Extrusion type catalyst for oil refining alkaline residue waste liquid treatment and preparation method thereof

By using alumina and non-noble metal oxides as the carrier and active components of the catalyst, the problems of high catalyst cost and poor sulfur resistance in the treatment of oil refining alkali residue wastewater are solved, and the preparation of low-cost and high sulfur resistance catalysts is achieved. It significantly reduces the chemical oxygen demand of alkali residue and is suitable for efficient treatment of oil refining alkali residue wastewater.

CN118767907APending Publication Date: 2024-10-15NANJING YANJIANG ACAD OF RESCOURCES & ECOLOGY SCI CO LTD
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202411000791.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing catalyst preparation costs in the treatment of oil refining alkali residue wastewater are high, the catalyst has poor sulfur resistance, the preparation process is complex, and the reaction conditions are harsh, which affects the application of the technology.

Method used

Alumina, non-noble metal oxides and cross-linking agents are mixed in a certain proportion, stirred and shaped into cylindrical particles, dried and roasted to prepare non-noble metal heterogeneous catalysts, using non-noble metal oxides such as zinc oxide and iron oxide as active components It uses alumina as a carrier, combined with an appropriate amount of water and adhesive, to form a catalyst with high sulfur resistance and low price.

Benefits of technology

It achieves low cost, high sulfur resistance, and mild catalytic reaction conditions for the treatment of oil refining alkali residue wastewater. The catalyst has a significant effect on reducing the COD of alkali residue and has good water resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005004023970000011
    Figure HDA0005004023970000011
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to an extrusion type catalyst for oil refining alkaline residue waste liquid treatment and a preparation method thereof, and relates to the field of catalysts for oil refining alkaline residue waste liquid treatment, and the key points of the technical scheme are as follows: the method comprises the following steps: uniformly mixing alumina, at least one non-noble metal oxide, at least one adhesive and water, stirring and kneading until a pug is formed, the preparation method comprises the following steps: preparing a catalyst, processing the catalyst into cylindrical particles, drying the cylindrical particles to obtain a catalyst semi-finished product, and roasting the catalyst semi-finished product to obtain a catalyst finished product. The obtained catalyst is low in price, high in sulfur resistance, simple in preparation process, mild in catalytic reaction condition, convenient to disassemble, good in effect of reducing the COD of the alkaline residues and good in water resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of catalysts for treating oil refining alkali residue waste liquid, and in particular to an integral wet oxidation catalyst for treating alkali residue and a preparation method thereof. Background Art

[0002] The waste alkali liquid produced after washing catalytic cracking gasoline, liquid hydrocarbons in gas separation units, etc. with alkali liquid is collectively called alkali slag. It contains a large amount of toxic and harmful substances such as neutral oil, organic acid, volatile phenol and sulfide. The wastewater is dark brown and has a foul odor. The COD is as high as hundreds of thousands. It is extremely difficult to treat and has always been a problem that has plagued oil refining companies.

[0003] At present, the most mainstream method for treating oil refining alkali residue wastewater is wet oxidation, which operates under high temperature (120-320°C) and high pressure (0.5-20MPa) conditions, using gaseous oxygen as an oxidant to oxidize and decompose organic matter in water into small molecular organic or inorganic matter. It has the characteristics of no secondary pollution and low treatment cost. However, traditional wet oxidation requires high temperature and pressure and relatively long residence time, high requirements for equipment materials, high one-time investment, and wet oxidation can only be used as pretreatment, and its effluent also has a high COD. In order to reduce the temperature and pressure required for the reaction and improve the treatment effect, catalytic wet air oxidation (CWAO) has become a research hotspot in recent years. However, for catalytic wet oxidation technology, the preparation of efficient catalysts is the core of its technology.

[0004] Wet oxidation catalyst can be divided into homogeneous catalyst and heterogeneous catalyst, the former has higher catalytic activity, but it is difficult to analyze from the system, it cannot be reused and easily causes secondary pollution, so it is less used, while the latter has the advantages of easy separation and reusability, so it is widely used. At present, heterogeneous catalyst is mainly a precious metal catalyst (CN107442148A, CN107442115B, CN107442116A) with platinum, palladium, rhodium, iridium and ruthenium as active components. Precious metal catalysts are superior in performance, high in catalytic activity, and strong in acid and alkali resistance, but expensive and very limited in use. The patent "An activated carbon-supported copper oxide catalyst and its preparation method" (application number 200610089575.0) uses activated carbon-supported copper oxide as a catalyst to work together with H2O2 to catalytically oxidize coking wastewater; the patent "A preparation method for a catalyst for catalytic wet oxidation of organic pollutants in water" (application number 201310117329.1) uses SBA-15 molecular sieve as a carrier and CuO as an active component as a catalyst to catalytically oxidize organic matter in water; the patent "A composite functional nanosphere catalyst with recyclable function loaded with precious metals and its application in catalytic reduction of p-nitrophenol" (application number 201310091252.5) ​​uses precious metal nanoparticles and magnetic nanoparticles to be coated in a polymer to obtain a composite functional nanosphere catalyst loaded with precious metals in a polar solvent.

