Solid alkali hydrotalcite catalyst as well as preparation method and application thereof
The Ca-Mg-AlLDHs and Ca-La-AlLDHs catalysts were synthesized by hydrothermal method, which solved the problem of low catalytic activity of calcium-aluminum hydrotalcite in the aldol condensation reaction of isobutyraldehyde, and achieved efficient reaction of acetaldehyde and isobutyraldehyde. The catalytic effect, especially the catalytic effect of Ca-La-AlLDHs, is optimal, and the conversion rate and selectivity are significantly improved.
Patent Information
- Application Number
- CN202410771626.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-15
- Publication Date
- 2024-10-15
AI Technical Summary
The catalytic activity of calcium aluminum hydrotalcite in the aldol condensation reaction of isobutyraldehyde is low, and it is difficult to effectively improve its catalytic performance with existing technology.
The solid alkali hydrotalcite catalysts Ca-Mg-AlLDHs and Ca-La-AlLDHs were synthesized using a hydrothermal method. The pH value was controlled to 10-11 by slowly adding sodium hydroxide dropwise in the deionized solution, and then calcined in a muffle furnace. , to prepare a catalyst with good catalytic effect.
Achieved high conversion rate and selectivity for the aldol condensation reaction of acetaldehyde and isobutyraldehyde. Ca-La-AlLDHs has the best catalytic effect. The reaction conversion rate is 71.32%, the selectivity is 73.36%, and the product yield is 52.32%. .
Smart Images

Figure CN118767905A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, in particular to a solid alkaline hydrotalcite catalyst and a preparation method and application thereof. Background Art
[0002] Hydrotalcite, also known as layered double hydroxides (LDHs), is a type of anionic layered crystal structure material, usually a hydroxide composed of two or more metal ions, with a regular octahedral structure similar to brucite (Mg(OH)2). The general formula of hydrotalcite is: Among them, M 2+ is a monovalent or divalent (mostly divalent) metal cation, M 3+ A is a trivalent metal cation. n - is an interlayer anion. Hydrotalcite has the characteristics of adjustable composition and structure, special layered structure, acidity and alkalinity, memory effect, thermal stability and flame retardancy. Therefore, hydrotalcite can be used to catalyze aldol condensation reaction, among which solid alkaline hydrotalcite containing calcium, magnesium and aluminum elements is most widely used in aldol condensation reaction. In recent years, hydrotalcite, as a new type of inorganic functional material, has certain alkalinity, special composition and structure, and exchangeability of interlayer anions, and has been widely used in catalysis, photochemistry, electrochemical building materials, water pollution treatment and other fields.
[0003] The main methods for preparing hydrotalcite-like substances in industry at present are:
[0004] (1) Coprecipitation method
[0005] The coprecipitation method is through Ca 2+ / Al 3+ Mix the metal solution with the precipitant (OH - / CO3 2- ) reaction to produce a uniform precipitate, which is then aged under certain conditions to obtain a hydrotalcite layered structure. The reaction pH value must be strictly controlled during its preparation.
[0006] (2) Urea method
[0007] Urea is used as precipitant and Ca, Al and other metal salt solutions are used as raw materials. When the mixed solution T≥90℃, urea is hydrolyzed (NH4 + and HCO3 - ), urea isomerization (CO(NH2)2), ammonium cyanate decomposition (CO2 and NH3), NH3 hydrolysis (NH3·H2O) and co-precipitation reaction, hydrotalcite is obtained, and the crystal size is uniform and has a good layered structure. The raw materials of this method are cheap and easy to obtain, the process is simple, and it is easy to obtain a single crystal phase.
[0008] (3) Ultrasonic synthesis
[0009] Ultrasonic synthesis is an improvement of the coprecipitation method. Synthesizing metal alkali hydrotalcite under ultrasonic conditions can effectively reduce reaction time and reaction control conditions, save preparation energy and materials, make the reaction easier to control, and the obtained product has a unique internal connection structure in ion exchange performance. The ultrasonic method uses the change of sound pressure to cause the rapid flow of fluid, thereby promoting the rapid movement of ions between catalyst layers and the reaction rate; at the same time, the collapse of cavitation bubble nuclei produces local high temperature, high pressure and strong shock waves and microjets, which promote the improvement of hydrotalcite crystal quality and the exchange capacity of interlayer anions.
