Catalyst for preparing green methanol from biomass synthesis gas as well as preparation method and application of catalyst
By introducing highly dispersed metal oxides with multiple interface active sites into the CuO-ZnO-Al2O3 catalyst, the activity of the catalyst is improved, the problem of low CO2 conversion rate in biomass synthesis gas is solved, and efficient, low-cost green methanol production is achieved , promoting the high-value utilization of biomass resources and the realization of the "double carbon" goal.
Patent Information
- Application Number
- CN202410762541.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-13
AI Technical Summary
When existing technology uses biomass synthesis gas to produce green methanol, the CO2 conversion rate is low, resulting in large carbon emissions, complex processes and high costs, making it difficult to achieve large-scale low-carbon or zero-carbon production.
CuO-ZnO-Al2O3 nanocatalysts promoted by metal oxides with highly dispersed multiple interface active sites are used. Through surfactant-assisted co-precipitation and alkaline solution dealumination treatment, the specific surface area and pore volume of the catalyst are increased, and CO2 adsorption and Activation ability promotes the efficient conversion of CO2 in hydrogen-rich biomass synthesis gas into methanol.
It significantly improves the selectivity and yield of methanol, reduces carbon emissions, simplifies the process, reduces production costs, and is suitable for large-scale green methanol production.
Smart Images

Figure CN118767924A_ABST
Abstract
Description
Technical field:
[0001] The present invention belongs to the field of green methanol synthesis, and in particular relates to a catalyst for preparing green methanol from hydrogen-rich biomass synthesis gas, and a preparation method and application thereof. Background technology:
[0002] Green methanol is a safe, efficient, renewable clean energy. It is liquid at room temperature and pressure. It has unique advantages in storage and transportation, multifunctional application and market potential. Its safety level is equivalent to gasoline. At present, methanol production still mainly uses three traditional raw materials: coal, coke oven gas and natural gas. However, the traditional process has large carbon emissions, and the CO2 emissions per ton of methanol reach 3.5 tons. If large-scale low-carbon and zero-carbon production of methanol can be achieved, it will surely promote the green and safe development of my country's energy.
[0003] Biomass is the only zero-carbon renewable resource in nature, with the characteristics of abundant resources and wide distribution. Biomass organic solid wastes such as crop straw and livestock and poultry manure are the most valuable and abundant renewable resources on the earth. my country's annual straw production is 800 million tons and the annual livestock and poultry manure production is 3.05 billion tons, but most of them have not been effectively utilized, which greatly wastes biomass resources. At present, the production of green methanol (hereinafter referred to as green methanol) by coupling the biomass synthesis gas obtained by gasification of biomass with renewable energy power generation-hydrogen production by electrolysis of water can achieve near-zero CO2 emissions, and multiple sets of equipment have been planned or under construction. However, the typical composition of the synthesis gas obtained after gasification of straw biomass is about 45% CO, 33% H2, 20% CO2 (the remaining components are CH4, N2, H2S, HCl, NH3, etc.), and the ratio of (H2-CO2) / (CO+CO2) is only 0.2, which is far less than the 2 / 1 required for methanol synthesis. It is often necessary to increase the H2 content and reduce the CO2 content in the synthesis gas through processes such as water-gas shift and decarbonization to meet the needs of methanol synthesis, which is bound to cause a large amount of CO2 emissions, and the process is complicated and costly, which is not conducive to large-scale application. The previous patent CN117106485A of this team discloses a method for preparing hydrogen-rich biomass synthesis gas by coupling biomass through catalytic cracking, steam reforming and water-gas shift reaction. The hydrogen content in the obtained synthesis gas is 50-90%, which is an ideal raw material for preparing green methanol. How to efficiently convert it into methanol urgently needs in-depth research.
[0004] Traditional methanol synthesis is mainly carbon monoxide hydrogenation, and the typical catalyst is CuO-ZnO-Al2O3 catalyst, Cu / ZnO is considered to be the main active metal, and Al2O3 is mainly a structural additive. However, the efficiency of the traditional CO hydrogenation methanol synthesis catalyst CuO-ZnO-Al2O3 for CO2 conversion to methanol is low, especially for synthesis gas containing both CO and CO2, it is more inclined to convert CO, and it is difficult to convert CO2. Patent CN117282432A discloses a catalyst and preparation method for combining Cu / ZnO and oxide solid solution to achieve biomass gasification coupling renewable energy hydrogen production to synthesize green methanol, but the applicable raw gas composition of this type of catalyst is CO, CO2, H2, wherein the molar content of CO is 40% to 50%, the molar content of CO2 is 15% to 25%, the molar content of H2 is 25% to 45%, the CO conversion rate is ≤35%, and the CO2 conversion rate is <7%, which limits its application in green alcohol synthesis. Regarding the hydrogen-rich biomass synthesis gas with higher CO2 content (gas composition is 65-75% H2, 15-20% CO2, 5-10% CO, 2-5% CH4, 1-3% other hydrocarbons) produced by coupling catalytic cracking and steam reforming reactions of CN117106485A biomass, how to achieve its direct and effective conversion into green methanol is of great significance for accelerating the high-value utilization and resource utilization of biomass organic solid waste and promoting the realization of my country's "dual carbon" goals. Summary of the invention:
[0005] The present invention provides a catalyst for preparing green methanol from hydrogen-rich biomass synthesis gas, a preparation method and application thereof. The hydrogen-rich biomass synthesis gas is hydrogen-rich synthesis gas prepared by coupling biomass through catalytic cracking-steam reforming in a one-step process, and the gas composition is 65-75% H2, 15-20% CO2, 5-10% CO, 2-5% CH4, and 1-3% other hydrocarbons. The catalyst is a metal oxide-promoted CuO-ZnO-Al2O3 nanocatalyst with highly dispersed multiple interface active sites, which can realize efficient conversion of CO2 in the hydrogen-rich biomass synthesis gas into methanol.
