Preparation method of ruthenium-based catalyst carrier, ruthenium-based catalyst and application of ruthenium-based catalyst carrier
FeCrAl alloy is prepared by hydrothermal method and combined with aging treatment and high-voltage electric field drying technology, which solves the problems of catalyst stability and high cost in the existing ammonia synthesis process, and achieves high-efficiency and low-cost ammonia synthesis catalytic effect.
Patent Information
- Application Number
- CN202310357084.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-15
AI Technical Summary
Existing ammonia synthesis processes such as the Haber-Bosch process have high energy consumption, high catalyst costs and poor stability, making it difficult to produce on a large scale in factories, and alternatives are not yet mature.
FeCrAl alloy was prepared using a hydrothermal method as a ruthenium-based catalyst carrier. The mechanical properties and catalytic activity stability of the catalyst were improved through aging treatment and high-voltage electric field drying technology, and Ru elements were impregnated with negative charges to improve catalytic performance.
It achieves efficient catalytic synthesis of ammonia from nitrogen and hydrogen under mild conditions, with high catalytic activity and good stability. The process is simple and low-cost, making it suitable for industrial production.
Smart Images

Figure CN118767931A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts for ammonia synthesis, and in particular to a method for preparing a ruthenium-based catalyst carrier, a ruthenium-based catalyst and application thereof in ammonia synthesis. Background Art
[0002] For the past 100 years, the Haber-Bosch process has been based on the use of nitrogen (N 2 ) and hydrogen (H 2 ) Production of NH 3 Unfortunately, this NH 3 The production of carbon dioxide results in a very large energy consumption, accounting for almost 2% of the total global primary energy consumption. In addition, the use of fossil fuels for synthesis releases about 3×10 -8 t tons of CO2. While the HB process has been fine-tuned and its efficiency has been massively improved over the period. Catalyst development for the process has been extensively studied, with fused iron catalysts developed in the 70s being the most efficient catalyst to date, the cost of more active metals has been prohibitive.
[0003] Patent application CN114653359A reports a catalyst for synthesizing ammonia made of a composite metal oxide composed of zinc, bismuth and zirconium. The pressure of the synthesis reaction is 20 kPa (A), the reaction temperature is 140°C, the conversion rate of urea is 99.5%, the yield of ammonia is 96.8%, and the yield of ethylene carbonate is 81.1%. However, its operation process is complicated, the required raw materials are highly toxic, and it is difficult to produce on a large scale in a factory.
[0004] Patent application CN114733551A reports a high-performance ruthenium-based mild ammonia synthesis catalyst and its preparation method and application. The Ru / BN catalyst is synthesized by synthesizing a BN carrier, and then the rare earth element is loaded on the Ru / BN catalyst by an equal volume impregnation method, and finally a RuM / BN catalyst is obtained. The catalyst has a high ammonia yield of 43.8 mmol g at 400 °C and 1 MPa. cat -1 h -1 The ammonia synthesis rate was increased, but the catalyst could only run for 140 h and the stability problem was not solved.
[0005] Patent application CN114789053A reports a ruthenium-based mild ammonia synthesis catalyst, its preparation method and its application. The catalyst comprises an active component Ru, an additive and a carrier Zr. 2 or ZrO 2 Composition modulation N 2The activation path of the catalyst can achieve the modulation of the performance of synthetic ammonia under mild conditions. The catalyst can reach 35.3mmol g cat -1 h -1 The ammonia synthesis rate is increased, but according to the data of the patent application, although it can run smoothly for 300 hours, the performance of the catalyst is significantly inferior to that of other inventions.
[0006] In summary, there is an urgent need to develop an alternative to the HB process in my country. Summary of the invention
[0007] Based on this, the present invention provides a preparation method of a ruthenium-based catalyst carrier, a ruthenium-based catalyst and its application. The ruthenium-based catalyst provided by the present invention has good catalytic performance in the reaction of catalyzing nitrogen and hydrogen to synthesize ammonia, has high catalytic activity and good stability, and has a simple preparation method and low cost.
[0008] To achieve the purpose, the present invention provides the following technical solutions:
[0009] The first aspect of the present invention provides a method for preparing a ruthenium-based catalyst carrier, the preparation method comprising the following steps:
[0010] 1) Mixing the mixed solution I and the mixed solution II, stirring, heating to 200-300° C. for reaction, preferably for 2-4 hours, reducing the metal ions in the solution to form nano-metal powders, then washing the nano-metal powders with nitric acid solution and deionized water until the washing solution is neutral, and then drying;
[0011] Wherein, the mixed solution I is Fe 3+ Cr 2+ 、Al 3+ The precursor salt is Na 2 CO 3 A mixed solution formed in the solution;
[0012] The mixed solution II is a mixed solution of acetic acid solution and NaOH solution;
[0013] 2) subjecting the nano metal powder obtained in step 1) to aging treatment, and obtaining the ruthenium-based catalyst carrier after cooling, which is an iron-chromium-aluminum alloy.