[0010] She Daocai et al. modulated Ca 2+ With Al 3+ The ratio of the amount of substance and the crystal chemistry theory were combined to establish the Ca / Al-LDHs microstructure model, which provides a valuable reference for the study of new intercalated Ca / Al-LDHs materials. The calcium aluminum hydrotalcite synthesized by Luo Fangmu et al. through coprecipitation method has good crystallinity, complete crystal structure, orderly arrangement of interlayer anions, and strong interaction between interlayer H2O molecules and layer hydroxyl groups. Wang Huimin et al. used the early structural topological transformation and memory effect of layered double hydroxides (LDHs) to prepare rehydrated Ca4Al 1-x Ga x -LDHs and Ca4Al 1-x In x -LDHs, and finally re-Ca4Al 0.90 Ga 0.10 -LDHs has the best catalytic activity for aldol condensation reaction. Bing Weihan [8] CaAl-LDHs was used as a precursor and converted into a composite metal oxide (denoted as CaAl-MMO) by high temperature calcination. The structure was then restored by hydration treatment, and OH was introduced into the interlayer. - ions, and obtained LDHs solid base catalyst (re-CaAl-LDHs), which showed significantly enhanced base catalytic performance for the condensation of formaldehyde and isobutyraldehyde to hydroxyl neopentaldehyde, which was significantly better than the traditional solid base catalysis. Zhao Ningbo studied the condensation reaction of formaldehyde and isobutyraldehyde with hydrotalcite and magnesium zirconium oxide as catalysts, and investigated the specific effects of various factors including phase transfer catalyst CTAB, raw material feed ratio, solvent, etc. on the reaction system. Zhang Ming prepared MgFe-CH2N2-LDHs precursor doped with cyanamide by nucleation crystallization isolation method, and obtained a series of magnetic magnesium-based composite metal oxides, MgFe2O4 / MgO, after high-temperature calcination, and used it for the transesterification reaction of tributyrin and methanol. Yang Kun et al. prepared a series of hydrotalcite samples HLDs with different magnesium-aluminum ratios by coprecipitation method, and obtained a series of magnesium-aluminum composite oxides by calcination of hydrotalcite.
[0011] Compared with the commonly used magnesium aluminum hydrotalcite and zinc aluminum hydrotalcite, calcium aluminum hydrotalcite (CaAl-LDHs) has a more thermally stable interlayer structure, less toxicity, and higher removal performance for heavy metal ions; it is easy to prepare and has low cost. However, its catalytic activity is still low when used for the aldol condensation reaction of isobutyraldehyde. Summary of the invention
[0012] In order to solve the above technical problems, the present invention provides a solid alkaline hydrotalcite catalyst and a preparation method and application thereof.
[0013] To achieve the above object, the present invention is implemented according to the following technical solutions:
[0014] One of the purposes of the present invention is to provide a method for preparing a solid alkali hydrotalcite catalyst, comprising the following steps:
[0015] S1. Dissolve Mg(NO3)2·6H2O or La(NO3)3·6H2O, Al(NO3)3·9H2O, and Ca(NO3)2·4H2O in a molar ratio of (0.5-1.5):1:1 in deionized water to obtain solution A;
[0016] S2, then slowly add 1.5 mol / L sodium hydroxide aqueous solution to solution A until the pH of the solution is 10-11, precipitate at 600 r / min at 60°C for 10 h, collect the precipitate by centrifugation, wash it with deionized water and ethanol several times, and then dry it to obtain a catalyst precursor;
[0017] S3. Place the catalyst precursor in a muffle furnace and calcine at 450° C. for 4 h to obtain a solid alkaline hydrotalcite catalyst.
[0018] Furthermore, in step S2, drying is performed at 80° C. for 24 hours.
[0019] Furthermore, in step S3, during calcination, the temperature in the muffle furnace is raised to 450° C. at a rate of 2 min / ° C.
[0020] Preferably, the molar ratio of Mg(NO3)2·6H2O or La(NO3)3·6H2O to Al(NO3)3·9H2O is 1:1.
[0021] The second object of the present invention is to provide a solid alkali hydrotalcite catalyst prepared by the above method.
