Multi-component alloy nano-catalyst with Yolk-Shell structure as well as preparation method and application of multi-component alloy nano-catalyst

By adopting a multi-alloy nanocatalyst with Yolk-Shell structure, the existing catalysts have poor stability and low selectivity in the catalytic hydrogenation reaction of halogenated nitrobenzene, and efficient catalytic hydrogenation and long-term stability are achieved.

CN119057057APending Publication Date: 2024-12-03NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411283746.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing catalysts have problems of poor stability, low selectivity and high cost in the catalytic hydrogenation of halogenated nitrobenzene, especially precious metal catalysts are prone to deactivate and have high cost.

Method used

Using a multi-alloy nanocatalyst with a Yolk-Shell structure, including platinum-palladium-based ternary alloy nanoparticles and porous carbon shells, a hollow core-shell structure is formed through a specific preparation method to improve catalytic activity and stability.

Benefits of technology

The catalytic hydrogenation activity and stability are improved, the selectivity of halogenated nitrobenzene is enhanced, and good catalytic performance and long-term stability are shown in the hydrogenation reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057057A_ABST
    Figure CN119057057A_ABST
Patent Text Reader

Abstract

The invention discloses a multi-component alloy nano-catalyst with a Yolk-Shell structure as well as a preparation method and application of the multi-component alloy nano-catalyst. The multi-element alloy nano-catalyst is of a hollow core-shell structure and comprises ternary alloy nano-particles serving as an active component and a porous carbon shell coating the active component, a cavity is formed between the active component and the porous carbon shell, and the ternary alloy nano-particles comprise platinum-palladium-based ternary alloy. Three metals in the multi-component alloy nano-catalyst can generate a synergistic effect and an electronic modulation effect, a large amount of activated hydrogen can be quickly generated, and the catalytic hydrogenation activity is improved; the special hollow structure of the porous carbon shell provides a large specific surface area, mesopores in the surface of the porous carbon shell prevent loss of active components and guarantee diffusion and enrichment of small molecular reaction substrates, the active components in the cavity are effectively protected, and the service life of the porous carbon shell is prolonged. The catalyst has good hydrogenation activity and catalytic stability in the reaction of preparing halogenated aniline through selective hydrogenation of halogenated nitrobenzene.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalyst preparation technology and thermal catalytic application, and more specifically, to a multi-element alloy nanocatalyst with a Yolk-Shell structure and a preparation method thereof, as well as an application in the reaction of preparing halogenated aniline by catalytic hydrogenation of halogenated nitrobenzene. Background Art

[0002] Halogenated aniline is a valuable fine chemical product and organic intermediate, which is widely used in the synthesis of fine chemicals such as medicine, dyes, pesticides, etc. Halogenated aniline is usually prepared by reduction of halogenated nitrobenzene. Common synthesis methods mainly include chemical reduction, electrochemical reduction and catalyst hydrogenation reduction. Among them, the catalytic reduction method has the advantages of mild reaction conditions, easy separation of products, and recyclable catalysts. It is widely used in the reaction of catalytic hydrogenation of halogenated nitrobenzene to halogenated aniline. When the functional group -NO2 of halogenated nitrobenzene is reduced to -NH2, the C-Cl bond will break to produce dechlorination by-products, which will produce substances that pollute the environment and reduce the selectivity of halogenated aniline, which will be limited in practical applications. Therefore, it is particularly important to explore an environmentally friendly, highly stable and highly selective catalyst.

[0003] The catalysts used in catalytic hydrogenation reactions are mostly precious metal catalysts. Many researchers have improved the selectivity of halogenated anilines by designing catalysts loaded with precious metals and non-precious metals. For example, platinum, gold, palladium, and nickel have shown good catalytic performance in the catalytic hydrogenation process. However, precious metal catalysts have problems such as easy deactivation, poor stability, and high cost. Summary of the invention

[0004] The main purpose of the present invention is to provide a multi-element alloy nanocatalyst with Yolk-Shell structure and a preparation method thereof, so as to overcome the deficiencies in the prior art.

[0005] Another object of the present invention is to provide the application of the multi-element alloy nanocatalyst with Yolk-Shell structure.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes: An embodiment of the present invention provides a multi-alloy nanocatalyst with a Yolk-Shell structure, which has a hollow core-shell structure. The multi-alloy nanocatalyst includes ternary alloy nanoparticles as an active component, and a porous carbon shell coating the active component, and there is a cavity between the active component and the porous carbon shell. The ternary alloy nanoparticles include a platinum-palladium-based ternary alloy.

[0007] In some embodiments, the ternary alloy nanoparticles include PtPdM, wherein M includes at least any one of Fe, Mn, Co, and Ni. The synergistic effect of the three metals (PtPdM (M = Fe, Mn, Co, Ni, etc.)) can quickly generate a large amount of activated hydrogen, thereby improving the catalytic activity.

[0008] The embodiment of the present invention also provides a method for preparing a multi-element alloy nanocatalyst having a Yolk-Shell structure, which comprises: The metal ions in the mixed system of metal ion salt, cyclohexane and surfactant are completely precipitated to form a stable microemulsion, and then tetraethyl silicate is added for hydrolysis to obtain a SiO2 nano-microsphere hard template encapsulating a metal hydroxide complex, wherein the metal ion salt comprises a mixture of platinum salt, palladium salt and M metal salt; Forming phenolic resin on the surface of the SiO2 nano-microsphere hard template wrapping the metal hydroxide complex by aldol condensation to obtain a metal hydroxide complex / SiO2 / phenolic resin composite nanomaterial; The metal hydroxide complex / SiO2 / phenolic resin composite nanomaterial is subjected to high temperature treatment, and SiO2 is removed by etching to obtain a multi-element alloy nanocatalyst with a Yolk-Shell structure.

[0009] The embodiment of the present invention also provides a multi-element alloy nanocatalyst having a Yolk-Shell structure prepared by the above-mentioned preparation method.

[0010] The embodiment of the present invention also provides the use of the multi-element alloy nanocatalyst with Yolk-Shell structure in the reaction of preparing halogenated aniline by catalytic hydrogenation of halogenated nitrobenzene.