[0006] The present invention is achieved through the following technical solutions:
[0007] A catalyst suitable for preparing green methanol from hydrogen-rich biomass synthesis gas, characterized in that the hydrogen-rich biomass synthesis gas is prepared by coupling biomass through catalytic cracking-steam reforming in a one-step process, see CN117106485A, and the gas composition is 65-75% H2, 15-20% CO2, 5-10% CO, 2-5% CH4, and 1-3% other hydrocarbons; the structural formula of the catalyst precursor is xCuO-yZnO-zAl2O3-mMO, wherein MO is a metal oxide, which is a mixture of one or two of CeO2 and TiO2; in the catalyst structural formula, x, y, z and m respectively represent the mass contents of CuO, ZnO, Al2O3 and the metal oxide MO, which are 50-60%, 20-30%, 5-15% and 5-15% respectively; when MO is a mixture of two of CeO2 and TiO2, the mixing ratio is 1:2 to 2:1.
[0008] The preparation method of the above catalyst comprises the following steps:
[0009] (1) dissolving a copper salt, a zinc salt, an aluminum salt and a precursor salt of a metal oxide MO in water to prepare a solution A, and dissolving a precipitant in water to prepare a solution B;
[0010] (2) adding solution A and solution B simultaneously dropwise to a container pre-filled with a certain amount of surfactant at a temperature of 60 to 70° C. for co-precipitation, controlling the pH of the solution to be 9.0 to 9.5, aging the resulting suspension solution at 80 to 90° C. for 3 to 6 hours, filtering, washing, drying, and calcining to obtain a catalyst precursor; the calcination temperature and time are 350 to 500° C. and 3 to 10 hours, respectively;
[0011] (3) The catalyst precursor is crushed, ground and sieved to >100 mesh, and then dealuminated using an alkaline solution at a temperature of 60 to 90° C. for 2 to 10 hours, and the catalyst is obtained after filtering, washing and drying.
[0012] In step (1), the copper salt is selected from one of copper nitrate, copper acetate or copper chloride; the zinc salt is selected from one of zinc nitrate, zinc acetate or zinc chloride; the aluminum salt is selected from one of aluminum nitrate, aluminum acetate or aluminum chloride; the precursor salt of the metal oxide MO is selected from at least one of cerium nitrate, cerium acetate, butyl titanate and titanium tetrachloride; the total concentration of the copper salt, zinc salt, aluminum salt and metal oxide MO precursor salt in the solution A is 0.2-1.5 mol / L; the precipitant is selected from one of a combination of sodium carbonate and sodium hydroxide and a combination of potassium carbonate and potassium hydroxide; the concentration of the precipitant in the solution B is 0.2-1.5 mol / L.
[0013] The surfactant in step (2) is selected from at least one of cetyltrimethylammonium bromide, cetyltrimethylammonium chloride, octadecyltrimethylammonium chloride, sodium dodecylbenzenesulfonate, sodium dodecyl sulfate, etc., and the ratio of its molar amount to the total concentration of copper salt, zinc salt, aluminum salt and metal oxide MO precursor salt in the solution A is 1:100 to 1:300; the drying temperature and time are 80 to 120°C and 10 to 24h, respectively.
[0014] Preferably, attapulgite powder is added to the surfactant in step (2) at the same time, and the added amount is 5% to 20% of the theoretical mass of the xCuO-yZnO-zAl2O3-mMO catalyst after calcination.
[0015] The alkaline solution in step (3) is an aqueous solution of sodium hydroxide or potassium hydroxide, the liquid-solid mass ratio in the dealumination process is 3:1 to 10:1, and the amount of the alkali is 5 to 20% of the mass of the catalyst.