[0022] The third object of the present invention is to provide an application of a solid alkaline hydrotalcite catalyst in catalyzing the aldol condensation reaction of acetaldehyde and isobutyraldehyde.
[0023] Compared with the prior art, the present invention synthesizes solid alkali hydrotalcite catalysts Ca-Mg-AlLDHs and Ca-La-AlLDHs by a hydrothermal method, has a simple preparation process, and has good catalytic effect when used for catalyzing the aldol condensation reaction of acetaldehyde and isobutyraldehyde, wherein Ca-La-AlLDHs has the best comprehensive catalytic effect, with a reaction conversion rate of 71.32%, a selectivity of 73.36%, and a product yield of 52.32%. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 SEM images of precursor (a), (b) and calcium magnesium aluminum solid base (c), (d).
[0025] Figure 2 SEM images of precursor (e), (f) and calcium lanthanum aluminum solid base (g), (h).
[0026] Figure 3 XRD spectra of calcium magnesium aluminum hydrotalcite with different Mg and Al ratios.
[0027] Figure 4 XRD spectra of calcium lanthanum aluminum hydrotalcite with different La:Al ratios.
[0028] Figure 5 Infrared spectra of calcium magnesium aluminum hydrotalcite with different Mg and Al ratios.
[0029] Figure 6 Infrared spectra of calcium lanthanum aluminum hydrotalcite with different La:Al ratios.
[0030] Figure 7 BET diagram of calcium magnesium aluminum hydrotalcite with different Mg and Al ratios.
[0031] Figure 8 BET diagram of calcium lanthanum aluminum hydrotalcite with different La:Al ratios.
[0032] Fig. 9 TG diagram of calcium magnesium aluminum hydrotalcite with different Mg and Al ratios.
[0033] Fig.10 TG diagram of calcium lanthanum aluminum hydrotalcite with different La:Al ratios.
[0034] Fig.11 The effects of different Mg / Al and La / Al on the reaction: (a) the effect of different Mg / Al on the reaction; (b) the effect of different La / Al on the reaction.
[0035] Fig.12 The effect of reaction time on the condensation reaction of acetaldehyde and isobutyraldehyde catalyzed by calcium lanthanum aluminum hydrotalcite (La / Al=1:1). DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the invention.
[0037] The related instruments and reagents used in the following examples, unless otherwise specified, are commercially available instruments and reagents, and the methods involved, unless otherwise specified, are well-known methods.
[0038] Example 1
[0039] 1) Dissolve Mg(NO3)2·6H2O, Al(NO3)3·9H2O and Ca(NO3)2·4H2O in molar ratios of 0:1:1, 0.5:1:1, 1.0:1:1 and 1.5:1:1 in 100 ml of deionized water to obtain solution A;
[0040] 2) Prepare 100 ml of 1.5 mol / L NaOH solution, then slowly add 1.5 mol / L sodium hydroxide aqueous solution to solution A until the pH value of the solution is 10-11, precipitate at 60°C and 600 r / min for 10 h, collect the precipitate by centrifugation, wash it with deionized water and ethanol for several times, and dry it at 80°C for 24 h to obtain a catalyst precursor;
[0041] 3) The catalyst precursor was placed in a muffle furnace, and the temperature was raised to 450° C. at a rate of 2 min / ° C. and calcined for 4 h to obtain several solid alkali hydrotalcite catalyst Ca-Mg-AlLDHs samples.
[0042] Example 2
[0043] 1) La(NO3)3·6H2O, Al(NO3)3·9H2O and Ca(NO3)2·4H2O in molar ratios of 0:1:1, 0.5:1:1, 1.0:1:1 and 1.5:1:1 were dissolved in 100 ml of deionized water to obtain solution A;
[0044] 2) Prepare 100 ml of 1.5 mol / L NaOH solution, then slowly add 1.5 mol / L sodium hydroxide aqueous solution to solution A until the pH value of the solution is 10-11, precipitate at 60°C and 600 r / min for 10 h, collect the precipitate by centrifugation, wash it with deionized water and ethanol for several times, and dry it at 80°C for 24 h to obtain a catalyst precursor;
[0045] 3) The catalyst precursor was placed in a muffle furnace, heated to 450° C. at a rate of 2 min / ° C., and calcined for 4 h to obtain several solid alkali hydrotalcite catalyst Ca-La-AlLDHs samples.