[0011] Compared with the prior art, the beneficial effects of the present invention include at least: The three metals PtPdM (M=Fe, Mn, Co, Ni, etc.) in the multi-element alloy nanocatalyst with Yolk-Shell structure provided by the present invention can produce synergistic effects and electronic modulation effects, can quickly produce a large amount of activated hydrogen, and thus improve the catalytic hydrogenation activity; the special hollow structure of the porous carbon shell provides a large specific surface area, and the micropores on its surface prevent the loss of active components while ensuring the diffusion and enrichment of small molecular reaction substrates, effectively protecting the active component ternary alloy nanoparticles inside the cavity, inhibiting the agglomeration of nanoparticles, so that the catalyst has very excellent catalytic stability, and has good hydrogenation activity and catalytic stability in the reaction of selective hydrogenation of halogenated nitrobenzene to prepare halogenated aniline. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the catalyst structure and reaction effect of the present invention, the present invention provides drawings to illustrate the catalysts and catalytic results involved in the embodiments. The following drawings are only for the catalyst materials involved in the embodiments. Researchers in this field can obtain other effective catalytic data based on these drawings without creative work.

[0013] Figure 1 This is a transmission electron microscope image of the multi-element alloy nanocatalyst PtPdFe@HCS having a Yolk-Shell structure prepared in Example 2 of the present invention; Figure 2 This is the XRD pattern of the multi-alloy nanocatalyst PtPdFe@HCS with Yolk-Shell structure prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0014] Compared with single metal or bimetallic structures, constructing multi-metal active centers is a promising method to improve hydrogenation selectivity. By changing the composition of the components to optimize the geometric site and electronic structure of the metal, the occurrence of side reactions such as carbon-halogen bond breakage can be effectively prevented, thereby improving hydrogenation selectivity. It often has better controllable capabilities for multiple active components and is the key to technology promotion.

[0015] Yolk-Shell nanostructure is a new type of nanomaterial discovered in recent years. It has an obvious shell-cavity-core three-dimensional structure. The cavity between the alloy core and the porous carbon shell allows the core to move freely in the shell, exposing more active sites and concentrating reactant molecules, thereby improving catalytic activity.

[0016] Therefore, in view of the deficiencies in the prior art, the inventors of this case have proposed the technical solution of the present invention after long-term research and extensive practice, which mainly provides a hollow nanostructure catalyst with a Yolk-Shell structure and a mesoporous carbon shell coated with a platinum-palladium-based ternary alloy (PtPdM (M=Fe, Mn, Co, Ni, etc.)) and a preparation method thereof. The technical solution, its implementation process and principle, etc. will be further explained as follows.

[0017] As one aspect of the technical solution of the present invention, a multi-element alloy nanocatalyst with a Yolk-Shell structure has a rattle-shaped hollow core-shell structure. The multi-element alloy nanocatalyst includes ternary alloy nanoparticles (PtPdM (M=Fe, Mn, Co, Ni, etc.)) as active components, and a porous carbon shell (@HCS) covering the active components, and there is a cavity between the active components and the porous carbon shell.

[0018] In some embodiments, the particle size of the ternary alloy nanoparticles is 6-7 nm.

[0019] In some embodiments, the porous carbon shell has a mesoporous structure.

[0020] Furthermore, the thickness of the porous carbon shell is 3-10 nm.

[0021] In some embodiments, the size of the multi-element alloy nanocatalyst having a Yolk-Shell structure is 40-50 nm.

[0022] In some more preferred embodiments, the multi-element alloy catalyst is a rattle-shaped hollow core-shell structure, which is a thin-walled HCS with a size of about 40-50 nm and a metal NP of about 6-7 nm encapsulated in the cavity, and the thickness of the HCS shell is about 3-10 nm. The special hollow structure of HCS provides a large specific surface area, and the mesopores on its surface prevent the loss of active components while ensuring the diffusion and enrichment of small molecule reaction substrates.

[0023] In some embodiments, the bulk content of platinum in the multi-element alloy nanocatalyst having a Yolk-Shell structure is 1.5 wt% to 2.6 wt%.

[0024] In some embodiments, the bulk content of palladium in the multi-element alloy nanocatalyst having a Yolk-Shell structure is 0.7 wt% to 1.4 wt%.

[0025] In some embodiments, the bulk content of M metal in the multi-element alloy nanocatalyst having a Yolk-Shell structure is 0.1 wt% to 0.7 wt%.

[0026] The ternary alloy nanoparticles in the multi-element alloy nanocatalyst of the present invention are hydrogenation active centers. The introduction of metal (M) into the PtPd alloy to form ternary alloy NPs (PtPdM (M=Fe, Mn, Co, Ni, etc.)) can produce synergistic effects and electronic modulation effects to improve the catalytic hydrogenation activity; the mesoporous carbon (HCS) is a protective shell, which effectively protects the active component ternary alloy nanoparticles (PtPdM (M=Fe, Mn, Co, Ni, etc.)) inside the cavity, inhibits the agglomeration of the nanoparticles, and makes it have very excellent catalytic stability.

[0027] As another aspect of the technical solution of the present invention, a method for preparing a multi-element alloy nanocatalyst having a Yolk-Shell structure involves: The metal ions in a mixed system comprising a metal ion salt, cyclohexane (as an oil phase) and a surfactant are completely precipitated to form a stable microemulsion, and then tetraethyl silicate (TEOS) is added for hydrolysis to obtain a SiO2 nano-microsphere hard template encapsulating a metal hydroxide complex, wherein the metal ion salt comprises a mixture of a platinum salt, a palladium salt and an M metal salt; Forming phenolic resin on the surface of the SiO2 nano-microsphere hard template wrapping the metal hydroxide complex by aldol condensation to obtain a metal hydroxide complex / SiO2 / phenolic resin composite nanomaterial; The metal hydroxide complex / SiO2 / phenolic resin composite nanomaterial is subjected to high temperature treatment, and SiO2 is removed by etching to obtain a multi-element alloy nanocatalyst with a Yolk-Shell structure.

[0028] The preparation mechanism of the present invention is: firstly, a reverse microemulsion system is used to precipitate metal ions in an aqueous phase and hydrolyze TEOS to obtain a CH@SiO2 nano-microsphere hard template encapsulating a metal hydroxide complex (CH), and then a phenolic resin (RF) is coated on its surface through aldol condensation, and then the organic film is pyrolyzed into carbon and the metal precursor is reduced at high temperature simultaneously, and finally SiO2 is removed by alkaline etching to obtain the final rattle-shaped hollow core-shell multi-element alloy nanocatalyst (also called nanoreactor PtPdM@HCS).