[0005] In summary, the catalysts used in the prior art have the disadvantages of extremely high preparation cost, complex catalyst preparation process, high catalytic reaction conditions, and poor catalyst sulfur resistance, which affect the application of this technology. Therefore, it is necessary to develop non-precious metal heterogeneous catalysts with low price, high sulfur resistance, simple preparation process, and mild catalytic reaction conditions. Summary of the invention

[0006] The purpose of the present invention is to provide an integral wet oxidation catalyst for alkaline slag treatment and a preparation method thereof, which has the advantages of developing a non-precious metal heterogeneous catalyst with low price, high sulfur resistance, simple preparation process and mild catalytic reaction conditions.

[0007] The present invention relates to a method for preparing a catalyst for treating oil refining alkali residue wastewater, the method comprising the following steps: 1) Mix alumina, non-precious metal oxide, cross-linking agent and water in a certain proportion; 2) stirring and kneading the mixture of the catalyst base material and water until a clay body is formed; 3) forming the clay into cylindrical particles of a certain diameter and length; 4) drying the cylindrical particles obtained in step 3) to obtain a catalyst semi-finished product; 5) calcining the semi-finished catalyst to obtain a finished catalyst.

[0008] Preferably, the non-precious metal oxide is one or more of zinc oxide, iron oxide, zirconium oxide, and cerium oxide, or the non-precious metal oxide is a mixture of zinc oxide and iron oxide, and the adhesive is selected from water glass, glucose, glycerol and a mixture thereof, or the adhesive is glycerol; Preferably, the aluminum oxide has a particle size of 1 μm to 100 μm, and the non-noble metal oxide has a particle size of 0.1 μm to 1 μm.

[0009] Preferably, the aluminum oxide has a particle size of 5 μm to 20 μm; and the non-precious metal oxide has a particle size of 0.1 μm to 0.3 μm.

[0010] Preferably, based on the total weight of the catalyst base material, the content of the non-precious metal oxide is 1% to 50%; the content of the aluminum oxide is 20% to 90%, the content of the adhesive is 1% to 30%; and the content of water is 20% to 50%.

[0011] Preferably, the content of the non-precious metal oxide is 5% to 25%; the content of the aluminum oxide is 40% to 70%; the content of the adhesive is 5% to 15%; and the content of water is 25% to 40%.

[0012] Preferably, when the molding is extrusion molding, the extrusion pressure is 1 MPa to 220 MPa; The drying temperature is 60°C to 400°C, the drying time is 0.5 h to 20 h, and the drying equipment is an oven, a hot air furnace or a track kiln; The calcination temperature is 200° C. to 900° C., and the calcination time is 1 h to 200 h.

[0013] Preferably, the extrusion pressure is 1 MPa to 100 MPa; the drying temperature is 100°C to 200°C; the drying time is 0.8 h to 15 h, or 1 h to 12 h; the roasting temperature is 400°C to 600°C; and the roasting time is 2 h to 48 h.

[0014] Another object of the present invention is to provide an extruded catalyst for treating oil refining alkali residue waste liquid.

[0015] Preferably, the obtained cylindrical particles have a diameter of 1 to 20 mm and a length of 2 to 100 mm.

[0016] The beneficial effects of the present invention are as follows: the process of preparing the catalyst for treating oil refining alkali residue wastewater according to the present invention is relatively simple, the obtained catalyst has a low price, high sulfur resistance, simple preparation process, mild catalytic reaction conditions, convenient disassembly, good effect on reducing the COD of alkali residue, and good water resistance. BRIEF DESCRIPTION OF THE DRAWINGS In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work. Figure 1 This is the flow chart of the catalyst performance evaluation device. DETAILED DESCRIPTION

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work. Figure 1 This is the flow chart of the catalyst performance evaluation device. The present application will be further described in detail below through specific implementation methods. It should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, but do not limit the present invention in any way.