[0014] In the process of preparing a ruthenium-based catalyst carrier, the present invention prepares an alloy by a hydrothermal method at 200-300°C using mixed solution I and mixed solution II. Compared with the traditional alloy preparation process, it not only greatly reduces energy consumption, but also makes the operation simpler and easy to industrialize. After the alloy is prepared by the hydrothermal method, it is further rinsed with nitric acid solution and deionized water to reduce the zero-point charge of the alloy, which is beneficial to the final carrier to better adsorb active metal components such as ruthenium when preparing a ruthenium-based catalyst, thereby improving the catalytic activity; after the nano-metal powder is prepared, the aging treatment is continued, which is beneficial to greatly improve the mechanical properties of the ruthenium-based catalyst carrier, and is beneficial to ultimately improve the catalytic activity stability of the ruthenium-based catalyst. The ruthenium-based catalyst carrier obtained by the preparation method of the present invention is used to prepare an ammonia synthesis reaction catalyst, which is beneficial to improve the catalytic activity and stability of the catalyst.
[0015] In some preferred embodiments, in step 1), the Fe 3+ Cr 2+ 、Al 3+ The molar ratio is 1:(0.126-0.306):(0.138-0.588); adopting the preferred molar ratio is beneficial to improving the catalytic activity of the catalyst in catalyzing the synthesis of ammonia from nitrogen and hydrogen.
[0016] In the present invention, Fe 3+ Cr 2+ 、Al 3+ There is no particular limitation on the precursor salt, preferably, FeCl 3 CrCl 2 、AlCl 3 As a precursor salt.
[0017] In some preferred embodiments, in step 1), the Na 2 CO 3 The concentration of the solution is 1-2 M. In some embodiments, Na 2 CO 3 The total amount is twice the molar amount of iron ions, but is not limited thereto, for example, 1.5-3 times.
[0018] In some preferred embodiments, in step 1), when preparing the mixed solution I, the precursor salt is added to the Na 2 CO 3 In the solution, preferably, stirring is carried out under strong magnetic stirring, and the stirring speed is preferably 300-500 r / min. The preferred stirring conditions are conducive to obtaining carrier particles with relatively uniform and fine particle sizes, which is conducive to further improving the performance of the subsequently obtained ruthenium-based catalyst.
[0019] In some preferred embodiments, in the mixed solution II of step 1), the concentrations of the acetic acid solution and the NaOH solution are 1-2 M respectively; preferably, in the mixed solution II, the acetic acid and the NaOH have the same molar amount; further preferably, the mixed solution II is a mixture of the acetic acid solution and the NaOH solution of the same concentration and the same volume, and this method is used to prepare the mixed solution II.
[0020] In some preferred embodiments, in step 1), the total molar amount of acetate ions in the mixed solution II is 3+ 2-6 times of the total molar amount, adopting the preferred dosage relationship is conducive to ensuring complete reduction of metal ions.
[0021] In some preferred embodiments, it is characterized in that, in step 1), the mixed solution I and the mixed solution II are mixed and stirred at a speed of 80-100 r / min, and preferably, the mixing process is carried out in a titanium autoclave;
[0022] In some preferred embodiments, in step 1), the drying is performed under vacuum, preferably at a temperature of 100 to 120° C. and for 8 to 12 hours.
[0023] In the present invention, in step 1), the nano metal powder is rinsed with nitric acid solution and deionized water until the washing solution is neutral, wherein the nitric acid solution is mainly used to wash and remove impurities, and the amount of nitric acid solution and deionized water is not particularly limited. Specifically, the two washings are preferably performed alternately for multiple times, and the specific amount is based on the final rinse to neutral. In some preferred embodiments, in step 1), the pH of the nitric acid solution is 2 to 4. Using a nitric acid solution with a preferred pH for washing can not only achieve a good cleaning effect, but also will not corrode the powder; if the acid is too strong, it may cause corrosion, and if the acid is too weak, it may not be possible to achieve the purpose of cleaning residues.