[0016] The core innovation of the present invention is that based on the traditional CuO-ZnO-Al2O3 methanol synthesis catalyst, a unique surfactant-assisted co-precipitation method is adopted to form a nanocatalyst with highly dispersed multiple interface active sites with CeO2 or / and TiO2 oxide as a promoter and CuO-ZnO-Al2O3, and the specific surface area and pore volume of the catalyst are increased by alkaline solution dealumination treatment, thereby increasing the oxygen vacancy concentration, thereby promoting CO2 adsorption and activation to improve its conversion rate, and at the same time improving the synergistic effect of the Cu / ZnO interface and the interface of different metal oxides to enhance the rapid formation and conversion of methanol intermediates, so that the high-concentration CO2 in the hydrogen-rich biomass synthesis gas can be directly converted into methanol under the premise of a small amount of decarbonization, thereby achieving the purpose of increasing methanol production.
[0017] The present invention also provides an application of the above catalyst in green methanol synthesis, comprising the following steps: tabletting, crushing, screening and then loading the catalyst powder into a fixed bed reactor, introducing hydrogen-rich biomass synthesis gas (for the synthesis of hydrogen-rich biomass synthesis gas, see CN117106485A) at a temperature of 220-300°C, a raw gas pressure of 2-8MPa, and a volume space velocity of 2000-10000h -1The green methanol is prepared by catalytic conversion reaction under the following conditions, wherein the green methanol is a mixed alcohol mainly composed of methanol, and the methanol selectivity is ≥80%; the biomass is selected from at least one of bagasse, straw, bamboo chips, wood powder, kitchen waste, livestock and poultry manure, etc.; the main components of the hydrogen-rich biomass synthesis gas include H2, CO2, CO, CH4 and other hydrocarbons, wherein the molar content of H2 is 65-75%, the molar content of CO2 is 15-20%, the molar content of CO is 5-10%, the molar content of CH4 is 2-5%, and the molar content of other hydrocarbons is 1-3%. The other hydrocarbons include at least one of ethylene, ethane, propylene, propane, etc.
[0018] Preferably, the reaction temperature is 280-300°C, the feed gas pressure is 6-8MPa, and the volume space velocity is 2000-6000h -1 .
[0019] In the above application process, the reduction activation process of the catalyst is carried out at a temperature of 250-350°C, a pressure of 0.1-1 MPa, and a volume space velocity of 500-2000 h -1 The catalyst is reduced using hydrogen or a mixture of hydrogen and an inert gas for 2 to 12 hours, wherein the inert gas is selected from one of helium, nitrogen or argon, and the hydrogen content in the mixture is 5 to 100%.
[0020] The beneficial effects of the present invention are:
[0021] The catalyst of the present invention is a CuO-ZnO-Al2O3 catalyst promoted by metal oxides such as CeO2 and TiO2. A surfactant is added during the precipitation process to induce metal ions to form mixed metal oxide seeds in a solution or on the surface of attapulgite, thereby achieving full contact and good dispersion of active sites at the interfaces of different metal oxides. The specific surface area and pore volume of the catalyst are increased by alkaline solution dealumination treatment, the oxygen vacancy concentration is increased, the adsorption and activation of CO2 in hydrogen-rich biomass synthesis gas and the formation and conversion of methanol intermediates are promoted, so that the catalyst exhibits good catalytic performance in the conversion of hydrogen-rich biomass synthesis gas with a high CO2 content (15-20%) to produce green alcohol. The catalyst preparation method is simple, low in cost, and easy to achieve large-scale preparation, providing an ideal choice for large-scale production of green methanol.
[0022] Instruction manual drawings:
[0023] Figure 1 This is a scanning electron microscope photograph of the 50CuO-30ZnO-10Al2O3-10CeO2 catalyst prepared according to Example 1.
[0024] Figure 2This is a scanning electron microscope photograph of the 60CuO-30ZnO-5Al2O3-5CeO2@10ATP catalyst prepared according to Example 5. Specific implementation method:
[0025] The following is a further description of the present invention, rather than a limitation of the present invention.
[0026] According to the method disclosed in patent CN117106485A of our team, referring to Example 4, hydrogen-rich synthesis gas was prepared using food waste as raw material, wherein the molar content of H2 was 70%, the molar content of CO2 was 20%, the molar content of CO was 4.5%, the molar content of CH4 was 3.5%, and the molar content of other hydrocarbons was 2%.
[0027] The following Examples 1 to 3 use the biomass synthesis gas as raw material gas for methanol synthesis. Example 4 uses different raw materials to prepare biomass synthesis gas, and obtains synthesis gas with different compositions for methanol synthesis. Example 5 compares and investigates the effect of attapulgite addition on the green alcohol synthesis performance of the catalyst.