[0018] Any specific numerical value disclosed herein (including the endpoint of the numerical range) is not limited to the exact value of the numerical value, but should be understood to also cover values ​​close to the exact value, such as all possible values ​​within the range of ±5% of the exact value. In addition, for the disclosed numerical range, the endpoint values ​​of the range, the endpoint values ​​and the specific point values ​​in the range, and the specific point values ​​can be arbitrarily combined to obtain one or more new numerical ranges, and these new numerical ranges should also be regarded as specifically disclosed herein.

[0019] Unless otherwise specified, the terms used herein have the same meaning as commonly understood by those skilled in the art. If a term is defined herein and its definition is different from the commonly understood meaning in the art, the definition herein shall prevail.

[0020] The expressions "comprising" or "including" herein should be interpreted as including all the specifically mentioned features as well as optional, additional, unspecified features. As used herein, the use of the term "comprising" also discloses solutions in which there are no further features than the specifically mentioned features, such as the expressions "consisting essentially of" and "consisting of".

[0021] The preparation method of the catalyst for treating oil refining alkali residue wastewater involved in the present invention comprises the following steps 1) to 5).

[0022] Step 1) Preparation of catalyst base material Aluminum oxide, non-precious metal oxide (one or more of zinc oxide, copper oxide, iron oxide, zirconium oxide, cerium oxide), a cross-linking agent and water are mixed in a certain proportion; The non-noble metal oxide is one or more of zinc oxide, iron oxide, zirconium oxide and cerium oxide. Preferably, the non-noble metal oxide is a mixture of zinc oxide and iron oxide.

[0023] The adhesive is selected from water glass, glucose, glycerol and a mixture thereof. Preferably, the adhesive is glucose.

[0024] The alumina has a particle size of 1 μm to 100 μm, preferably 5 μm to 20 μm. The non-precious metal oxide has a particle size of 0.1 μm to 1 μm, preferably 0.1 μm to 0.3 μm. The above particle size can be measured using conventional particle size testing methods, including but not limited to laser particle size analyzer method, radar measurement method, electron microscopy method and sedimentation method. Preferably, the above particle size is measured using a laser particle size analyzer. Among them, alumina is used as a carrier, non-precious metal oxide is used as a catalytically active component, and the particle size of the catalytically active component is controlled at 0.1 μm to 1 μm, which can improve the dispersibility of the active component in the carrier and increase the number of catalytically active sites per unit catalyst volume.

[0025] The content of the non-noble metal oxide may be 1% to 50%, preferably 5% to 25%, based on the total weight of the catalyst base material.

[0026] The content of the alumina may be 20% to 90%, preferably 40% to 70%, based on the total weight of the catalyst base material.

[0027] The content of the adhesive may be 1% to 30%, preferably 5% to 15%, based on the total weight of the catalyst base material.

[0028] The water content may be 20% to 50%, preferably 25% to 40%, based on the total weight of the catalyst base material.

[0029] The above ratio is based on the following considerations: 1. Non-precious metal oxides are the main active components, and alumina is used as a carrier. Within the ratio range selected by this method, non-precious metal oxides can be highly dispersed in the alumina carrier, and the internal pores of alumina can also play a confining role to prevent the loss of active components. If the ratio is lower than that of this method, there will be insufficient active sites and unsatisfactory catalytic performance. If the ratio is higher than that of this method, the confinement effect will be reduced, which will cause the loss of active components; 2. The main function of the cross-linking agent is to bond the components. If the amount of cross-linking agent added is lower than the lower limit of the proportion of this scheme, the components will not be able to bond with each other. If the amount of cross-linking agent added is higher than the upper limit of the proportion of this scheme, the components will not be able to achieve uniform distribution during the subsequent mixing and tempering process, affecting the quality of the final product.

[0030] 3. The water content is used to adjust the viscosity of the coating slurry and to produce mesoporous channels during the drying process, providing channels for the pollutants to be treated in the wastewater to contact the active sites inside the catalyst. If the water content is higher than the upper limit of this scheme, the mesopore ratio will be too large, the catalyst strength will be too low, and it will not be suitable for use under high temperature and high pressure. If the water content is lower than the upper limit of this scheme, the mesopore content will be insufficient, the active sites inside the catalyst cannot be fully utilized, and the catalytic activity is too low.

[0031] Step 2) Prepare the mud tire The catalyst base is stirred and kneaded until a clay is formed.