[0024] In some preferred embodiments, in step 2), the conditions of the aging treatment include: a temperature of 100 to 150° C., a time of 6 to 12 hours, and a protective gas, preferably nitrogen or argon. Specifically, the aging treatment can be carried out in a tubular furnace. Aging treatment at the above preferred temperature and time is beneficial to improving the hardness and strength of the carrier, and is beneficial to improving the performance of the ruthenium-based catalyst finally obtained.
[0025] A second aspect of the present invention provides a method for preparing a ruthenium-based catalyst, comprising the following steps:
[0026] S1, immersing a ruthenium-based catalyst support in an impregnation liquid containing ruthenium ions, and connecting an external power supply to make the surface of the ruthenium-based catalyst support negatively charged, and removing the upper layer of liquid after the impregnation to retain the residue; the ruthenium-based catalyst support is prepared by the preparation method described above;
[0027] S2. Drying the residue from step 1) using a high-voltage electric field drying technique to obtain the ruthenium-based catalyst.
[0028] The ruthenium-based catalyst prepared by the above method using the ruthenium-based catalyst carrier of the present invention is particularly suitable for catalyzing the synthesis of ammonia from nitrogen and hydrogen, and the catalyst exhibits extremely high ammonia synthesis performance under mild conditions. The present invention prepares the ruthenium-based catalyst based on the ruthenium-based catalyst carrier prepared by a specific process. During the process of impregnating the loaded ruthenium element, a negative charge is applied to the carrier, which can make it easier to adsorb Ru in the impregnation solution. 3+ Ions are conducive to making better use of precious metals, improving utilization efficiency, saving costs, and improving catalyst performance. After impregnation, high-voltage electric field drying technology is used for drying, which not only has high drying efficiency and low energy consumption, but also enables water molecules to move freely on the inner and outer surfaces of the catalyst, forming more pores, increasing the specific surface area of the catalyst, and thus helping to improve catalytic performance. The ruthenium-based catalyst prepared by the method of the present invention has excellent electrical conductivity, mechanical strength and catalytic activity in the reaction of catalyzing nitrogen and hydrogen to synthesize ammonia. The obtained catalyst not only has high catalytic activity, but also has better catalytic activity stability, low cost, and simple preparation process.
[0029] In some embodiments, in step S1, the ruthenium ions in the impregnation solution come from a ruthenium precursor salt, and the ruthenium precursor salt can be selected from but not limited to one or more of ruthenium acetylacetonate, ruthenium nitrosyl nitrate, ruthenium trichloride, and ruthenium acetate;
[0030] In some preferred embodiments, in step S1, the amount of ruthenium ions used is 2 to 4 wt% based on the mass of the carrier; using the preferred ruthenium element loading amount not only makes it less likely to agglomerate, but also allows for excellent catalytic activity.
[0031] In some preferred embodiments, in step S1, the voltage of the external power supply is 10-20V, and the impregnation time is 8-12h; the preferred voltage range is beneficial to the effective loading of the active component and to improve the catalytic performance of the ruthenium-based catalyst finally obtained. In some preferred embodiments, in step S2, when the high-voltage electric field drying technology is used for drying, the electric field strength is 10-20kV / cm, and the drying time is, for example, but not limited to, 8h.
[0032] In some specific embodiments, in step S1, the impregnation liquid is an aqueous solution of a ruthenium precursor salt. Specifically, some ethanol can be added thereto. For example, the impregnation liquid is obtained by adding a ruthenium precursor salt solution into ethanol and stirring. Adding ethanol is conducive to more uniform dispersion. There is no particular restriction on the amount of solvent used, as long as good dispersion and dissolution can be achieved.
[0033] The present invention also provides a ruthenium-based catalyst prepared by the preparation method described above. The ruthenium-based catalyst provided by the present invention is particularly suitable for catalyzing the synthesis of ammonia from nitrogen and hydrogen under mild conditions, and the catalyst has excellent catalytic activity. In some embodiments, the reaction conditions for synthesizing ammonia from nitrogen and hydrogen in the presence of the ruthenium-based catalyst of the present invention include: a reaction temperature of 350 to 400° C., a reaction pressure of 1 to 1.5 MPa, and a raw gas mass ratio of, for example, but not limited to, n(N 2 ):n(H 2 )=1:3, mass space velocity is 50000~60000mL·g -1 ·h -1 .
[0034] Another aspect of the present invention provides use of the ruthenium-based catalyst described above in a synthetic ammonia reaction. Preferably, the ruthenium-based catalyst is used as a catalyst in a catalytic reaction of synthesizing ammonia from nitrogen and hydrogen.
