reaction was stirred for 2 h; 0.054 g of di-sec-butylaminodiphenylmethane and 0.01 g of bis(hydroxyethyl) diselenide were further added to the reactor, the temperature was raised to 110°C, the reaction was carried out for 2 h, and the temperature was lowered to obtain diselenyl polyurethane.

[0197] Preparation of the inner layer: 1.5 g of diselenyl polyurethane was dissolved in 10 g of hexafluoroisopropanol, and electrospun at a voltage of 12 kV, with a receiving distance of 15 cm, a spinning solution flow rate of 1.5 mL / h, and a receiving speed of 700 rpm for 2.5 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm2, a rotating diameter of about 2.5 mm, and a receiver diameter of 2.5 mm. The electrospinning was continued for 15 min.

[0198] (2) Preparation of outer layer: Replace the spinning solution with a 15% polyethylene terephthalate / xylene solution, continue spinning for 20 min, with a receiving distance of 10 cm, a spinning solution flow rate of 2 mL / h, and a receiving speed of 700 rpm.

[0199] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution of 10 mL of ethanol and water (1:9) containing 3 g of gelatin and 0.6 g of sodium heparin for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0200] Example 16

[0201] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0202] A method for preparing an artificial blood vessel comprises the following steps:

[0203] (1) Preparation of diselenyl polyurethane: 0.1 g of stannous octoate, 4 g of resorcinol, and 4 g of hexamethylene diisocyanate were added to a reactor, heated to 70°C, and stirred for reaction for 2 h; 0.054 g of 3,3'-dichloro-4,4'-diaminophenylmethane and 0.01 g of selenocystamine were further added to the reactor, heated to 110°C, reacted for 2 h, and cooled to obtain diselenyl polyurethane.

[0204] Preparation of the inner layer: 1.5 g of diselenyl polyurethane was dissolved in 10 g of hexafluoroisopropanol, and electrospun at a voltage of 12 kV, with a receiving distance of 15 cm and a spinning solution flow rate of 1.5 mL / h. The spinning speed was 700 rpm for 2.5 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm 2 , the spinner diameter is about 2.5 mm, and the receiver diameter is 2.5 mm. The electrospinning was continued for 15 min.

[0205] (2) Preparation of outer layer: Replace the spinning solution with a 15% polyethylene terephthalate / xylene solution, continue spinning for 20 min, with a receiving distance of 10 cm, a spinning solution flow rate of 2 mL / h, and a receiving speed of 700 rpm.

[0206] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution of 10 mL of ethanol and water (1:9) containing 3 g of gelatin and 0.6 g of sodium heparin for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0207] Embodiment 17

[0208] An artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, the inner layer comprises a matrix and a support ring buried in the matrix, the matrix is ​​diselenide polyurethane, the artificial blood vessel is coated with an anticoagulant layer, the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise sodium heparin.

[0209] A method for preparing an artificial blood vessel comprises the following steps:

[0210] (1) Preparation of diselenyl polyurethane: 0.1 g of stannous octoate, 4 g of hydroquinone dihydroxyethyl ether, and 4 g of 4,4'-diphenylmethane diisocyanate were put into a reactor, heated to 70°C, and stirred for reaction for 2 h; 0.05 g of 4,4'-methylene-bis(3-chloro-2,6-diethylaniline) and 0.01 g of selenocystamine were further added to the reactor, heated to 110°C, reacted for 2 h, and cooled to obtain diselenyl polyurethane.

[0211] Preparation of the inner layer: 1.5 g of diselenyl polyurethane was dissolved in 10 g of hexafluoroisopropanol, and electrospun at a voltage of 12 kV, with a receiving distance of 15 cm and a spinning solution flow rate of 1.5 mL / h. The spinning speed was 700 rpm for 2.5 h to obtain a semi-finished artificial blood vessel, and then a continuous polyperfluoroethylene propylene support ring was added. The support ring had a circular cross-sectional area of ​​0.2 mm 2 , the spinner diameter is about 2.5 mm, and the receiver diameter is 2.5 mm. The electrospinning was continued for 15 min.

[0212] (2) Preparation of outer layer: Replace the spinning solution with a 15% polyethylene terephthalate / xylene solution, continue spinning for 20 min, with a receiving distance of 10 cm, a spinning solution flow rate of 2 mL / h, and a receiving speed of 700 rpm.