[0029] The present invention encapsulates the ternary metal alloy in a hollow structure and uses a recyclable carbon shell as a spherical shell. The ternary metal alloy structure has a unique geometric structure and electronic structure, and the excellent alloy effect can improve the catalytic activity, while the hollow structure and its mesoporous carbon shell can provide good stability.

[0030] In some embodiments, the molar ratio of the platinum salt, palladium salt and M metal salt is 1:1:0.25 to 1:1:1.

[0031] In some embodiments, the preparation method specifically includes: stirring and dissolving cyclohexane and a surfactant at 50-70°C until clear and transparent, then adding a metal ion salt to completely precipitate the metal ions to form a stable microemulsion, and then adding tetraethyl silicate for hydrolysis for several hours to obtain a SiO2 nanosphere hard template wrapped with a metal hydroxide complex.

[0032] Furthermore, the surfactant may be Brij C10, Brij C20, etc., but is not limited thereto.

[0033] In some embodiments, the preparation method specifically includes: evenly mixing an ethanol solution containing a SiO2 nanosphere hard template wrapped with a metal hydroxide complex, resorcinol, hexadecyltrimethylammonium bromide and concentrated ammonia water, and maintaining the mixture at 25-40°C for 0.5-2 h for aldol condensation reaction, then adding formaldehyde aqueous solution and stirring for 4-8 h, aging after the reaction, and obtaining a metal hydroxide complex / SiO2 / phenolic resin composite nanomaterial.

[0034] In some more preferred embodiments, the concentration of the SiO2 nanosphere hard template encapsulating the metal hydroxide complex in the ethanol solution containing the SiO2 nanosphere hard template encapsulating the metal hydroxide complex is 5 to 20 mg / mL, preferably 8 to 18 mg / mL. The SiO2 nanospheres formed in this step can well protect the internal metal precursor during the synthesis process, so there is almost no loss of metal elements during the synthesis.

[0035] Furthermore, the mass volume ratio of the resorcinol, hexadecyltrimethylammonium bromide, concentrated ammonia water and formaldehyde aqueous solution is 0.1-0.3 g: 2.5-4.0 g: 0.04-0.06 mL: 0.18-0.38 mL, wherein the formaldehyde aqueous solution is a commercially available product.

[0036] In some embodiments, the preparation method specifically includes: placing the metal hydroxide complex / SiO2 / phenolic resin composite nanomaterial in a tube furnace, heating the temperature from room temperature to 120-220°C at a heating rate of 3-10°C / min and maintaining for 0.5-2 h, and then heating the temperature to 600-900°C for 3-6 h to achieve the formation of alloy nanoparticles and the pyrolysis of phenolic resin into carbon. Among them, when the SiO2 nanosphere hard template wrapped with the metal hydroxide complex synthesized in the synthesis process is reduced at high temperature, the SiO2 shell can effectively prevent the aggregation of alloy nanoparticles (NPs) and control the size of NPs. Metal hydroxides are co-reduced internally to form alloy NPs.

[0037] In some embodiments, the preparation method specifically includes: after the high temperature treatment is completed, etching with alkaline solution to remove SiO2 to form a multi-element alloy nanocatalyst with a cavity.

[0038] Furthermore, the concentration of the alkali solution is 2-4 mol / L.

[0039] Among them, in some more specific implementation schemes, the specific steps of a method for preparing a multi-element alloy nanocatalyst having a Yolk-Shell structure are as follows: (1) Synthesis of CH@SiO2 nanospheres: First, cyclohexane and surfactant were stirred and dissolved in a water bath at 50-70°C, and metal ion salt solution was added to completely precipitate the metal ions to form a stable microemulsion. Then tetraethyl silicate (TEOS) was added and hydrolyzed for several hours. Finally, the CH@SiO2 silicon sphere hard template was obtained by centrifugation and washing. The obtained CH@SiO2 was dispersed in 10-20 mL of anhydrous ethanol for the next step of synthesis (concentration of about 8-18 mg / mL).

[0040] (2) Synthesis of CH@SiO2@RF composite nanomaterials: Resorcinol, CTAB and concentrated ammonia were added to CH@SiO2 ethanol solution and maintained in a water bath at 25-40 °C for 0.5-2 h for aldol condensation reaction. Then, formaldehyde aqueous solution was added and stirred for 4-8 h. After the reaction, the temperature was cooled to room temperature and aged overnight. The product was washed by centrifugation and dried in the shade to obtain CH@SiO2@RF composite nanomaterials with corresponding metal components.

[0041] (3) Synthesis of Yolk-Shell structure (PtPdM (M = Fe, Mn, Co, Ni, etc.))@HCS multi-element alloy nanocatalyst: The solid powder of CH@SiO2@RF composite nanomaterial is placed in a tubular furnace, and the organic film is pyrolyzed into carbon and the metal precursor is reduced simultaneously at high temperature. After cooling, it is etched with 2~4 mol / L NaOH solution. After one day, fresh alkali solution is replaced and etching is continued for another day. Finally, the product is collected by centrifugal washing and dried in the shade to obtain the (PtPdM (M = Fe, Mn, Co, Ni, etc.))@HCS multi-element alloy nanocatalyst.

[0042] Furthermore, in step (2), 0.1-0.3 g of resorcinol, 2.5-4.0 g of CTAB, 0.04-0.06 mL of concentrated aqueous ammonia and 0.18-0.38 mL of aqueous formaldehyde solution are added.

[0043] Furthermore, in step (3), the high temperature treatment, i.e., the calcination procedure is as follows: 8% hydrogen-argon mixed gas is introduced for purging (to remove air in the tube), the temperature is first raised from room temperature to 120-220°C at a heating rate of 3-10°C / min and maintained for 0.5-2 h to remove moisture and organic solvents, and then the temperature is raised to 600-900°C and maintained for 3-6 h. In this process, the formation of alloy nanoparticles and RF pyrolysis to carbon are completed.

[0044] Furthermore, in the present invention, the hollow structure is formed by hydrolyzing TEOS under alkaline conditions to generate silicon dioxide, and then etching with NaOH alkaline solution.

[0045] As another aspect of the technical solution of the present invention, it also relates to a multi-element alloy nanocatalyst with a Yolk-Shell structure prepared by the above-mentioned preparation method.