[0028] The micro fixed bed reactor used in the listed examples has an inner diameter of 8 mm and a length of 200 mm. The gas flow is regulated by a mass flow meter, the system pressure is regulated by a pressure reducer and a back pressure valve, and the reactor temperature is measured and regulated by a thermocouple and a temperature controller. After the reduction process (reduction conditions: pure hydrogen or a mixture of hydrogen and an inert gas, 250-350° C. for 2-12 h, pressure 0.1-1 MPa) is completed, the temperature is adjusted to the required temperature for the reaction, and then the synthesis gas is introduced to set the system pressure through the back pressure valve and the temperature is gradually increased for the reaction. The raw gas enters the reactor after being measured by a mass flow meter, and the cold trap separates the synthetic product and the tail gas. The tail gas enters the back pressure valve to release to normal pressure and then enters the six-way valve and is analyzed by an online GC 9800 gas chromatograph (Shanghai Kechuang), Ar is used as the carrier gas (flow rate 30 mL / min), and is detected by a thermal conductivity detector (TCD), and TDX-01 (2m×3mm) carbon molecular sieve is used as the chromatographic column; after the reaction is completed, the liquid product is collected and analyzed offline by an Agilent 7890 gas chromatograph, a hydrogen flame ionization detector (FID), and the chromatographic column is a FFAP capillary column (30m×0.25mm×0.25μm), and Ar is used as the carrier gas (flow rate 30mL / min).
[0029] According to the content of each component in the reaction tail gas, the carbon dioxide conversion rate in the synthesis gas and the methanol yield and selectivity are calculated by the molar number of carbon atoms. The calculation formula is as follows:
[0030] CO2 conversion rate = [n(CO2)in - n(CO2)out] / [n(CO2)in]
[0031] Methanol selectivity = n(MeOH) / [n(CO2)in - n(CO2)out]
[0032] Methanol space-time yield = m(MeOH) / [m(catalyst)×t]
[0033] In the formula, n(CO2)in and n(CO2)out are the molar numbers of CO2 in the feed gas and the tail gas, respectively; n(MeOH) and m(MeOH) are the molar number and mass of methanol in the product, respectively; m(catalyst) and t are the mass of the catalyst and the reaction time, respectively.
[0034] Embodiment 1:
[0035] Preparation and application of 50CuO-30ZnO-10Al2O3-10CeO2 catalyst:
[0036] 9.5g Cu(NO3)2·3H2O, 5.48g Zn(NO3)2·6H2O, 3.68g Al(NO3)3·9H2O and 1.26g Ce(NO3)2·6H2O were weighed and dissolved in 64.5mL water to prepare a metal salt solution A with a total metal ion concentration of 1.0mol / L; 10.6g anhydrous Na2CO3 and 4g NaOH were weighed and dissolved in 100mL water to prepare a precipitant solution B; 0.26g hexadecyltrimethylammonium bromide was weighed and fully dissolved in 20mL water, then added to a 250mL three-necked flask and heated to 70°C; solution A and solution B were simultaneously added dropwise to the beaker under stirring, and the mixture was stirred at 40°C. The pH value of the solution was controlled to be 9.0 by adjusting the dropping speed, and the precipitation was completed when the dropping of solution A was completed; the obtained suspension was heated to 80°C and aged for 6h, then filtered and washed to neutrality, the obtained filter cake was dried at 100°C for 24h and then calcined in an air atmosphere at 350°C for 6h to obtain a catalyst 50CuO-30ZnO-10Al2O3-10CeO2, which was crushed, ground and sieved to >100 mesh to obtain a catalyst precursor powder; 0.5g of sodium hydroxide was weighed and dissolved in 25g of water to prepare an alkaline solution, which was then heated to 80°C, 5g of the catalyst precursor powder was added thereto, stirred and reacted for 5h, then filtered and washed to neutrality, and the obtained filter cake was dried at 105°C for 12h to obtain a catalyst powder. Figure 1 is a SEM image of the catalyst in this Example 1. Figure 1 It can be seen that the catalyst prepared in this example is in the form of a large number of spherical particles uniformly dispersed on the surface of the flakes.
[0037] The catalyst powder was pressed into tablets, crushed and sieved to obtain catalyst particles of 60-80 mesh. 1g of the screened catalyst particles was weighed and loaded into the reactor. The temperature was 300℃, the pressure was 0.1MPa, and the air velocity was 2000h -1The catalyst was reduced using 10% H2 / Ar under the conditions of 10 h, and a synthesis gas with a composition of n(H2):n(CO2):n(CO):n(CH4):n(other hydrocarbons)=70:20:4.5:3.5:2 was introduced at a temperature of 220-300°C, a pressure of 5.0 MPa, and a space velocity of 4000 h -1 Methanol was synthesized under the following conditions. The reaction results are shown in Table 1. As can be seen from Table 1, with the increase of reaction temperature, the CO2 conversion rate and the time-space yield of methanol both gradually increase.