[0213] (3) Preparation of anticoagulant layer: After the artificial blood vessel is immersed in a mixed solution of 10 mL of ethanol and water (1:9) containing 3 g of gelatin and 0.6 g of sodium heparin for 1 min, the blood vessel is freeze-dried and cross-linked under glutaraldehyde vapor for 2 h to obtain an artificial blood vessel.

[0214] Comparative Example 1

[0215] An artificial blood vessel, which differs from Example 1 in that the diselenyl polyurethane is replaced by a commercially available diselenyl polyurethane (BASF).

[0216] Comparative Example 2

[0217] An artificial blood vessel, which is different from Example 2 in that the anticoagulant layer does not contain heparin.

[0218] Comparative Example 3

[0219] An artificial blood vessel, which differs from Example 2 in that it does not contain an inner layer and a support ring.

[0220] Comparative Example 4

[0221] An artificial blood vessel, which differs from Example 2 in that it does not contain a support ring.

[0222] Product effect testing

[0223] 1. Anticoagulation test

[0224] The blood was collected in a vial containing 3.6 mL of sodium citrate solution (mass fraction 3.5%) to prevent coagulation, and 200 μL of the blood was dripped onto the artificial blood vessel prepared in Example 1 and the glass surface, respectively, and then 20 μL of calcium chloride solution (0.2 mol / L) was dripped onto each of them, and incubated at 37°C for 5 min. After completion, 25 mL of deionized water was added to destroy the uncoagulated red blood cells, and the anticoagulation ability of the coating was detected using an ELISA instrument. BCI (coagulation index) represents the anticoagulation ability. The larger the BCI value, the better the anticoagulation effect. The calculation formula of the BCI is shown in the following formula (1):

[0225] BCI=OD sample / OD blank ×100% (1)

[0226] Among them, in formula (1), OD sample OD is the absorbance of the sample measured by the microplate reader at 541 nm. blankIt is the absorbance of the sample at 541 nm after 200 μL of fresh blood was hemolyzed with 25 mL of deionized water.

[0227] The results are as follows Figure 4 As shown in FIG. 1 , the difference between the BCI values ​​of the artificial blood vessel and the glass shows that the artificial blood vessel of Example 1 has significant anticoagulant ability. Similarly, the BCT (whole blood coagulation time) of the artificial blood vessel and the control group glass was measured using the kit ( Figure 5 ). The above results show that the artificial blood vessel of Example 1 prolongs the coagulation time and has a significant anticoagulant effect.

[0228] 2. NO release experiment

[0229] The artificial blood vessel and glass of Example 1 were immersed in a 0.01 mmol / L aqueous solution of sodium nitroprusside, the NO content in the solution was detected every 24 hours, and a curve of the change of NO content was drawn.

[0230] The results are as follows Figure 6 As shown, artificial blood vessels can continuously catalyze the decomposition of sodium nitroprusside to release NO gas, thereby promoting the growth and migration of endothelial cells and inhibiting the proliferation of smooth muscle cells.

[0231] 3. Cell experiments

[0232] The artificial blood vessel of Example 1 and the glass were immersed in a culture medium containing smooth muscle cells, and 0.01 mmol / L sodium nitroprusside was added to the culture medium, and cultured at 37° C. and 5% CO 2 for 24 hours. After completion, the number of cells in the culture dish was counted.

[0233] Figure 7 The figure shows the comparison of the number of smooth muscle cells in different groups. It can be seen from the figure that artificial blood vessels can inhibit the proliferation of smooth muscle cells.

[0234] The artificial blood vessel prepared in Example 1 was immersed in a culture medium containing vascular endothelial cells and 0.01 mmol / L sodium nitroprusside was added to the culture medium and cultured at 37° C. in 5% CO 2 for 24 hours. After completion, the number of cells in the culture dish was counted. Figure 8 The data show that the artificial blood vessels can significantly promote the proliferation of endothelial cells.

[0235] 4. Performance comparison of artificial blood vessels prepared in different embodiments and comparative examples

[0236] Blood vessel leakage: The artificial blood vessels prepared in the above embodiments and comparative examples were punctured 2000 times with a 21G needle, and the artificial blood vessels were connected to a peristaltic pump. The water flow rate in the pump was controlled to be 80 mL / s, and the leakage of the artificial blood vessels was observed.