[0035] The technical solution provided by the present invention has the following beneficial effects:
[0036] The ruthenium-based catalyst carrier prepared by the preparation method of the present invention is easy to prepare a catalyst having excellent catalytic activity and good catalytic stability, which is particularly suitable for ammonia synthesis. The catalyst has good mechanical properties and can well adsorb active metal elements such as ruthenium, which is beneficial to improving the catalytic activity and stability of the catalyst. A ruthenium-based catalyst carrier provided by the present invention is prepared, which is particularly suitable for catalyzing the synthesis of ammonia from nitrogen and hydrogen. A negative charge is applied during the impregnation of the loaded ruthenium, and a high-voltage electric field drying technology is used for drying after the impregnation is completed. The catalyst finally obtained has excellent electrical conductivity, mechanical strength and catalytic activity, and exhibits excellent catalytic activity stability.
[0037] The preparation process of the ruthenium-based catalyst carrier and the ruthenium-based catalyst provided by the present invention has the characteristics of easy availability of reagents, non-toxicity, simple process, etc., and is easy to mass produce and realize industrialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 It is a summary diagram of the ammonia synthesis reaction experimental results obtained in the examples and comparative examples;
[0039] Figure 2This is the XRD characterization diagram of the FeCrAl alloy and catalyst in Example 1 (corresponding to 2% Ru / FeCrAl in the figure). DETAILED DESCRIPTION
[0040] In order to facilitate the understanding of the present invention, the present invention will be further described below in conjunction with examples. It should be understood that the following examples are only for a better understanding of the present invention and do not mean that the present invention is limited to the following examples.
[0041] Where specific experimental steps or conditions are not specified in the examples, the corresponding conventional experimental steps or conditions in the art can be used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be purchased commercially.
[0042] In the examples or comparative examples, all reagents used are commercially available products, FeCl 3 CrCl 2 、AlCl 3 The purity was >99.5% and no further purification was required.
[0043] In the examples and comparative examples, during the ammonia synthesis reaction, NH in the tail gas was measured by ion chromatography. 3 The concentration is used to calculate the synthesis rate of ammonia, which is used to reflect the ammonia synthesis performance of the catalyst.
[0044] Example 1
[0045] A ruthenium-based catalyst for ammonia synthesis reaction, the preparation method comprising the following steps:
[0046] 1) Preparation of carrier:
[0047] Weigh 162.2g FeCl 3 、35.3g CrCl 2 and 18.94 g AlCl 3 Mix well, then add 2L of 1M Na 2 CO 3 aqueous solution to obtain a mixed solution I.
[0048] 3 L of acetic acid aqueous solution and NaOH aqueous solution, both with a concentration of 2 M, were taken and mixed to obtain a mixed solution II.
[0049] The mixed solutions I and II were mixed and stirred at a stirring rate of 80 r / min in a titanium autoclave, and then the temperature was raised to 200°C and maintained for 2 hours to reduce the metal ions in the solution to nano-metal powders. The nano-metal powders formed in the titanium autoclave were then repeatedly rinsed with nitric acid solution (pH = 2, each amount was about 1 times the mass of the nano-metal powder) and deionized water alternately until the washing solution was neutral, and then vacuum dried at 120°C for 8 hours.
[0050] Finally, the nano-metal powder was subjected to aging treatment in a tubular furnace under a nitrogen atmosphere at a temperature of 100° C. for 6 h, and the FeCrAl carrier 1 (hereinafter referred to as “carrier 1”) was obtained after natural cooling.
[0051] 2) Preparation of catalyst:
[0052] Pour 10 mL of ethanol into a culture dish, then pour 2 mL of a 0.989 M ruthenium trichloride aqueous solution, stir thoroughly, and obtain an immersion solution.
[0053] 10 g of carrier 1 was added to the above-mentioned impregnation solution, and a 15 V negative power supply was connected to the surface of carrier 1 to make it negatively charged. After impregnation for 8 hours, the upper liquid was filtered out, and then a high-voltage electric field drying device was used to dry the residue at an intensity of 15 kV / cm for 8 hours to obtain Ru / FeCrAl catalyst 1 (hereinafter referred to as "catalyst 1") for synthetic ammonia reaction.