[0046] As another aspect of the technical solution of the present invention, it also relates to the application of the multi-element alloy nanocatalyst with Yolk-Shell structure.

[0047] Furthermore, the multi-element alloy nanocatalyst with Yolk-Shell structure of the present invention has obvious structural advantages and has good hydrogenation activity and catalytic stability in the reaction of selective hydrogenation of halogenated nitrobenzene to halogenated aniline.

[0048] Furthermore, the multi-element alloy nanocatalyst with Yolk-Shell structure of the present invention can be used to catalyze the selective hydrogenation of halogenated nitrobenzene to prepare halogenated aniline under normal pressure and temperature conditions, providing new ideas for the selective hydrogenation of halogenated aromatic compounds and other unsaturated aromatic small molecules.

[0049] Furthermore, catalytic tests were performed to evaluate the performance of the catalyst, and the reaction conditions were a normal pressure H2 atmosphere and a reaction temperature of 40°C.

[0050] Various embodiments of the present invention are now described in detail, however, these detailed embodiments are not intended to limit the present invention, but should be understood as a more detailed description of certain aspects of the catalyst covered by the present invention. The terms involved in the present invention are not intended to limit the present invention, and the numerical range in the present invention should be understood as each numerical value in the upper and lower limits of the range. Among them, the numerical range of the present invention should also be understood as any smaller range included therein. The terms involved are all meanings that can be understood by a person skilled in the art.

[0051] Other implementation methods obtained from the description of the present invention are simple and easy for technicians. This description and examples are only exemplary. The raw materials used in the examples of the present invention can be purchased through commercial channels, and the reagents and equipment used in the examples are all conventional reagents and equipment in the art.

[0052] In the catalyst test in the embodiment of the present invention, p-chloronitrobenzene is used as a model catalyst for halogenated nitrobenzene, which is a typical halogenated nitrobenzene. However, the application field of the catalyst can be targeted at the selective hydrogenation field of other halogenated nitrobenzenes. In the test, the reaction conditions used were set as follows: normal pressure H2 atmosphere; 40°C temperature; catalyst loading of 1 wt%; high speed to eliminate the diffusion effect.

[0053] Method for calculating the selectivity of preparing p-chloroaniline from p-chloronitrobenzene: Analyze the product by gas chromatography, and the p-chloroaniline content in the product is the selectivity.

[0054] Comparative Example 1 The preparation process of a PtPd@HCS catalyst involved in this comparative example comprises the following steps: (1) Synthesis of CH@SiO2 nanospheres: First, 80 ml of cyclohexane and 12 g of BrijC20 were stirred and dissolved in a warm water bath, and a mixture containing Pt 2+ and Pd 2+ 0.8 ml of 0.02 mmol aqueous solution was stirred for 0.5 h to allow the metal ions to completely precipitate and form a stable microemulsion; then 1.6 ml of concentrated ammonia was added and maintained for 1 h; then 2 ml of tetraethyl silicate (TEOS) was added and hydrolyzed for 3 h; finally, the CH@SiO2 silicon sphere hard template was obtained by centrifugation and washing. The obtained CH@SiO2 was dispersed in anhydrous ethanol for the next step of synthesis (about 10 mg / mL).

[0055] (2) Synthesis of CH@SiO2@RF composite nanomaterials: Take 12 ml of the prepared CH@SiO2 ethanol solution, add 28 ml of deionized water, then add 0.14 g of resorcinol, 2.0 g of CTAB and 0.04 ml of concentrated ammonia water, transfer to a 35 °C water bath and maintain for 0.5 h, then add 0.2 ml of formaldehyde aqueous solution and stir for 6 h. After the reaction, cool to room temperature and age overnight. The product is washed by centrifugation and dried in the shade to obtain CH@SiO2@RF composite nanomaterials with corresponding metal components.

[0056] (3) Synthesis of Yolk-Shell structured PtPd@HCS catalyst: CH@SiO2@RF solid powder was placed in a tubular furnace and purged with 8% hydrogen-argon mixed gas (to remove air in the tube). The temperature was raised from room temperature to 150 °C and maintained for 1 h to remove moisture and organic solvents. The temperature was then raised to 700 °C and maintained for 4 h. During this process, the formation of alloy nanoparticles and the thermal decomposition of RF into carbon were completed. After cooling, the black solid powder was etched with a 2.5 mol / L NaOH solution under stirring. After one day, the alkali solution was replaced and the etching treatment was continued for another day. Finally, the product was collected by centrifugation, washed with deionized water and acetone, and dried in the shade to obtain the PtPd@HCS catalyst.

[0057] Comparative Example 2 This embodiment involves a PtPdFe 1.25 The preparation process of @HCS multi-element alloy nanocatalyst includes the following steps: (1) Synthesis of CH@SiO2 nanospheres: First, 80 ml of cyclohexane and 13 g of BrijC20 were stirred and dissolved in a warm water bath, and a mixture containing Pt 2+ and Pd 2+ 0.02mmol each and Fe2+ 0.8 ml of 0.025 mmol aqueous solution was stirred for 0.5 h to completely precipitate the metal ions and form a stable microemulsion; then 1.6 ml of concentrated ammonia was added and maintained for 1 h; then 2 ml of tetraethyl silicate (TEOS) was added and hydrolyzed for 3 h; finally, the CH@SiO2 silicon sphere hard template was obtained by centrifugation and washing. The obtained CH@SiO2 was dispersed in anhydrous ethanol for the next step of synthesis (about 10 mg / mL).

[0058] (2) Synthesis of CH@SiO2@RF composite nanomaterials: Take 12 ml of the prepared CH@SiO2 ethanol solution, add 28 ml of deionized water, then add 0.14 g of resorcinol, 2.0 g of CTAB and 0.04 ml of concentrated ammonia water, transfer to a 35 °C water bath and maintain for 0.5 h, then add 0.2 ml of formaldehyde aqueous solution and stir for 6 h. After the reaction, cool to room temperature and age overnight. The product is washed by centrifugation and dried in the shade to obtain CH@SiO2@RF composite nanomaterials with corresponding metal components.