[0038] Table 1 Effect of reaction temperature on methanol synthesis performance
[0039] Reaction temperature (℃) <![CDATA[CO2 conversion rate (%)]]> Methanol selectivity (%) <![CDATA[Methanol space-time yield (g / g cat. ·h)]]> 220 7.8 93.5 0.23 240 12.5 88.3 0.47 260 17.2 85.1 0.65 280 22.7 82.9 0.82 300 26.1 80.5 1.05
[0040] Comparative Example 1:
[0041] The 50CuO-30ZnO-10Al2O3-10CeO2 catalyst was prepared by referring to the method of Example 1, crushed, tableted, and sieved to 60-80 mesh catalyst particles to obtain catalyst precursor powder, which was then directly used for green alcohol synthesis without alkali treatment. The reaction conditions were: temperature 280°C, pressure 5.0MPa, space velocity 4000h -1 The obtained CO2 conversion rate was 16.3%, the methanol selectivity was 78.5%, and the methanol space-time yield was 0.56 g / g cat. ·h.
[0042] Compared with the catalyst treated with alkali in Example 1, both the CO2 conversion rate and the methanol yield are significantly reduced. It can be seen that alkali treatment dealumination is crucial to improving the green alcohol synthesis performance of the catalyst. Catalyst alkali treatment and de-Al removal can not only increase the specific surface area and pore volume of the catalyst, improve the dispersion of metal Cu, promote the adsorption and dissociation of H2, but also increase the oxygen vacancy concentration of the catalyst, thereby promoting CO2 adsorption and activation to improve its conversion rate and methanol yield.
[0043] Embodiment 2:
[0044] Preparation and application of 60CuO-20ZnO-5Al2O3-5CeO2-10TiO2 catalyst:
[0045] 9.42gCu(CH3CO2)2·H2O, 3.66gZn(NO3)2·6H2O, 1.84gAl(NO3)3·9H2O, 0.57gCe(CH3CO2)3·4H2O and 2.13gCHO4Ti were weighed and dissolved in 141.1mL water to prepare a metal salt solution A with a total metal ion concentration of 0.5mol / L; 10.6g anhydrous Na2CO3 and 4gNaOH were weighed and dissolved in 200mL water to prepare a precipitant solution B; 0.25g octadecyltrimethylammonium chloride was weighed and fully dissolved in 20mL water, then added to a 500mL three-necked flask and heated to 60°C; solution A and solution B were simultaneously added dropwise to the flask under stirring. In the beaker, the pH value of the solution is controlled to be 9.2 by adjusting the dropping speed, and the precipitation is completed when the solution A is added dropwise; the obtained suspension is heated to 90°C and aged for 5h, then filtered and washed to neutrality, the obtained filter cake is dried at 120°C for 10h and then calcined in an air atmosphere at 500°C for 3h to obtain a catalyst 60CuO-20ZnO-5Al2O3-5CeO2-10TiO2, which is crushed, ground and sieved to >100 mesh to obtain a catalyst precursor powder; 0.25g of potassium hydroxide is weighed and dissolved in 50g of water to prepare an alkaline solution, which is then heated to 90°C, 5g of the catalyst precursor powder is added thereto, stirred and reacted for 10h, then filtered and washed to neutrality, and the obtained filter cake is dried at 110°C for 8h to obtain a catalyst powder.
[0046] The catalyst powder was pressed into tablets, crushed and sieved to obtain catalyst particles of 60-80 mesh. 1g of the screened catalyst particles was weighed and loaded into the reactor. The temperature was 250℃, the pressure was 0.5MPa, and the air velocity was 1000h -1 The catalyst was reduced with hydrogen for 2 h under the conditions of 250 °C, 2-8 MPa pressure, and 4000 h-1 gas. -1 Methanol was synthesized under the conditions. The reaction results are shown in Table 2. As can be seen from Table 2, with the increase of reaction pressure, the CO2 conversion rate and the space-time yield of methanol gradually increased.
[0047] Table 2 Effect of reaction pressure on methanol synthesis performance
[0048] Reaction pressure (MPa) <![CDATA[CO2 conversion rate (%)]]> Methanol selectivity (%) <![CDATA[Methanol space-time yield (g / g cat. ·h)]]> 2 12.5 81.8 0.32 4 14.1 83.5 0.55 6 17.9 89.7 0.79 8 21.6 92.1 1.07
[0049] Embodiment 3:
[0050] Preparation and application of 55CuO-25ZnO-10Al2O3-10TiO2 catalyst:
[0051] Weigh 5.82gCuCl2, 2.09gZnCl2, 2.0g(CH3CO2)3Al, 0.87gC 16 H 36 O4Ti was dissolved in 49.5mL water to prepare a metal salt solution A with a total metal ion concentration of 1.5mol / L; 20.73g of anhydrous K2CO3 and 8.42g of KOH were weighed and dissolved in 100mL of water to prepare a precipitant solution B; 0.25g of sodium dodecylbenzenesulfonate was weighed and fully dissolved in 20mL of water and then added to a 250mL three-necked flask and heated to 65°C; solution A and solution B were simultaneously added dropwise to the beaker under stirring, and the pH of the solution was controlled to 9.1 by adjusting the dropping speed. When the dropping of solution A was completed, the precipitation was completed; the resulting suspension The liquid was heated to 85°C and aged for 3h, then filtered and washed to neutrality. The filter cake was dried at 105°C for 15h and then calcined in an air atmosphere at 400°C for 10h to obtain a catalyst 55CuO-25ZnO-10Al2O3-10TiO2, which was crushed, ground and sieved to >100 mesh to obtain a catalyst precursor powder; 1g of sodium hydroxide was weighed and dissolved in 15g of water to prepare an alkaline solution, which was then heated to 60°C, 5g of the catalyst precursor powder was added thereto, stirred and reacted for 2h, then filtered and washed to neutrality, and the filter cake was dried at 100°C for 24h to obtain a catalyst powder.