[0054] 3) Application of catalyst 1 in ammonia synthesis reaction:
[0055] 0.2 g of catalyst 1 was weighed and reacted in a continuous flow micro fixed bed reactor at a reaction pressure of 1 MPa, a temperature of 400 °C, and a mass space velocity of 60000 mL g -1 ·h -1 The ammonia synthesis performance was measured; the amount of substance introduced was n(N 2 ):n(H 2 )=1:3N 2 and H 2 At the beginning of the reaction, the ammonia synthesis rate of catalyst 1 (corresponding to Figure 1 The "highest activity" in the above table is 32.8 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 1 (corresponding to Figure 1 The "400-hour activity" in the above text is 31.6 mmol gcat -1 h -1 , with better catalytic activity and catalytic activity stability.
[0056] Figure 2Shown is the XRD characterization diagram of the FeCrAl carrier 1 and the catalyst (i.e., 2% Ru / FeCrAl in the figure) prepared in Example 1. It can be seen that the dispersion of ruthenium in the prepared catalyst is very good.
[0057] Example 2
[0058] A ruthenium-based catalyst for ammonia synthesis reaction, the preparation method comprising the following steps:
[0059] 1) Preparation of carrier:
[0060] Weigh 162.2g FeCl 3 、35.3g CrCl 2 and 78.4 g AlCl 3 Mix well, then add 2L of 1M Na 2 CO 3 aqueous solution to obtain a mixed solution I.
[0061] 3 L of acetic acid aqueous solution and NaOH aqueous solution, both with a concentration of 2 M, were taken and mixed to obtain a mixed solution II.
[0062] The mixed solutions I and II were mixed and stirred at a stirring rate of 100 r / min in a titanium autoclave, and then the temperature was raised to 200°C and maintained for 3 hours to reduce the metal ions in the solution to nano-metal powders. The nano-metal powders formed in the titanium autoclave were then rinsed alternately with nitric acid solution (pH = 4, each amount was about 1 times the mass of the nano-metal powder) and deionized water until the washing solution was neutral, and then vacuum dried at 120°C for 10 hours.
[0063] Finally, the nano-metal powder was subjected to aging treatment in a tubular furnace under a nitrogen atmosphere at a temperature of 100° C. for 6 h, and the FeCrAl carrier 2 (hereinafter referred to as “carrier 2”) was obtained after natural cooling.
[0064] 2) Preparation of catalyst:
[0065] Pour 10 mL of ethanol into a culture dish, then pour 2.5 mL of a 0.989 M ruthenium trichloride aqueous solution, stir thoroughly, and obtain an immersion solution.
[0066] 10 g of carrier 2 was added to the above-mentioned impregnation solution, and a 20 V negative power supply was connected to the surface of carrier 2 to make it negatively charged. After impregnation for 10 hours, the upper liquid was filtered out, and then a high-voltage electric field drying device was used to dry the residue at an intensity of 15 kV / cm for 8 hours to obtain Ru / FeCrAl catalyst 2 (hereinafter referred to as "catalyst 2") for synthetic ammonia reaction.
[0067] 3) Application of catalyst 2 in ammonia synthesis reaction:
[0068] The ammonia synthesis catalytic performance test of Catalyst 2 was carried out with reference to the reaction conditions of Example 1.
[0069] At the beginning of the reaction, the ammonia synthesis rate of catalyst 2 was 31.6 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 2 was 30.5 mmol gcat -1 h -1 , with better catalytic activity and catalytic activity stability.
[0070] Example 3
[0071] A ruthenium-based catalyst for ammonia synthesis reaction, the preparation method comprising the following steps:
[0072] 1) Preparation of carrier:
[0073] Weigh 162.2g FeCl 3 、15.5g CrCl 2 and 35.2 g AlCl 3 Mix well, then add 2L of 1M Na 2 CO 3 aqueous solution to obtain a mixed solution I.
[0074] 3 L of acetic acid aqueous solution and NaOH aqueous solution, both with a concentration of 2 M, were taken and mixed to obtain a mixed solution II.
[0075] The mixed solutions I and II were mixed and stirred at a stirring rate of 85 r / min in a titanium autoclave, and then the temperature was raised to 250°C and maintained for 3 hours to reduce the metal ions in the solution to nano-metal powders. The nano-metal powders formed in the titanium autoclave were then repeatedly rinsed with nitric acid solution (pH = 2.5, each amount was about 1 times the mass of the nano-metal powder) and deionized water alternately until the washing solution was neutral, and then vacuum dried at 120°C for 12 hours.
[0076] Finally, the nano-metal powder was subjected to aging treatment in a tubular furnace under an argon atmosphere at a temperature of 120° C. for 8 h, and FeCrAl carrier 3 (hereinafter referred to as “carrier 3”) was obtained after natural cooling.