[0059] (3) Yolk-Shell structure PtPdFe 1.25 Synthesis of @HCS multi-element alloy nanocatalyst: CH@SiO2@RF solid powder was placed in a tubular furnace, purged with 8% hydrogen-argon mixed gas (to remove the air in the tube), and the temperature was raised from room temperature to 150 °C and maintained for 1 h to remove moisture and organic solvents, and then the temperature was raised to 700 °C and maintained for 4 h. In this process, the formation of alloy nanoparticles and the thermal decomposition of RF into carbon were completed; after cooling, the black solid powder was etched with 2.5 M NaOH solution under stirring, and fresh alkali solution was replaced after one day for another etching treatment; finally, the product was collected by centrifugation, washed with deionized water and acetone, and dried in the shade to obtain PtPdFe 1.25 @HCS multi-alloy nanocatalyst, in which the content of Pt is 2wt%, the content of Pd is 1.2wt%, and the content of Fe is 0.375wt%.

[0060] Example 1 This embodiment involves a PtPdFe 0.25 The preparation process of @HCS multi-element alloy nanocatalyst includes the following steps: (1) Synthesis of CH@SiO2 nanospheres: First, 80 ml of cyclohexane and 13 g of BrijC20 were stirred and dissolved in a 50 °C warm water bath, and a mixture containing Pt 2+ and Pd 2+ 0.02mmol each and Fe 2+0.8 ml of 0.005 mmol aqueous solution was stirred for 0.5 h to completely precipitate the metal ions and form a stable microemulsion; then 1.6 ml of concentrated ammonia was added and maintained for 1 h; then 2 ml of tetraethyl silicate (TEOS) was added and hydrolyzed for 3 h; finally, the CH@SiO2 silicon sphere hard template was obtained by centrifugation and washing. The obtained CH@SiO2 was dispersed in anhydrous ethanol for the next step of synthesis (about 10 mg / mL).

[0061] (2) Synthesis of CH@SiO2@RF composite nanomaterials: Take 12 ml of the prepared CH@SiO2 ethanol solution, add 28 ml of deionized water, then add 0.14 g of resorcinol, 2.0 g of CTAB and 0.04 ml of concentrated ammonia water, transfer to a 35 °C water bath and maintain for 0.5 h, then add 0.2 ml of formaldehyde aqueous solution and stir for 6 h. After the reaction, cool to room temperature and age overnight. The product is washed by centrifugation and dried in the shade to obtain CH@SiO2@RF composite nanomaterials with corresponding metal components.

[0062] (3) Yolk-Shell structure PtPdFe 0.25 Synthesis of @HCS multi-element alloy nanocatalyst: CH@SiO2@RF solid powder was placed in a tubular furnace, purged with 8% hydrogen-argon mixed gas (to remove the air in the tube), and heated from room temperature to 150 °C at a rate of 5 °C / min and maintained for 1 h to remove moisture and organic solvents, and then heated to 700 °C and maintained for 4 h. In this process, the formation of alloy nanoparticles and the thermal decomposition of RF into carbon were completed; after cooling, the black solid powder was etched with 2.5 mol / L NaOH solution under stirring, and fresh alkali solution was replaced after one day for another etching treatment; finally, the product was collected by centrifugation, washed with deionized water and acetone, and dried in the shade to obtain PtPdFe 0.25 @HCS multi-alloy nanocatalyst, in which the content of Pt is 2wt%, the content of Pd is 1.2wt%, and the content of Fe is 0.075wt%.

[0063] Example 2 This embodiment involves a PtPdFe 0.5 The preparation process of @HCS multi-element alloy nanocatalyst includes the following steps: (1) Synthesis of CH@SiO2 nanospheres: First, 80 ml of cyclohexane and 13 g of BrijC20 were stirred and dissolved in a 50 °C warm water bath, and a mixture containing Pt 2+ and Pd 2+ 0.02mmol each and Fe 2+0.8 ml of 0.01 mmol aqueous solution was stirred for 0.5 h to completely precipitate the metal ions and form a stable microemulsion; then 1.6 ml of concentrated ammonia was added and maintained for 1 h; then tetraethyl silicate (TEOS) was added and hydrolyzed for 3 h; finally, the CH@SiO2 silicon sphere hard template was obtained by centrifugation and washing. The obtained CH@SiO2 was dispersed in anhydrous ethanol for the next step of synthesis (about 10 mg / mL).

[0064] (2) Synthesis of CH@SiO2@RF composite nanomaterials: Take 12 ml of the prepared CH@SiO2 ethanol solution, add 28 ml of deionized water, then add 0.14 g of resorcinol, 2.0 g of CTAB and 0.04 ml of concentrated ammonia water, transfer to a 35 °C water bath and maintain for 0.5 h, then add 0.2 ml of formaldehyde aqueous solution and stir for 6 h. After the reaction, cool to room temperature and age overnight. The product is washed by centrifugation and dried in the shade to obtain CH@SiO2@RF composite nanomaterials with corresponding metal components.

[0065] (3) Yolk-Shell structure PtPdFe 0.5 Synthesis of @HCS multi-element alloy nanocatalyst: CH@SiO2@RF solid powder was placed in a tubular furnace, purged with 8% hydrogen-argon mixed gas (to remove the air in the tube), and heated from room temperature to 150 °C at a rate of 5 °C / min and maintained for 1 h to remove moisture and organic solvents, and then heated to 700 °C and maintained for 4 h. During this process, the formation of alloy nanoparticles and the thermal decomposition of RF into carbon were completed; after cooling, the black solid powder was etched with 2.5 M NaOH solution under stirring, and fresh alkali solution was replaced after one day for another etching treatment; finally, the product was collected by centrifugation, washed with deionized water and acetone, and dried in the shade to obtain PtPdFe 0.5 @HCS multi-alloy nanocatalyst, in which the content of Pt is 2wt%, the content of Pd is 1.2wt%, and the content of Fe is 0.15wt%.

[0066] After testing, the multi-element alloy nanocatalyst PtPdFe with Yolk-Shell structure obtained in this embodiment 0.5 @HCS transmission electron microscope image Figure 1 As shown, the XRD pattern is Figure 2 As shown. Among them, PtPdFe 0.5 The particle size of the ternary alloy NPs is 6~7 nm, and the thickness of the porous carbon shell HCS is 3~10 nm.