[0032] The kneading can be performed by any kneading equipment commonly used in the field of catalyst preparation, wherein the kneading equipment is preferably a screw kneader.

[0033] When a kneader is used, the kneading pressure is preferably 80 MPa to 400 MPa, preferably 100 MPa to 300 MPa; the rotation speed is preferably 10 r / min to 300 r / min, preferably 20 r / min to 180 r / min; and the temperature is preferably 10°C to 50°C.

[0034] As known to those skilled in the art of catalysts, the clay refers to a solid like plasticine or dough.

[0035] Step 3) Clay molding The clay mold is molded into cylindrical particles of a certain diameter and length. When the molding is extrusion molding, the extrusion pressure can be 1 MPa to 220 MPa, preferably 1 MPa to 100 MPa. The obtained cylindrical particles have a diameter of 1 to 20 mm and a length of 2 to 100 mm.

[0036] Step 4) Drying The cylindrical particles obtained in step 3) are dried to obtain a catalyst semi-finished product.

[0037] The drying temperature may be 60°C to 400°C, preferably 100°C to 200°C.

[0038] The drying time may be 0.5 h to 20 h, preferably 0.8 h to 15 h, more preferably 1 h to 12 h.

[0039] The drying can be performed by any commonly used drying equipment in the field of catalyst preparation. Preferably, the drying equipment can be an oven, a hot air furnace or a track kiln.

[0040] Step 5) Calcination of the semi-finished catalyst The obtained catalyst semi-finished product is calcined to obtain the catalyst finished product.

[0041] The calcination can be carried out by any conventional calcination method and equipment in the field of catalyst preparation.

[0042] The calcination temperature may be 200°C to 900°C, preferably 400°C to 600°C.

[0043] The calcination time may be 1 h to 200 h, preferably 2 h to 48 h. Example

[0044] The present invention is further described in detail below using examples, but the present invention is not limited to these examples. Example 1

[0045] 1) Mix 600 g of aluminum oxide, 300 g of zinc oxide (D90 = 0.2 μm), 100 g of glycerol and 500 g of water, and then dry stir until the mixture is uniform; 2) Mechanically kneading the mixture in 1) at a kneading pressure of 200 MPa and a rotation speed of 120 r / min until a plasticine-like clay is formed; 3) Extruding the clay with a die at a pressure of 20 MPa into cylindrical particles with a diameter of 4 mm and a length of 10 mm; 4) drying the cylindrical particles obtained in step 3) at 150° C. for 4 h to obtain a catalyst semi-finished product; 5) The catalyst semi-finished product obtained in step 4) was calcined at 500°C for 4 h to obtain a catalyst finished product 1, wherein the catalyst active component is zinc oxide (33%wt), numbered 1-1. Example 2

[0046] 1) Mix 600 g of aluminum oxide, 300 g of iron oxide (D90 = 0.2 μm), 100 g of glycerol and 500 g of water, and then dry-mix until the mixture is uniform; 2) Mechanically kneading the mixture in 1) at a kneading pressure of 200 MPa and a rotation speed of 120 r / min until a plasticine-like clay is formed; 3) Extruding the clay with a die at a pressure of 20 MPa into cylindrical particles with a diameter of 4 mm and a length of 10 mm; 4) drying the cylindrical particles obtained in step 3) at 150° C. for 4 h to obtain a catalyst semi-finished product; 5) The catalyst semi-finished product obtained in step 4) was calcined at 500°C for 4 h to obtain a catalyst product 1, wherein the catalyst active component is iron oxide (33%wt), numbered 1-2. Example 3

[0047] 1) Mix 500 g of aluminum oxide, 100 g of zinc oxide (D90=0.2 μm), 100 g of iron oxide (D90=0.2 μm), 100 g of zirconium oxide (D90=0.2 μm), 100 g of cerium oxide (D90=0.2 μm), 50 g of glucose, 50 g of glycerol and 500 g of water, and then dry-mix until the mixture is uniform; 2) Mechanically kneading the mixture in 1) at a kneading pressure of 200 MPa and a rotation speed of 120 r / min until a plasticine-like clay is formed; 3) Extruding the clay with a die at a pressure of 20 MPa into cylindrical particles with a diameter of 4 mm and a length of 10 mm; 4) drying the cylindrical particles obtained in step 3) at 150° C. for 4 h to obtain a catalyst semi-finished product; 5) The catalyst semi-finished product obtained in step 4) was calcined at 500°C for 4 h to obtain a catalyst product 1, wherein the catalyst active components are zinc oxide (11%wt), iron oxide (11%wt), zirconium oxide (11%wt) and cerium oxide (11%wt), numbered 1-3. Example 4