[0077] 2) Preparation of catalyst:
[0078] Pour 10 mL of ethanol into a culture dish, then pour 2.5 mL of a 0.989 M ruthenium trichloride aqueous solution, stir thoroughly, and obtain an immersion solution.
[0079] 10 g of carrier 3 was added to the above-mentioned impregnation solution, and a 10 V negative power supply was connected to the surface of carrier 3 to make it negatively charged. After impregnation for 12 hours, the upper liquid was filtered out, and then a high-voltage electric field drying device was used to dry the residue at an intensity of 10 kV / cm for 8 hours to obtain Ru / FeCrAl catalyst 3 (hereinafter referred to as "catalyst 3") for synthetic ammonia reaction.
[0080] 3) Application of catalyst 3 in ammonia synthesis reaction:
[0081] The ammonia synthesis catalytic performance of catalyst 3 was tested under the reaction conditions of Example 1. In the initial stage of the reaction, the ammonia synthesis rate of catalyst 3 was 31.5 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 3 was 30.5 mmol gcat -1 h -1 , with better catalytic activity and catalytic activity stability.
[0082] Example 4
[0083] A ruthenium-based catalyst for ammonia synthesis reaction, the preparation method comprising the following steps:
[0084] 1) Preparation of carrier:
[0085] Weigh 162.2g FeCl 3 、37.6g CrCl 2 and 78.4 g AlCl 3 Mix well, then add 2L of 1M Na 2 CO 3 aqueous solution to obtain a mixed solution I.
[0086] 3 L of acetic acid aqueous solution and NaOH aqueous solution, both with a concentration of 2 M, were taken and mixed to obtain a mixed solution II.
[0087] The mixed solutions I and II were mixed and stirred at a stirring rate of 90 r / min in a titanium autoclave, and then the temperature was raised to 300°C and maintained for 4 hours to reduce the metal ions in the solution to nano-metal powders. The nano-metal powders formed in the titanium autoclave were then rinsed alternately with nitric acid solution (pH=3, each amount was about 1 times the mass of the nano-metal powder) and deionized water until the washing solution was neutral, and then vacuum dried at 120°C for 8 hours.
[0088] Finally, the nano-metal powder was subjected to aging treatment in a tubular furnace under an argon atmosphere at a temperature of 150° C. for 10 h, and after natural cooling, the FeCrAl carrier 4 (hereinafter referred to as “carrier 4”) was obtained.
[0089] 2) Preparation of catalyst:
[0090] Pour 10 mL of ethanol into a culture dish, then pour 2 mL of a 0.989 M ruthenium trichloride aqueous solution, stir thoroughly, and obtain an immersion solution.
[0091] 10 g of carrier 4 was added to the above-mentioned impregnation solution, and a 14 V negative power supply was connected to the surface of carrier 4 to make it negatively charged. After impregnation for 10 hours, the upper liquid was filtered out, and then a high-voltage electric field drying device was used to dry the residue at an intensity of 12 kV / cm for 8 hours to obtain Ru / FeCrAl catalyst 4 (hereinafter referred to as "catalyst 4") for synthetic ammonia reaction.
[0092] 3) Application of catalyst 4 in ammonia synthesis reaction:
[0093] The ammonia synthesis catalytic performance of catalyst 4 was tested under the reaction conditions of Example 1. In the initial stage of the reaction, the ammonia synthesis rate of catalyst 4 was 30.4 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 4 was 29.3 mmol gcat -1 h -1 , with better catalytic activity and catalytic activity stability.
[0094] Comparative Example 1: No aging treatment of the alloy
[0095] This comparative example was carried out with reference to Example 1, except that: when preparing the carrier, the nano metal powder was not subjected to aging treatment; the same points as Example 1 are not repeated. The catalyst finally obtained is recorded as "Catalyst 5".
[0096] Referring to step 3 of Example 1, the catalyst 5 obtained in Comparative Example 1 was tested for its catalytic performance in ammonia synthesis.
[0097] Experimental results: At the initial stage of the reaction, the ammonia synthesis rate of catalyst 5 was 30.7 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 5 was 13.2 mmol gcat -1 h -1 Although the catalyst obtained in this comparative example has good initial catalytic activity, its stability is poor.
[0098] Comparative Example 2: The alloy is not connected to an external power source during dipping
[0099] Comparative Example 2 was carried out with reference to Example 1, except that when the carrier was added to the impregnation solution for impregnation, the carrier was not connected to an external power source; the same points as Example 1 are not repeated. The obtained catalyst is recorded as "Catalyst 6".