[0067] Example 3 The preparation process of a PtPdFe@HCS multi-element alloy nanocatalyst involved in this embodiment includes the following steps: (1) Synthesis of CH@SiO2 nanospheres: First, 80 ml of cyclohexane and 13 g of BrijC20 were stirred and dissolved in a 50 °C warm water bath, and a mixture containing Pt 2+ , Pd 2+ , Fe 2+ 0.8 ml of 0.02 mmol aqueous solution was stirred for 0.5 h to allow the metal ions to completely precipitate and form a stable microemulsion; then 1.6 ml of concentrated ammonia was added and maintained for 1 h; then 2 ml of tetraethyl silicate (TEOS) was added and hydrolyzed for 3 h; finally, the CH@SiO2 silicon sphere hard template was obtained by centrifugation and washing. The obtained CH@SiO2 was dispersed in anhydrous ethanol for the next step of synthesis (about 10 mg / mL).

[0068] (2) Synthesis of CH@SiO2@RF composite nanomaterials: Take 12 ml of the prepared CH@SiO2 ethanol solution, add 28 ml of deionized water, then add 0.14 g of resorcinol, 2.0 g of CTAB and 0.04 ml of concentrated ammonia water, transfer to a 35 °C water bath and maintain for 0.5 h, then add 0.2 ml of formaldehyde aqueous solution and stir for 6 h. After the reaction, cool to room temperature and age overnight. The product is washed by centrifugation and dried in the shade to obtain CH@SiO2@RF composite nanomaterials with corresponding metal components.

[0069] (3) Synthesis of Yolk-Shell structured PtPdFe@HCS multi-element alloy nanocatalyst: CH@SiO2@RF solid powder was placed in a tubular furnace and purged with 8% hydrogen-argon mixed gas (to remove air in the tube). The temperature was raised from room temperature to 150 °C at a rate of 5 °C / min and maintained for 1 h to remove moisture and organic solvents. The temperature was then raised to 700 °C and maintained for 4 h. During this process, the formation of alloy nanoparticles and the thermal decomposition of RF into carbon were completed. After cooling, the black solid powder was etched with a 2.5 M NaOH solution under stirring. After one day, the alkali solution was replaced and the etching treatment was continued for another day. Finally, the product was collected by centrifugation, washed with deionized water and acetone, and dried in the shade to obtain a PtPdFe@HCS multi-element alloy nanocatalyst with a Pt content of 2 wt%, a Pd content of 1.2 wt%, and a Fe content of 0.3 wt%.

[0070] Example 4 The preparation process of a PtPdCo@HCS multi-element alloy nanocatalyst involved in this embodiment includes the following steps: (1) Synthesis of CH@SiO2 nanospheres: First, 80 ml of cyclohexane and 13 g of BrijC20 were stirred and dissolved in a 50 °C warm water bath, and a mixture containing Pt 2+ , Pd 2+ 、Co 2+0.8 ml of 0.02 mmol aqueous solution was stirred for 0.5 h to allow the metal ions to completely precipitate and form a stable microemulsion; then 1.6 ml of concentrated ammonia was added and maintained for 1 h; then 2 ml of tetraethyl silicate (TEOS) was added and hydrolyzed for 3 h; finally, the CH@SiO2 silicon sphere hard template was obtained by centrifugation and washing. The obtained CH@SiO2 was dispersed in anhydrous ethanol for the next step of synthesis (about 10 mg / mL).

[0071] (2) Synthesis of CH@SiO2@RF composite nanomaterials: Take 12 ml of the prepared CH@SiO2 ethanol solution, add 28 ml of deionized water, then add 0.14 g of resorcinol, 2.0 g of CTAB and 0.04 ml of concentrated ammonia water in sequence, transfer to a 25 °C water bath and maintain for 2 h, then add 0.2 ml of formaldehyde aqueous solution and stir for 4 h. After the reaction, cool to room temperature and age overnight. The product is washed by centrifugation and dried in the shade to obtain CH@SiO2@RF composite nanomaterials with the corresponding metal components.

[0072] (3) Synthesis of Yolk-Shell structured PtPdCo@HCS multi-element alloy nanocatalyst: CH@SiO2@RF solid powder was placed in a tubular furnace and purged with 8% hydrogen-argon mixed gas (to remove air in the tube). The temperature was raised from room temperature to 150 °C at a rate of 6 °C / min and maintained for 1 h to remove moisture and organic solvents. The temperature was then raised to 700 °C and maintained for 4 h. During this process, the formation of alloy nanoparticles and the thermal decomposition of RF into carbon were completed. After cooling, the black solid powder was etched with a 2.5 M NaOH solution under stirring. After one day, the alkali solution was replaced and the etching treatment was continued for another day. Finally, the product was collected by centrifugation, washed with deionized water and acetone, and dried in the shade to obtain the PtPdCo@HCS multi-element alloy nanocatalyst.

[0073] Example 5 The preparation process of a PtPdMn@HCS multi-element alloy nanocatalyst involved in this embodiment includes the following steps: (1) Synthesis of CH@SiO2 nanospheres: First, 80 ml of cyclohexane and 13 g of BrijC20 were stirred and dissolved in a 60 °C warm water bath, and a mixture containing Pt 2+ , Pd 2+ , Mn 2+ 0.8 ml of 0.02 mmol aqueous solution was stirred for 0.5 h to allow the metal ions to completely precipitate and form a stable microemulsion; then 1.6 ml of concentrated ammonia was added and maintained for 1 h; then 2 ml of tetraethyl silicate (TEOS) was added and hydrolyzed for 3 h; finally, the CH@SiO2 silicon sphere hard template was obtained by centrifugation and washing. The obtained CH@SiO2 was dispersed in anhydrous ethanol for the next step of synthesis (about 10 mg / mL).

[0074] (2) Synthesis of CH@SiO2@RF composite nanomaterials: Take 12 ml of the prepared CH@SiO2 ethanol solution, add 28 ml of deionized water, then add 0.1 g of resorcinol, 2.5 g of CTAB and 0.04 ml of concentrated ammonia water, transfer to a 35 °C water bath and maintain for 1.5 h, then add 0.18 ml of formaldehyde aqueous solution and stir for 8 h. After the reaction, cool to room temperature and age overnight. The product is washed by centrifugation and dried in the shade to obtain CH@SiO2@RF composite nanomaterials with corresponding metal components.