[0237] Table 1 Performance comparison of artificial blood vessels prepared in different embodiments and comparative examples

[0238]

[0239] It can be seen from the results in the above table that the diselenyl polyurethanes prepared in Examples 1-17 of the present invention have excellent mechanical properties, and the prepared artificial blood vessels have good anticoagulant effects. The artificial blood vessels can continuously catalyze the decomposition of sodium nitroprusside to release NO gas, thereby promoting the growth and migration of endothelial cells, inhibiting the proliferation of smooth muscle cells, and preventing blood vessels from leaking after multiple punctures.

[0240] The inner layer of Comparative Example 1 is made of commercially available polyurethane, which results in the inability of the artificial blood vessel to decompose and release NO gas, and the ability to inhibit smooth muscle cell proliferation is poor. The anticoagulant layer of the artificial blood vessel of Comparative Example 2 does not contain heparin, resulting in poor anticoagulant effect. The artificial blood vessel of Comparative Example 3 does not contain an inner layer and a support ring, resulting in severe penetration. The artificial blood vessel of Comparative Example 4 does not contain a support ring, which makes it difficult for the blood vessel to maintain a tubular shape for a long time.

Claims

1. An artificial blood vessel, It is characterized in that The artificial blood vessel comprises a tube wall and a tube cavity, wherein the tube wall comprises an outer layer and an inner layer, wherein the inner layer comprises a matrix and a support ring buried in the matrix, wherein the matrix is ​​diselenide polyurethane, and the artificial blood vessel is coated with an anticoagulant layer, wherein the raw material components of the anticoagulant layer comprise anticoagulant components, and the anticoagulant components comprise heparin salt.

2. The artificial blood vessel according to claim 1, It is characterized in that The material of the outer layer is at least one of polytetrafluoroethylene, polyethylene terephthalate, and polyamide.

3. The artificial blood vessel according to claim 1, It is characterized in that The raw materials for preparing the diselenyl polyurethane include: diol compounds, diisocyanate compounds, chain extenders and catalysts.

4. The artificial blood vessel according to claim 1, It is characterized in that The support ring is made of polytetrafluoroethylene and / or poly(perfluoroethylene propylene).

5. The artificial blood vessel according to claim 1, It is characterized in that The raw material components of the anticoagulation layer also include biocompatible materials.

6. A method for preparing an artificial blood vessel, It is characterized in that The steps include: (1) taking a diselenyl polyurethane solution, performing electrospinning to obtain a tubular structure and adding a support ring to the outside of the tubular structure, and then continuing electrospinning to obtain an inner layer; (2) taking the outer layer solution and performing electrospinning on the outside of the inner layer to obtain a tube containing the inner layer and the outer layer; (3) placing the tube of step (3) in a solution containing an anticoagulant component, taking it out and drying it, and then cross-linking it to obtain the artificial blood vessel.

7. The method for preparing an artificial blood vessel according to claim 6, It is characterized in that In step (1), the preparation method of the diselenyl polyurethane comprises the following steps: under the action of a catalyst, a diol compound and a diisocyanate compound undergo a prepolymerization reaction at 60-80°C for 1-6 hours, and then a chain extension reaction is continued with a chain extender at 100-120°C for 2-24 hours to obtain the diselenyl polyurethane.

8. The method for preparing an artificial blood vessel according to claim 6, It is characterized in that In steps (1)-(2), the temperature of the electrospinning is 20-50°C, and / or the receiving distance of the electrospinning is 5-50cm, and / or the injection speed of the electrospinning is 0.1-5mL / h, and / or the voltage of the electrospinning is 5-30kV, and / or the spinning time of the electrospinning is 0.5-3h, and / or the spinning solution flow rate of the electrospinning is 0.5-3mL / h, and / or the rotation speed of the receiver of the electrospinning is 50-1000rpm.

9. The method for preparing an artificial blood vessel according to claim 6, It is characterized in that In step (3), the cross-linking is carried out in an atmosphere of cross-linking agent vapor, and / or the cross-linking time is 2-6 hours.

10. Use of the artificial blood vessel according to any one of claims 1 to 5 in vascular replacement, treatment of blood access diseases, treatment of atherosclerosis, vascular bypass, and preparation of arteriovenous fistula for dialysis.

Citation Information

Cited By

  • Selenium-containing high-molecular compound modified zinc alloy material as well as preparation method and application thereof

    CN121422298A