[0052] The catalyst powder was tableted, crushed and sieved to obtain catalyst particles of 60-80 mesh. 1g of the screened catalyst particles was weighed and loaded into the reactor at a temperature of 350°C, a pressure of 1MPa and a space velocity of 500h. -1 The catalyst was reduced with 50% H2 / N2 for 6 h under the conditions of 260°C, 4 MPa, and 2000-10000 h / min. Synthesis gas with the composition of n(H2):n(CO2):n(CO):n(CH4):n(other hydrocarbons)=70:20:4.5:3.5:2 was introduced. -1 Methanol was synthesized under the conditions. The reaction results are shown in Table 3. As can be seen from Table 3, with the increase of the reaction space velocity, the CO2 conversion rate gradually decreases, but the methanol space-time yield gradually increases.
[0053] Table 3 Effect of reaction space velocity on methanol synthesis performance
[0054] <![CDATA[Space velocity (h -1 )]]> <![CDATA[CO2 conversion rate (%)]]> Methanol selectivity (%) <![CDATA[Methanol space-time yield (g / g cat. ·h)]]> 2000 20.2 85.6 0.41 4000 18.7 86.1 0.55 6000 16.3 87.2 0.73 8000 13.9 86.8 0.85 10000 11.4 87.0 1.02
[0055] Embodiment 4:
[0056] Preparation and application of 50CuO-20ZnO-15Al2O3-10CeO2-5TiO2 catalyst:
[0057] 9.5g Cu(NO3)2·3H2O, 2.7g (CH3CO2)2Zn·2H2O, 5.52g Al(NO3)3·9H2O, 1.92g Ce(NO3)2·6H2O and 0.59g TiCl4 were weighed and dissolved in 75.8mL water to prepare a metal salt solution A with a total metal ion concentration of 0.8mol / L; 16.6g anhydrous K2CO3 and 6.7g KOH were weighed and dissolved in 100mL water to prepare a precipitant solution B; 0.27g hexadecyltrimethylammonium bromide was weighed and fully dissolved in 20mL water, then added to a 250mL three-necked flask and heated to 65°C; solution A and solution B were simultaneously added dropwise to the beaker under stirring. The pH value of the solution is controlled to be 9.2 by adjusting the dropping speed, and the precipitation is completed when the solution A is added dropwise; the obtained suspension is heated to 80°C and aged for 5h, then filtered and washed to neutrality, the obtained filter cake is dried at 105°C for 12h and then calcined in an air atmosphere at 400°C for 5h to obtain a catalyst 50CuO-20ZnO-15Al2O3-10CeO2-5TiO2, which is crushed, ground and sieved to >100 mesh to obtain a catalyst precursor powder; 0.8g of sodium hydroxide is weighed and dissolved in 20g of water to prepare an alkaline solution, which is then heated to 75°C, 5g of the catalyst precursor powder is added thereto, stirred and reacted for 8h, then filtered and washed to neutrality, and the obtained filter cake is dried at 100°C for 20h to obtain a catalyst powder.
[0058] The catalyst powder was pressed into tablets, crushed and sieved to obtain catalyst particles of 60-80 mesh. 1g of the sieved catalyst particles was weighed and loaded into the reactor. The temperature was 280℃, the pressure was 0.5MPa, and the air velocity was 1000h -1 The catalyst was reduced with 10% H2 / He for 5 h under the same conditions, and hydrogen-rich synthesis gas prepared by catalytic cracking-steam reforming of five raw materials, namely sawdust, wheat straw, bagasse, branches and pig manure, was introduced at a temperature of 280 ° C, a pressure of 5.0 MPa and a space velocity of 5000 h -1 Methanol was synthesized under the following conditions. The reaction results are shown in Table 4. As can be seen from Table 4, the catalyst of the present invention can effectively convert hydrogen-rich synthesis gas produced by different biomass raw materials into green methanol, and has broad prospects for industrial application.