[0075] (3) Synthesis of Yolk-Shell structured PtPdMn@HCS multi-element alloy nanocatalyst: CH@SiO2@RF solid powder was placed in a tubular furnace and purged with 8% hydrogen-argon mixed gas (to remove air in the tube). The temperature was raised from room temperature to 120 °C at a rate of 3 °C / min and maintained for 2 h to remove moisture and organic solvents. The temperature was then raised to 600 °C and maintained for 6 h. During this process, the formation of alloy nanoparticles and the thermal decomposition of RF into carbon were completed. After cooling, the black solid powder was etched with a 2.5 mol / L NaOH solution under stirring. After one day, the alkali solution was replaced and the etching treatment was continued for another day. Finally, the product was collected by centrifugation, washed with deionized water and acetone, and dried in the shade to obtain the PtPdMn@HCS multi-element alloy nanocatalyst.

[0076] Example 6 The preparation process of a PtPdNi@HCS multi-element alloy nanocatalyst involved in this embodiment includes the following steps: (1) Synthesis of CH@SiO2 nanospheres: First, 80 ml of cyclohexane and 13 g of BrijC20 were stirred and dissolved in a 70 °C warm water bath, and a mixture containing Pt 2+ , Pd 2+ 、Ni 2+ 0.8 ml of 0.02 mmol aqueous solution was stirred for 0.5 h to allow the metal ions to completely precipitate and form a stable microemulsion; then 1.6 ml of concentrated ammonia was added and maintained for 1 h; then 2 ml of tetraethyl silicate (TEOS) was added and hydrolyzed for 3 h; finally, the CH@SiO2 silicon sphere hard template was obtained by centrifugation and washing. The obtained CH@SiO2 was dispersed in anhydrous ethanol for the next step of synthesis (about 10 mg / mL).

[0077] (2) Synthesis of CH@SiO2@RF composite nanomaterials: Take 12 ml of the prepared CH@SiO2 ethanol solution, add 28 ml of deionized water, then add 0.3 g of resorcinol, 4.0 g of CTAB and 0.06 ml of concentrated ammonia water in sequence, transfer to a 40 °C water bath and maintain for 0.5 h, then add 0.38 ml of formaldehyde aqueous solution and stir for 7 h. After the reaction, cool to room temperature and age overnight. The product is washed by centrifugation and dried in the shade to obtain CH@SiO2@RF composite nanomaterials with corresponding metal components.

[0078] (3) Synthesis of Yolk-Shell structured PtPdNi@HCS multi-element alloy nanocatalyst: CH@SiO2@RF solid powder was placed in a tubular furnace and purged with 8% hydrogen-argon mixed gas (to remove air in the tube). The temperature was raised from room temperature to 220 °C at a rate of 10 °C / min and maintained for 0.5 h to remove moisture and organic solvents. The temperature was then raised to 900 °C and maintained for 3 h. During this process, the formation of alloy nanoparticles and the thermal decomposition of RF into carbon were completed. After cooling, the black solid powder was etched with 4 mol / L NaOH solution under stirring. After one day, the alkali solution was replaced and the etching treatment was continued for another day. Finally, the product was collected by centrifugation, washed with deionized water and acetone, and dried in the shade to obtain the PtPdNi@HCS multi-element alloy nanocatalyst.

[0079] Application Example 1 In this example, the PtPdFe@HCS multi-element alloy nanocatalyst prepared in Example 3 is used for catalytic hydrogenation of p-chloronitrobenzene, and the specific steps are as follows: 3 mmol of p-chloronitrobenzene, 0.05 g of internal standard and 10 mg of PtPdFe@HCS multi-element alloy nanocatalyst (1 wt%) were placed in a three-necked flask, 10 mL of anhydrous ethanol was added, and then H2 gas flow was introduced to remove the air in the system, and the reaction was carried out in a water bath at 40°C for 3 h. After the reaction was completed, the catalyst was removed by filtration through a filter membrane to obtain a clear solution, and the liquid sample was analyzed.

[0080] Application Example 2 In this example, the PtPdMn@HCS multi-element alloy nanocatalyst prepared in Example 5 is used for catalytic hydrogenation of p-chloronitrobenzene, and the specific steps are as follows: 3 mmol of p-chloronitrobenzene, 0.05 g of internal standard and 10 mg of PtPdMn@HCS multi-element alloy nanocatalyst (1 wt%) were placed in a three-necked flask, and 10 mL of anhydrous ethanol was added. Then, H2 gas flow was introduced to remove the air in the system, and the reaction was carried out in a water bath at 40°C for 3 h. After the reaction was completed, the catalyst was removed by filtration through a filter membrane to obtain a clear solution, and the liquid sample was analyzed.

[0081] Application Example 3 In this example, the PtPdCo@HCS multi-element alloy nanocatalyst prepared in Example 4 was used for catalytic hydrogenation of p-chloronitrobenzene, and the specific steps were as follows: 3 mmol of p-chloronitrobenzene, 0.05 g of internal standard and 10 mg of PtPdCo@HCS multi-element alloy nanocatalyst (1 wt%) were placed in a three-necked flask, 10 mL of anhydrous ethanol was added, and then H2 gas flow was introduced to remove the air in the system, and the reaction was carried out in a water bath at 40°C for 3 h. After the reaction was completed, the catalyst was removed by filtration through a filter membrane to obtain a clear solution, and the liquid sample was analyzed.

[0082] Application Example 4 In this example, the PtPdNi@HCS multi-element alloy nanocatalyst prepared in Example 6 is used for catalytic hydrogenation of p-chloronitrobenzene, and the specific steps are as follows: 3 mmol of p-chloronitrobenzene, 0.05 g of internal standard and 10 mg of PtPdNi@HCS multi-element alloy nanocatalyst (1wt%) were placed in a three-necked flask, 10 mL of anhydrous ethanol was added, and then H2 gas flow was introduced to remove the air in the system, and the reaction was carried out in a water bath at 40°C for 3 h. After the reaction was completed, the catalyst was removed by filtration through a filter membrane to obtain a clear solution, and the liquid sample was analyzed.

[0083] Table 1 shows the selectivity and activity of the catalysts involved in different embodiments of the present invention for catalytic hydrogenation of p-chloronitrobenzene to p-chloroaniline.