[0046] Several solid alkali hydrotalcite catalyst Ca-Mg-AlLDHs samples prepared in Example 1 and several solid alkali hydrotalcite catalyst Ca-La-AlLDHs samples prepared in Example 2 were respectively taken for characterization and analysis, and the specific operations were as follows:
[0047] (1) SEM
[0048] SEM can be used to visually observe the surface morphology of the material and analyze the particle size and pore arrangement.
[0049] (2) Powder X-ray diffraction analysis (XRD)
[0050] X-ray diffraction analysis uses a Bruker X-ray diffractometer to perform powder XRD tests in an air atmosphere with a scanning temperature of 25°C, a scanning angle of 5°-75°, and a scanning speed of 0.2. Small-angle XRD can be used to study the mesoporous structure of nano-mesoporous materials, because the orderly arranged pores will produce corresponding diffraction peaks in the small-angle field. Therefore, XRD can be used to understand the crystal form, configuration parameters, etc. of mesoporous materials.
[0051] (3) Fourier transform infrared spectroscopy (FT-IR)
[0052] FT-IR and Raman spectroscopy can help us understand the bonding conditions and existing forms of organic functional groups and various chemical bonds, among which FT-IR is the most widely used.
[0053] (4) Low temperature N2 adsorption-desorption (BET)
[0054] The type and characteristics of the pore structure can be determined by the adsorption characteristic curve, and low-temperature N2 adsorption-desorption can obtain information such as the specific surface area, pore size distribution and pore size of the material.
[0055] (5) Thermogravimetric analysis (TG)
[0056] It is a method to measure the relationship between the mass of a substance and temperature or time under program-controlled temperature. The TG weight loss curve can be used to intuitively see the mass change of the material within a certain temperature range, so as to better understand the physical and chemical changes of the material at each temperature point, and to know its stability and heat resistance, etc.
[0057] The characterization results are as follows Figure 1-Figure 10 As shown, from Figure 1 It can be seen that calcium magnesium aluminum solid alkali and its precursor are composed of particles of different sizes; their sizes are between 2 and 10 μm. There are more large particles and fewer small particles in the calcium magnesium aluminum solid alkali precursor, and the particle surface is denser and smoother. There are more small particles and fewer large particles in the calcium magnesium aluminum solid alkali, and the particle surface is loose and rough, basically showing a flaky structure.2+ The disorder of the system can be increased, so the test results are basically consistent.
[0058] from Figure 2 It can be seen that calcium lanthanum aluminum solid base and its precursor are composed of particles of different sizes; their sizes are between 2 and 100 μm. There are more large particles and fewer small particles in the calcium lanthanum aluminum solid base precursor, and the agglomeration phenomenon is more serious, showing a cauliflower shape. After calcination, the calcium lanthanum aluminum solid base basically presents a flake structure.
[0059] Figure 3 For different [Mg 2+ ] / [Al 3+ ]Comparison of XRD patterns of the synthesized products. By comparison, it can be seen that the positions of the diffraction peaks in the sample patterns of each ratio are basically the same. It can be inferred that each sample has a layered structure of calcium-magnesium-aluminum hydrotalcite, and the peak shape is relatively symmetrical and sharp, indicating that the co-precipitation method synthesized a LDHs precursor with a better crystal form. From the above figure, it can be seen that the peak intensity of the sample of curve d is relatively the strongest, and the half-peak width is the narrowest. The second is the sample of curve c, whose peak intensity and half-peak width are better than those of curves a and b, but worse than those of curve d. The sample of curve d is formed under a certain temperature, pressure and reasonable crystallization environment. The hydrotalcite particles have better crystallinity and more regular crystal forms, thereby forming better calcium-magnesium-aluminum hydrotalcite crystals.
[0060] Figure 4 For different 2+ ] / [Al 3+ ]Comparison of XRD patterns of the synthesized products. By comparison, it can be seen that the positions of the diffraction peaks in the patterns of each sample are basically the same, and it can be inferred that each sample has a layered structure of calcium lanthanum aluminum hydrotalcite. At the same time, it can be seen that the peak intensity of the sample of curve c is relatively the strongest. The sample crystal of curve c crystallizes under a mild environment, the crystallinity of the hydrotalcite particles is better, and the diffraction peak intensity in the -30-XRD pattern is the strongest, so it is known that a better calcium lanthanum aluminum hydrotalcite crystal is formed.