[0100] Referring to step 3 of Example 1, the catalyst 6 obtained in Comparative Example 2 was tested for its catalytic performance in ammonia synthesis.
[0101] Experimental results: At the initial stage of the reaction, the ammonia synthesis rate of catalyst 6 was 28.2 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 6 was 26.6 mmol gcat -1 h -1 The catalytic activity and stability of the catalyst obtained in this comparative example are significantly lower than those in Example 1.
[0102] Comparative Example 3: Alloy not treated with nitric acid
[0103] Comparative Example 3 was carried out with reference to Example 1, except that when preparing the carrier, the obtained nanometal powder was not washed with nitric acid, but only washed with deionized water until neutral. The same points as Example 1 are not repeated here. The obtained catalyst is recorded as "Catalyst 7".
[0104] Referring to step 3 of Example 1, the catalyst 7 obtained in Comparative Example 3 was tested for its catalytic performance in ammonia synthesis.
[0105] Experimental results:
[0106] In the initial stage of the reaction, the ammonia synthesis rate of catalyst 7 was 28.1 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis performance of catalyst 7 was 26.4 mmol gcat -1 h -1 The catalytic activity and stability of the catalyst obtained in this comparative example are significantly lower than those in Example 1.
[0107] Comparative Example 4: No high voltage electric field drying was used during the preparation of the catalyst
[0108] Comparative Example 4 was carried out with reference to Example 1, except that when preparing the catalyst, the method of drying the residue using a high-voltage electric field drying device was replaced by vacuum drying at 120° C. for 10 h. The same points as Example 1 are not repeated here. The obtained catalyst is recorded as “Catalyst 8”.
[0109] Referring to step 3 of Example 1, the catalyst 8 obtained in Comparative Example 4 was tested for its catalytic performance in ammonia synthesis.
[0110] Experimental results:
[0111] At the beginning of the reaction, the ammonia synthesis rate of catalyst 8 was 27.4 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 8 was 25.8 mmol gcat -1 h -1 The catalytic activity and stability of the catalyst obtained in this comparative example are significantly lower than those in Example 1.
[0112] Comparative Example 5: Preparation of carrier Fe 3+ Cr 2+ 、Al 3+ The molar ratio is 1:1:1
[0113] This comparative example was carried out with reference to Example 1, except that:
[0114] When preparing the carrier, the mixed solution I was prepared as follows: 162.2 g FeCl 3 、122.9gCrCl 2 and 133.3 g AlCl 3 Mix well, then add 6L of 1M Na 2 CO 3 aqueous solution to obtain a mixed solution I.
[0115] The mixed solution II was prepared as follows: 6 L of 2M acetic acid aqueous solution and NaOH aqueous solution were taken and mixed to obtain a mixed solution II.
[0116] The remaining operations are the same as those in Example 1 and will not be described again; the catalyst obtained in this comparative example is recorded as "catalyst 9".
[0117] Referring to step 3 of Example 1, the catalyst 9 obtained in Comparative Example 4 was tested for its catalytic performance in ammonia synthesis.
[0118] Experimental results: At the initial stage of the reaction, the ammonia synthesis rate of catalyst 9 was 8.2 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 9 was 3.5 mmol gcat -1 h -1 .
[0119] Comparative Example 6: Direct reaction with FeCrAl alloy
[0120] 0.2 g of the FeCrAl carrier 1 prepared in Example 1 was weighed and quenched in a continuous flow micro fixed bed reactor at a reaction pressure of 1 MPa, a temperature of 400°C, and a mass space velocity of 60000 mL·g -1 ·h -1 The ammonia synthesis performance was measured, and the amount of substance introduced was n(N 2 ):n(H 2 )=1:3N 2 and H 2 At the beginning of the reaction, the ammonia synthesis rate of FeCrAl support 1 was 3.2 mmol gcat - 1 h -1 After 400 hours of reaction, the ammonia synthesis rate of carrier 1 was 1.1 mmol gcat -1 h -1 .
[0121] Comparative Example 7 (When preparing the carrier, Fe 3+ Cr 2+ 、Al 3+ The molar ratio is 1:0.1:0.1)
[0122] This comparative example was carried out with reference to Example 1, except that:
[0123] When preparing the carrier, the mixed solution I was prepared as follows: 162.2 g FeCl 3 、12.29gCrCl 2 and 13.33 g AlCl 3 Mix well, then add 6L of 1M Na 2 CO 3 aqueous solution to obtain a mixed solution I.
[0124] The mixed solution II was prepared as follows: 6 L of 2M acetic acid aqueous solution and NaOH aqueous solution were taken and mixed to obtain a mixed solution II.