[0084] Table 1 Selectivity and activity of hydrogenation of p-chloronitrobenzene to p-chloroaniline over different catalysts ; It can be seen that Example 2 has the best effect, while Comparative Example 2 has the lowest conversion rate. The reason may be that too much Fe is added, covering a part of the active sites of PtPdFe.

[0085] Comparative Example 3 Compared with Example 2, the difference is that the temperature of the high temperature treatment is 1000°C.

[0086] The results show that calcination at too high a temperature will cause shell collapse and is not conducive to the synthesis of the catalyst.

[0087] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0088] It should be understood that the order of the various steps or the order in which a particular action is performed is not very important, as long as the teachings of the present invention remain operable. In addition, two or more steps or actions may be performed simultaneously.

[0089] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made and that elements of the described embodiments may be substituted with substantial equivalents without departing from the spirit and scope of the present invention. In addition, many modifications may be made to adapt a particular situation or material to the teachings of the present invention without departing from the scope of the present invention. Therefore, it is not intended herein to limit the present invention to the specific disclosed embodiments for carrying out the present invention, but rather it is intended that the present invention will include all embodiments within the scope of the appended claims.

Claims

1. A multi-element alloy nanocatalyst with Yolk-Shell structure, characterized in that: The multi-element alloy nanocatalyst has a hollow core-shell structure, including ternary alloy nanoparticles as active components and a porous carbon shell covering the active components, with a cavity between the active components and the porous carbon shell, and the ternary alloy nanoparticles include a platinum-palladium-based ternary alloy.

2. The multi-element alloy nanocatalyst according to claim 1, characterized in that: The ternary alloy nanoparticles include PtPdM, wherein M includes at least any one of Fe, Mn, Co, and Ni; And / or, the particle size of the ternary alloy nanoparticles is 6-7 nm.

3. The multi-element alloy nanocatalyst according to claim 1, characterized in that: The porous carbon shell has a mesoporous structure; and / or the thickness of the porous carbon shell is 3-10 nm; And / or, the size of the multi-element alloy nanocatalyst is 40-50 nm.

4. The multi-element alloy nanocatalyst according to claim 2, characterized in that: The bulk content of platinum in the multi-element alloy nanocatalyst is 1.5 wt%~2.6 wt%; and / or, the bulk content of palladium in the multi-element alloy nanocatalyst is 0.7 wt% to 1.4 wt%; and / or, the bulk content of M in the multi-element alloy nanocatalyst is 0.1 wt% to 0.7 wt%; And / or, the molar ratio of Pt, Pd and M in the ternary alloy nanoparticles is 1:1:0.25~1:1:

1.

5. A method for preparing a multi-element alloy nanocatalyst having a Yolk-Shell structure, characterized in that: include: The metal ions in the mixed system of metal ion salt, cyclohexane and surfactant are completely precipitated to form a stable microemulsion, and then tetraethyl silicate is added for hydrolysis to obtain a SiO2 nano-microsphere hard template encapsulating a metal hydroxide complex, wherein the metal ion salt comprises a mixture of platinum salt, palladium salt and M metal salt; Forming phenolic resin on the surface of the SiO2 nano-microsphere hard template wrapping the metal hydroxide complex by aldol condensation to obtain a metal hydroxide complex / SiO2 / phenolic resin composite nanomaterial; The metal hydroxide complex / SiO2 / phenolic resin composite nanomaterial is subjected to high temperature treatment, and SiO2 is removed by etching to obtain a multi-element alloy nanocatalyst with a Yolk-Shell structure.

6. The preparation method according to claim 5, characterized in that: include: Cyclohexane and surfactant are stirred and dissolved at 50-70°C, and then metal ion salt is added to completely precipitate the metal ions to form a stable microemulsion, and then tetraethyl silicate is added for hydrolysis to obtain a SiO2 nano-microsphere hard template wrapped with a metal hydroxide complex; Preferably, the molar ratio of the platinum salt, palladium salt and M metal salt is 1:1:0.25 to 1:1:1.

25.

7. The preparation method according to claim 5, characterized in that include: An ethanol solution containing a SiO2 nanosphere hard template wrapped with a metal hydroxide complex, resorcinol, hexadecyltrimethylammonium bromide and concentrated ammonia water are uniformly mixed, and the mixture is maintained at 25-40°C for 0.5-2 h for aldol condensation reaction, and then a formaldehyde aqueous solution is added and stirred for 4-8 h, and the mixture is aged after the reaction to obtain a metal hydroxide complex / SiO2 / phenolic resin composite nanomaterial; Preferably, the concentration of the SiO2 nano-microsphere hard template encapsulating the metal hydroxide complex in the ethanol solution containing the SiO2 nano-microsphere hard template encapsulating the metal hydroxide complex is 5 to 20 mg / mL, preferably 8 to 18 mg / mL; Preferably, the mass volume ratio of the resorcinol, hexadecyltrimethylammonium bromide, concentrated ammonia water and formaldehyde aqueous solution is 0.1-0.3 g: 2.5-4.0 g: 0.04-0.06 mL: 0.18-0.38 mL.

8. The preparation method according to claim 5, characterized in that include: The metal hydroxide composite / SiO2 / phenolic resin composite nanomaterial is placed in a tube furnace, and the temperature is first raised from room temperature to 120-220°C at a heating rate of 3-10°C / min and maintained for 0.5-2 h, and then the temperature is raised to 600-900°C for high temperature treatment for 3-6 h to achieve the formation of alloy nanoparticles and the thermal decomposition of the phenolic resin into carbon; And / or, the preparation method comprises: after the high temperature treatment is completed, etching with alkaline solution to remove SiO2 to form a multi-element alloy nanocatalyst with a cavity; Preferably, the concentration of the alkali solution is 2-4 mol / L.

9. A multi-element alloy nanocatalyst having a Yolk-Shell structure prepared by the preparation method according to any one of claims 5 to 8.

10. Use of the multi-element alloy nanocatalyst with Yolk-Shell structure according to any one of claims 1 to 4 and 9 in the reaction of preparing halogenated aniline by catalytic hydrogenation of halogenated nitrobenzene.

Citation Information

Cited By

  • Multi-element metal alloy nano-particle / biochar composite nano-catalyst rich in vacancy defects and preparation method of multi-element metal alloy nano-particle / biochar composite nano-catalyst

    CN119685860A

  • Normal-temperature oxygen and hydrogen removal bifunctional catalyst as well as preparation method and application thereof

    CN120502337A