[0061] Depend on Figure 5 It can be seen that the infrared spectroscopy analysis of the hydrotalcite solid base catalyst with different magnesium-aluminum ratios (a, b, c, d in the above figure are 0:1, 0.5:1, 1:1, 1.5:1 respectively) shows that the infrared spectroscopy of each sample is 500-1400 cm -1 There is obvious infrared absorption in the wave number range, within this wavelength range 1400 and 821,657cm -1 The absorption peak comes from CO3 in ion-pillared hydrotalcite 2- There are three antisymmetric stretching vibration modes. -1The absorption peak is the stretching vibration peak of the -OH bond, which is lower than the absorption wave number of the -OH bond of free water. -1 The peak in the range is Ca 2+ The vibration peak, 1630cm -1 The peaks in the range are the -OH bending vibration peaks of adsorbed water on the surface of hydrotalcite and crystalline water in the interlayer region.
[0062] Depend on Figure 6 It can be seen that the IR spectrum of the hydrotalcite solid base catalysts with different lanthanum-aluminum ratios (a, b, c, and d in the figure above are 0:1, 0.5:1, 1:1, and 1.5:1, respectively) was analyzed at 500-1400 cm -1 There is obvious infrared absorption in the wave number range, within this wavelength range 1400 and 821,657cm -1 The absorption peak comes from CO3 in ion-pillared hydrotalcite 2- There are three antisymmetric stretching vibration modes. -1 The absorption peak is the stretching vibration peak of the -OH bond, which is lower than the absorption wave number of the -OH bond of free water. -1 The peak in the range is Ca 2+ The vibration peak, 1630cm -1 The peaks in the range are the -OH bending vibration peaks of the adsorbed water on the surface of hydrotalcite and the crystal water in the interlayer region. The introduction of rare earth ions slightly shifts the peaks of calcium lanthanum aluminum hydrotalcite, but the peak shapes are basically the same.
[0063] Depend on Figure 7 It can be seen that curves a, b, c, and d are respectively Mg-Al 0:1, 0.5:1, 1:1, and 1.5:1. Curve a is calcium aluminum hydrotalcite, and the curve type is H2 type, with a more complex pore structure. The others are H3 type, and their isotherms do not have an obvious saturated adsorption platform. The specific surface area of calcium magnesium aluminum hydrotalcite curve c is 12.8351m 2 / g, and the optimal pore width is 0.9906nm.
[0064] Depend on Figure 8 It can be seen that curves a, b, c, and d are lanthanum aluminum 0:1, 0.5:1, 1:1, and 1.5:1, respectively. Curves a and c are of type H2, with a more complex pore structure, and the others are of type H3, with no obvious saturated adsorption platform in their isotherms. The specific surface area of calcium lanthanum aluminum hydrotalcite curve c is 111.7177m 2 / g, and the optimal pore width is 0.9033nm.
[0065] Depend on Fig. 9It can be seen that the calcium magnesium aluminum solid base catalyst curves a, c, and d have an obvious weight loss step at 100-200°C; curves b and c are relatively stable below 500°C, and have an obvious weight loss step at 500-600°C. After 800°C, the mass basically does not change with temperature, and is mainly composed of CaO and MgO crystals.
[0066] Depend on Fig.10 It can be seen that curve c of the calcium lanthanum aluminum solid base catalyst has an obvious weight loss step at 500°C, and curve a has an obvious weight loss step at 100°C; the weight loss of the other two curves is relatively smooth, and the mass basically does not change with temperature after 800°C, and they are mainly composed of two crystals, CaO and LaO.
[0067] Therefore, the optimal synthesis conditions of Ca-Mg-AlLDHs and Ca-La-AlLDHs are determined as follows: n(Mg 2+ ):n(Al 3+ )=1:1,n(La 2+ ):n(Al 3+ )=1:1, hydrothermal temperature 60℃, hydrothermal time 12h. The following examples synthesized Ca-Mg-AlLDHs and Ca-La-AlLDHs under this condition.