[0059] Table 4 Effect of biomass raw materials on methanol synthesis performance
[0060]
[0061] Embodiment 5:
[0062] Preparation and application of 60CuO-30ZnO-5Al2O3-5CeO2@ATP catalyst with different ATP addition amounts:
[0063] 9.11g Cu(NO3)2·3H2O, 5.48g Zn(NO3)2·6H2O, 1.84g Al(NO3)3·9H2O and 0.63g Ce(NO3)2·6H2O were weighed and dissolved in 57.52mL water to prepare a metal salt solution A with a total metal ion concentration of 1mol / L; 10.6g anhydrous Na2CO3 and 4g NaOH were weighed and dissolved in 100mL water to prepare a precipitant solution B; 0.23g hexadecyltrimethylammonium bromide CTAB and 0, 0.25, 0.5, 0.75, 1.0g attapulgite ATP were weighed and fully dissolved in 20mL water, then added into a 250mL three-necked flask and heated to 70°C; solution A was stirred. and solution B are added dropwise into the beaker at the same time, and the pH value of the solution is controlled to be 9.2 by adjusting the dropping speed. When the dropping of solution A is completed, the precipitation is completed; the obtained suspension is heated to 80°C and aged for 5h, then filtered and washed to neutrality, the obtained filter cake is dried at 100°C for 24h and then calcined in an air atmosphere at 450°C for 5h to obtain a catalyst 60CuO-30ZnO-5Al2O3-5CeO2@ATP, which is crushed, ground and sieved to >100 mesh to obtain a catalyst precursor powder; 0.5g of sodium hydroxide is weighed and dissolved in 25g of water to prepare an alkaline solution, which is then heated to 80°C, 5g of the catalyst precursor powder is added thereto, stirred and reacted for 5h, then filtered and washed to neutrality, and the obtained filter cake is dried at 105°C for 12h to obtain a catalyst powder.
[0064] The catalyst powder was pressed into tablets, crushed and sieved to obtain catalyst particles of 60-80 mesh. 1g of the screened catalyst particles was weighed and loaded into the reactor. The temperature was 250℃, the pressure was 0.5MPa, and the air velocity was 1000h -1 The catalyst was reduced using 10% H2 / N2 for 5 h under the conditions of 10% H2 / N2, and a synthesis gas with a composition of n(H2):n(CO2):n(CO):n(CH4):n(other hydrocarbons)=68:17.5:7.5:5:2 was introduced at a temperature of 280°C, a pressure of 6.0 MPa, and a space velocity of 5000 h -1 Methanol was synthesized under the conditions. The reaction results are shown in Table 5. It can be seen from Table 5 that with the increase in the amount of attapulgite, the conversion rate of CO2 and CO in the synthesis gas, the selectivity and yield of methanol first increased and then decreased, reaching the highest when its dosage was 10% of the theoretical mass of the catalyst. When its dosage was further increased, various performance indicators decreased. This is because during the co-precipitation process, adding attapulgite at the same time as the surfactant is added is conducive to the coating of the surfactant on the surface of the attapulgite, improving the adsorption capacity of attapulgite for metal ions and enhancing the dispersion of mixed metal oxide particles ( Figure 2), improve the performance of the catalyst; when the amount of attapulgite is too high, the number of hydrogenation metal species in the catalyst will be reduced, thereby reducing the catalytic performance of the synthesis gas conversion to green alcohol. It can be seen that the present invention provides a high-performance catalyst for the conversion of hydrogen-rich biomass synthesis gas with a high CO2 content to produce green methanol, which can realize the simultaneous conversion of CO and CO2 in the synthesis gas to produce green methanol.
[0065] Table 5 Effect of attapulgite addition on methanol synthesis performance
[0066]
[0067] The above embodiments illustrate a catalyst for directly preparing green methanol from biomass synthesis gas provided by the present invention, as well as its preparation method and application, to help understand the method of the present invention and its core idea. It should be pointed out that for those skilled in the art, without departing from the principles of the present invention, several improvements and modifications can be made to the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A catalyst suitable for preparing green methanol from hydrogen-rich biomass synthesis gas, It is characterized in that The hydrogen-rich biomass synthesis gas is produced by coupling biomass through catalytic cracking and steam reforming in one step, and the gas composition is 65-75% H 2 15-20% CO 2 , 5-10% CO, 2-5% CH 4 , 1 to 3% other hydrocarbons; the structural formula of the catalyst precursor is xCuO-yZnO-zAl 2 O 3 -mMO, where MO is a metal oxide, CeO 2 、TiO 2 In the catalyst structure, x, y, z and m represent CuO, ZnO, Al 2 O 3 and metal oxide MO, are 50-60%, 20-30%, 5-15% and 5-15% respectively; when MO is CeO 2 、TiO 2 When the mixture of the two is prepared, the mixing ratio is 1:2 to 2:1; the preparation method of the catalyst comprises the following steps: (1) dissolving a copper salt, a zinc salt, an aluminum salt and a precursor salt of a metal oxide MO in water to prepare a solution A, and dissolving a precipitant in water to prepare a solution B; (2) adding solution A and solution B simultaneously dropwise to a container pre-filled with a certain amount of surfactant at a temperature of 60 to 70° C. for co-precipitation, controlling the pH of the solution to be 9.0 to 9.5, aging the resulting suspension solution at 80 to 90° C. for 3 to 6 hours, filtering, washing, drying, and calcining to obtain a catalyst precursor; the calcination temperature and time are 350 to 500° C. and 3 to 10 hours, respectively; (3) The catalyst precursor is crushed, ground and sieved to >100 mesh, and then dealuminated using an alkaline solution at a temperature of 60 to 90° C. for 2 to 10 hours, and the catalyst is obtained after filtering, washing and drying.