[0048] 1) Mix 600 g aluminum oxide, 150 g zinc oxide (D90 = 0.2 μm), 150 g iron oxide (D90 = 0.2 μm), 100 g glycerol and 500 g water, and then dry stir until the mixture is uniform; 2) Mechanically kneading the mixture in 1) at a kneading pressure of 200 MPa and a rotation speed of 120 r / min until a plasticine-like clay is formed; 3) Extruding the clay with a die at a pressure of 20 MPa into cylindrical particles with a diameter of 4 mm and a length of 10 mm; 4) drying the cylindrical particles obtained in step 3) at 150° C. for 4 h to obtain a catalyst semi-finished product; 5) The catalyst semi-finished product obtained in step 4) was calcined at 500°C for 4 h to obtain a catalyst finished product 1, wherein the catalyst active components are zinc oxide (16.67%wt) and iron oxide (16.67%wt), numbered 1-4.

[0049] Comparative Example

[0050] As Comparative Example 1, copper oxide was used instead of zinc oxide and iron oxide used in Example 4.

[0051] As Comparative Example 2, ordinary zinc oxide and iron oxide (D90=10 μm) were used to replace the nano-grade zinc oxide and iron oxide used in Example 4.

[0052] Comparative Example 1

[0053] 1) Mix 600 g of aluminum oxide, 300 g of copper oxide (D90 = 0.2 μm), 100 g of glycerol and 500 g of water, and then dry stir until the mixture is uniform; 2) Mechanically kneading the mixture in 1) at a kneading pressure of 200 MPa and a rotation speed of 120 r / min until a plasticine-like clay is formed; 3) Extruding the clay with a die at a pressure of 20 MPa into cylindrical particles with a diameter of 4 mm and a length of 10 mm; 4) drying the cylindrical particles obtained in step 3) at 150° C. for 4 h to obtain a catalyst semi-finished product; 5) The catalyst semi-finished product obtained in step 4) was calcined at 500°C for 4 h to obtain a catalyst finished product 1, wherein the catalyst active component is copper oxide (33%wt), numbered 2-1. Comparative Example 2

[0054] 1) Mix 600 g aluminum oxide, 150 g zinc oxide (D90 = 10 μm), 150 g iron oxide (D90 = 10 μm), 100 g glucose and 500 g water, and then dry stir until the mixture is uniform; 2) Mechanically kneading the mixture in 1) at a kneading pressure of 200 MPa and a rotation speed of 120 r / min until a plasticine-like clay is formed; 3) Extruding the clay with a die at a pressure of 20 MPa into cylindrical particles with a diameter of 4 mm and a length of 10 mm; 4) drying the cylindrical particles obtained in step 3) at 150° C. for 4 h to obtain a catalyst semi-finished product; 5) The catalyst semi-finished product obtained in step 4) was calcined at 500°C for 4 h to obtain a catalyst product 1, wherein the catalyst active components are zinc oxide (16.67%wt) and iron oxide (16.67%wt), numbered 2-2.

[0055] The prepared catalyst was used in the wet oxidation experiment of oil refining waste alkali residue. The experimental flow chart is as follows: Figure 1 As shown in the figure, under high temperature and high pressure, the oil refining waste alkali slag with a COD of 100,000 mg / L (including sulfide content of 50,000 mg / L) continuously enters a reactor equipped with a catalyst, and at the same time, a high-pressure oxygen-containing gas (air) is introduced. The organic matter and sulfur-containing compounds in the oil refining waste alkali slag are degraded into CO2, H2O and SO4 under the action of the catalyst and oxygen. 2- , thereby achieving the effect of significantly reducing COD.

[0056] Evaluation conditions: temperature 200°C, pressure 0.5MPaG, catalyst loading 0.5L, waste alkali liquid flow 1.5L / h, air flow 0.5Nm 3 / h.

[0057] The test results of Examples 1-1 to 1-4 and Comparative Examples 2-1 and 2-2 are shown in Table 1.