[0068] Application Example 1
[0069] Evaluation system for catalytic acetaldehyde and isobutyraldehyde aldol condensation reaction: The condensation reaction of acetaldehyde and isobutyraldehyde is carried out in a three-necked flask of a batch reactor. 0.2 grams of fresh hydrotalcite solid base catalyst Ca-Mg-AlLDHs or Ca-La-AlLDHs is dispersed in isobutyraldehyde (0.55 mol) and 40% acetaldehyde aqueous solution. Under the protection of nitrogen atmosphere, a magnetic stirrer (15w, 600r / min) is used to start the reaction at a reaction temperature of 60°C. Samples are taken and filtered at a fixed time, and a gas chromatography hydrogen ion flame detector (FID) is used for detection and analysis. The conversion rate and selectivity are measured based on the gas distribution area of IBD and HPA. This reaction has many side reactions, and the sample should be diluted before testing to make the test results more accurate.
[0070] The test results are as follows Fig.11 and Fig.12 As shown, from Fig.11 and Fig.12 It can be concluded that the yield of the product gradually increases with the extension of the reaction time. When the reaction time is 6h, the reaction basically reaches equilibrium. Among them, Ca-La-AlLDHs has the best catalytic effect on the reaction, and the product yield can reach 52.32%, which is better than Ca-Mg-AlLDHs. Fig.11It can be seen that with the increase of the ratio of Mg and La atoms, the conversion rate of acetaldehyde and isobutyraldehyde and the yield of the product showed a trend of first increasing and then decreasing. Among them, Ca-La-AlLDHs had the best comprehensive catalytic effect, with a reaction conversion rate of 71.32%, a selectivity of 73.36%, and a product yield of 52.32%.
[0071] In summary, the Ca-La-AlLDHs prepared in the present invention has a good catalytic effect when used to catalyze the aldol condensation reaction of acetaldehyde and isobutyraldehyde.
[0072] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. All technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.
Claims
1. A method for preparing a solid alkali hydrotalcite catalyst, characterized in that: The following steps are involved: S1. Dissolve Mg(NO3)2·6H2O or La(NO3)3·6H2O, Al(NO3)3·9H2O, and Ca(NO3)2·4H2O in a molar ratio of (0.5-1.5):1:1 in deionized water to obtain solution A; S2, then slowly add 1.5 mol / L sodium hydroxide aqueous solution to solution A until the pH of the solution is 10-11, precipitate at 600 r / min at 60°C for 10 h, collect the precipitate by centrifugation, wash it with deionized water and ethanol several times, and then dry it to obtain a catalyst precursor; S3. Place the catalyst precursor in a muffle furnace and calcine at 450° C. for 4 h to obtain a solid alkaline hydrotalcite catalyst.
2. The method for preparing the solid alkali hydrotalcite catalyst according to claim 1, characterized in that: In the step S2, drying is performed at 80° C. for 24 hours.
3. The method for preparing the solid alkali hydrotalcite catalyst according to claim 1, characterized in that: In the step S3, during calcination, the temperature in the muffle furnace is raised to 450° C. at a rate of 2 min / ° C.
4. The method for preparing the solid alkali hydrotalcite catalyst according to claim 1, characterized in that: The molar ratio of Mg(NO3)2·6H2O or La(NO3)3·6H2O to Al(NO3)3·9H2O is 1:
1.
5. A solid alkali hydrotalcite catalyst prepared by the method according to any one of claims 1 to 4.
6. Use of the solid alkaline hydrotalcite catalyst as claimed in claim 5 in catalyzing the aldol condensation reaction of acetaldehyde and isobutyraldehyde.
Citation Information
Patent Citations
Modified magnalium composite oxide catalyst for acetone condensation as well as preparation method and application thereof
CN104874386A
Biodiesel catalyst X-Ca-Zn-Al-O and preparation method
CN105642267A
Biodiesel catalyst X-Ca-Mg-Al-O and preparation method
CN105642268A
Method for synthesizing ethyl methyl carbonate under catalysis of magnesium-aluminum-lanthanum composite oxide
CN106748782A
Preparation method and use method of hydroxyl intercalated calcium magnesium aluminum hydrotalcite solid base catalyst
CN110624529A
Cited By
Anti-coking aldehyde ketone polycondensation catalyst, and preparation method and application thereof
CN123148956A