2. The catalyst according to claim 1, It is characterized in that In step (1), the copper salt is selected from one of copper nitrate, copper acetate or copper chloride; the zinc salt is selected from one of zinc nitrate, zinc acetate or zinc chloride; the aluminum salt is selected from one of aluminum nitrate, aluminum acetate or aluminum chloride; the precursor salt of the metal oxide MO is selected from at least one of cerium nitrate, cerium acetate, butyl titanate and titanium tetrachloride; the total concentration of the copper salt, zinc salt, aluminum salt and metal oxide MO precursor salt in the solution A is 0.2-1.5 mol / L; the precipitant is selected from one of a combination of sodium carbonate and sodium hydroxide and a combination of potassium carbonate and potassium hydroxide; the concentration of the precipitant in the solution B is 0.2-1.5 mol / L.
3. The catalyst according to claim 1, It is characterized in that The surfactant in step (2) is selected from at least one of cetyltrimethylammonium bromide, cetyltrimethylammonium chloride, octadecyltrimethylammonium chloride, sodium dodecylbenzenesulfonate, sodium dodecyl sulfate, etc., and the ratio of its molar amount to the total concentration of copper salt, zinc salt, aluminum salt and metal oxide MO precursor salt in the solution A is 1:100 to 1:300; the drying temperature and time are 80 to 120°C and 10 to 24h, respectively.
4. The catalyst according to claim 1, It is characterized in that At the same time, attapulgite powder is added to the surfactant in step (2), and the addition amount is xCuO-yZnO-zAl 2 O 3 -5% to 20% of the theoretical mass of the mMO catalyst after calcination.
5. The catalyst according to claim 1, It is characterized in that The alkaline solution in step (3) is an aqueous solution of sodium hydroxide or potassium hydroxide, the liquid-solid mass ratio in the dealumination process is 3:1 to 10:1, and the amount of the alkali is 5 to 20% of the mass of the catalyst.
6. Use of the catalyst according to claim 1, It is characterized in that The method comprises the following steps: tabletting, crushing and screening the catalyst powder and then loading it into a fixed bed reactor; introducing hydrogen-rich biomass synthesis gas after reduction activation; and heating the catalyst powder at a temperature of 220 to 300°C, a raw gas pressure of 2 to 8 MPa, and a volume space velocity of 2000 to 10000 h / min. -1 The catalytic conversion reaction is carried out under the following conditions to produce green methanol; the main components of the hydrogen-rich biomass synthesis gas include H 2 , CO 2 , CO, CH 4 and other hydrocarbons, among which H 2 The molar content is 65-75%, CO 2 The molar content of is 15-20%, the molar content of CO is 5-10%, and the molar content of CH 4 The molar content of is 2-5%, and the molar content of other hydrocarbons is 1-3%.
7. The use according to claim 5, It is characterized in that The biomass is selected from at least one of bagasse, straw, bamboo chips, wood chips, branches, bark, kitchen waste, livestock and poultry manure, etc.; the other hydrocarbons include at least one of ethylene, ethane, propylene, and propane.
8. The use according to claim 5, It is characterized in that The reduction activation process of the catalyst is carried out at a temperature of 250-350°C, a pressure of 0.1-1 MPa, and a volume space velocity of 500-2000 h -1 The catalyst is reduced using hydrogen or a mixture of hydrogen and an inert gas for 2 to 12 hours, wherein the inert gas is selected from one of helium, nitrogen or argon, and the hydrogen content in the mixture is 5 to 100%.
9. The use according to claim 5, It is characterized in that The reaction temperature is 280-300℃, the feed gas pressure is 6-8MPa, and the volume space velocity is 2000~6000h -1 .
10. The use according to claim 5, It is characterized in that The green methanol is a mixed alcohol mainly composed of methanol, and the methanol selectivity is ≥80%.
Citation Information
Patent Citations
Attapulgite-based composite material loaded Cu-Zn-Fe based catalyst, preparation method and applications thereof
CN104815664A
Method for producing hydrogen through cyclic catalytic reaction of biomass waste
CN117106485A
Catalyst for synthesizing green methanol by coupling biomass gasification with renewable energy hydrogen production as well as preparation method and application of catalyst
CN117282432A