[0125] The remaining operations are the same as those in Example 1 and will not be repeated herein; the catalyst obtained in this comparative example is recorded as “catalyst 10”.
[0126] Referring to step 3 of Example 1, the catalyst 10 obtained in Comparative Example 7 was tested for its catalytic performance in ammonia synthesis.
[0127] Experimental results: At the initial stage of the reaction, the ammonia synthesis rate of catalyst 10 was 7.9 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 10 was 3.2 mmol gcat -1h -1 .
[0128] It is easy to understand that the above embodiments are only examples for clear explanation and do not mean that the present invention is limited thereto. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the protection scope of the present invention.
Claims
1. A method for preparing a ruthenium-based catalyst carrier, characterized in that: The preparation method comprises the following steps: 1) Mixing the mixed solution I and the mixed solution II and stirring them, heating them to 200-300° C. for reaction, preferably for 2-4 hours, to obtain nano metal powders, then washing the nano metal powders with nitric acid solution and deionized water until the washing solution is neutral, and then drying; Wherein, the mixed solution I is Fe 3+ Cr 2+ 、Al 3+ A mixed solution formed by a precursor salt in a Na2CO3 solution; The mixed solution II is a mixed solution of acetic acid solution and NaOH solution; 2) subjecting the nano metal powder obtained in step 1) to aging treatment, and obtaining the ruthenium-based catalyst carrier after cooling.
2. The preparation method according to claim 1, characterized in that: In step 1), the Fe 3+ Cr 2+ 、Al 3+ The molar ratio is 1:(0.126-0.306):(0.138-0.588); And / or, in step 1), the concentration of the Na2CO3 solution is 1-2M; And / or, in step 1), when preparing the mixed solution I, the precursor salt is added to the Na2CO3 solution under stirring, and the stirring speed is 300-500 r / min; And / or, in the mixed solution II of step 1), the concentrations of the acetic acid solution and the NaOH solution are 1-2 M respectively; preferably, in the mixed solution II, the acetic acid and the NaOH have the same molar amount.
3. The preparation method according to claim 2, characterized in that: In step 1), the total molar amount of acetate ions in the mixed solution II is equal to the molar amount of Fe 3+ 2-6 times the total molar amount.
4. The preparation method according to any one of claims 1 to 3, characterized in that: In step 1), the mixed solution I and the mixed solution II are mixed and stirred at a speed of 80-100 r / min; And / or, in step 1), the drying is carried out under vacuum, preferably at a temperature of 100 to 120° C. and for 8 to 12 hours.
5. The preparation method according to any one of claims 1 to 3, characterized in that: In step 1), the pH of the nitric acid solution is 2-4.
6. The preparation method according to any one of claims 1 to 3, characterized in that: In step 2), the aging treatment conditions include: a temperature of 100 to 150° C., a time of 6 to 12 hours, and the treatment is carried out under a protective gas. Preferably, the protective gas is nitrogen or argon.
7. A method for preparing a ruthenium-based catalyst, characterized in that: The steps include: S1. Immersing a ruthenium-based catalyst carrier in an impregnation solution containing ruthenium ions, and connecting an external power source to make the surface of the ruthenium-based catalyst carrier negatively charged, and removing the upper layer of liquid after impregnation to retain the residue; the ruthenium-based catalyst carrier is prepared by the preparation method according to any one of claims 1 to 6; S2. Drying the residue from step 1) using a high-voltage electric field drying technique to obtain the ruthenium-based catalyst.
8. The preparation method according to claim 7, characterized in that: In step S1, the ruthenium ions in the impregnation solution come from a ruthenium precursor salt, and the ruthenium precursor salt is preferably selected from one or more of ruthenium acetylacetonate, ruthenium nitrosyl nitrate, ruthenium trichloride, and ruthenium acetate; And / or, in step S1, the amount of the ruthenium ions is 2-4 wt% based on the mass of the carrier; And / or, in step S1, the voltage of the external power supply is 10 to 20 V, and the immersion time is 8 to 12 hours; And / or, in step S2, when the high-voltage electric field drying technology is used for drying, the electric field strength is 10-20 kV / cm.
9. A ruthenium-based catalyst prepared by the preparation method according to claim 7 or 8.
10. Use of the ruthenium-based catalyst according to claim 9 in a synthetic ammonia reaction, preferably, the ruthenium-based catalyst is used as a catalyst in a catalytic reaction of synthesizing ammonia from nitrogen and hydrogen.