[0059] Table 1 Catalyst activity evaluation results

[0060] It can be seen from Table 1 that for catalysts 1-1 to 1-4 prepared by the method of the present invention, COD≤5000mg / L after treating alkali residue wastewater, and can be directly subjected to biochemical treatment subsequently. However, for catalysts 2-1 and 2-2 not prepared by the method of the present invention, COD>5000mg / L after treating alkali residue wastewater, and cannot be directly subjected to biochemical treatment subsequently. At the same time, the performance of the catalyst prepared by the method of the present invention can remain stable for a long time under the condition of extremely high sulfide content. However, the activity of the catalyst not prepared by the method of the present invention rapidly decays under the condition of extremely high sulfide content; When the sulfide content of the wastewater to be treated is extremely high, under the process conditions of high pressure and high temperature, a very high concentration of sulfate ions will be produced during the wet catalytic oxidation process, which can easily cause the active components to be stripped from the catalyst in the form of cations, resulting in a decrease in catalyst activity. The present invention uses low-cost non-precious metal oxides such as zinc oxide and iron oxide as active components, and aluminum oxide as a carrier. Within the ratio range selected by this method, the non-precious metal oxides can be highly dispersed in the aluminum oxide carrier, and the internal pores of the aluminum oxide can also play a limiting role to prevent the loss of active components. At the same time, during the preparation process of the present invention, a certain proportion of water is appropriately added, which produces a certain amount of mesopores during the drying and roasting process, so that the internal active potential of the catalyst can fully contact the pollutants in the wastewater, thereby improving the catalytic performance of the catalyst.

Claims

1. A method for preparing an extruded catalyst for treating oil refining alkali residue waste liquid, characterized in that: The method comprises the following steps: 1) Mix alumina, non-precious metal oxide, cross-linking agent and water in a certain proportion; 2) stirring and kneading the mixture of the catalyst base material and water until a clay is formed; 3) forming the clay into cylindrical particles of a certain diameter and length; 4) drying the cylindrical particles obtained in step 3) to obtain a semi-finished catalyst; 5) calcining the semi-finished catalyst to obtain a finished catalyst.

2. The method according to claim 1, characterized in that In step 1), the non-noble metal oxide is one or more of zinc oxide, iron oxide, zirconium oxide, and cerium oxide, or the non-noble metal oxide is a mixture of zinc oxide and iron oxide, and the adhesive is selected from water glass, glucose, glycerol, and a mixture thereof, or the adhesive is glycerol.

3. The method according to claim 1, characterized in that In step 1), the aluminum oxide has a particle size of 1 μm to 100 μm, and the non-noble metal oxide has a particle size of 0.1 μm to 1 μm.

4. The method according to claim 3, characterized in that The aluminum oxide has a particle size of 5 μm to 20 μm; and the non-noble metal oxide has a particle size of 0.1 μm to 0.3 μm.

5. The method according to claim 1, characterized in that In step 1), based on the total weight of the catalyst base material, the content of the non-noble metal oxide is 1% to 50%; the content of the aluminum oxide is 20% to 90%; the content of the adhesive is 1% to 30%; and the content of water is 20% to 50%.

6. The method according to claim 5, characterized in that The content of the non-noble metal oxide is 5% to 25%; the content of the aluminum oxide is 40% to 70%; the content of the adhesive is 5% to 15%; and the content of water is 25% to 40%.

7. The method according to claim 1, characterized in that When the molding is extrusion molding, the extrusion pressure is 1 MPa to 220 MPa; The drying temperature is 60°C to 400°C, the drying time is 0.5 h to 20 h, and the drying equipment is an oven, a hot air furnace, or a rail kiln; The calcination temperature is 200° C. to 900° C., and the calcination time is 1 h to 200 h.

8. The method according to claim 7, characterized in that The extrusion pressure is 1 MPa to 100 MPa; the drying temperature is 100°C to 200°C; the drying time is 0.8 h to 15 h, or 1 h to 12 h; the roasting temperature is 400°C to 600°C; and the roasting time is 2 h to 48 h.

9. An extruded catalyst for treating oil refining alkali residue waste liquid prepared by the method according to any one of claims 1 to 8.

10. The extruded catalyst for treating oil refining alkali residue waste liquid according to claim 9, characterized in that: The obtained cylindrical particles have a diameter of 1 to 20 mm and a length of 2 to 100 mm.

Citation Information

Patent Citations

  • Noble metal supported composite functional nano sphere catalyst having recoverability function and application thereof in catalyzing reduction of p-nitrophenol

    CN103157493A

  • Method for preparing catalyst for catalyzing organic pollutants in wet oxidation water

    CN103157501A

  • A wet oxidation catalyst for oil refinery waste alkali residue and its preparation method

    CN107442115B

  • Modified wet oxidation catalyst and its preparation method

    CN107442116A

  • Wet oxidation catalyst and its preparation method

    CN107442148A