Preparation method of cascade pore desulfurization catalyst

Through the combination of an alumina carrier with a ladder pore structure and multiple active metal components, the problems of difficult macromolecule diffusion and insufficient matching of active metals in the heavy oil hydrogenation reaction of existing catalysts are solved, and efficient hydrogenation and dehydration are achieved. Metal and desulfurization activity improve the long-term operation capability of the catalyst.

CN118767935AActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310356266.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-15
Estimated Expiration
2043-04-06

AI Technical Summary

Technical Problem

In the hydrogenation reaction of heavy oil, existing catalysts have problems such as difficulty in diffusion of macromolecules and insufficient matching between active metal components and pore channels, resulting in low catalytic activity.

Method used

Using an alumina carrier with a stepped pore structure, by preparing pseudo-boehmite with high crystallinity and flaky structure, and impregnating it with multiple active metal components, a macroporous-mesoporous structure is formed to improve the hydrogenation reaction of the catalyst active.

Benefits of technology

It achieves efficient hydrodemetallization and desulfurization activities in heavy oil hydrogenation reactions, and improves the long-term operation capability of the catalyst and the uniformity of active metal distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767935A_ABST
    Figure CN118767935A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a cascade pore desulfurization catalyst. The preparation method comprises the following steps: (1) preparing first pseudo-boehmite with the following properties: 1.0 lt; p1 < = 1.3, 1.1 lt; p1 is less than or equal to 1.5, P2 is less than or equal to 1.5, P1 is equal to D (120) / D (031), P2 is equal to D (120) / D (020), and D represents the grain size of a crystal face corresponding to a characteristic peak in a pseudo-boehmite grain XRD spectrogram; (2) impregnating the first pseudo-boehmite with the first active component impregnation liquid, and drying to obtain modified pseudo-boehmite; (3) mixing, kneading and forming the modified pseudo-boehmite and the second pseudo-boehmite, and drying and roasting the formed product to obtain a modified alumina carrier; and (4) impregnating the modified alumina carrier with the second active component impregnation liquid, drying, and roasting to obtain the cascade pore desulfurization catalyst. The catalyst provided by the invention has a macroporous-mesoporous cascade pore structure, the hydrogenation reaction activity at macropores is high, the high hydrogenation reaction activity site is well matched with the pore channel of the catalyst, and the catalyst has a wide application prospect in the field of heterogeneous catalysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalyst preparation, and in particular relates to a method for preparing a stepped pore desulfurization catalyst. Background Art

[0002] In recent years, with the heavy quality of crude oil resources, the growth of fuel oil consumption demand and increasingly stringent environmental regulations, the use of hydrogenation technology to convert residual oil into high-quality light fuel oil and chemical products is helpful to improve the depth of crude oil processing, reduce environmental pollution, increase the yield of light oil and improve product quality. Residual oil is enriched with most of the heteroatoms in crude oil, such as sulfur, nitrogen and metals (mainly Ni and V). The metals in residual oil are mainly present in macromolecular compounds such as colloids and asphaltene, which have complex structures, large molecular sizes and difficult diffusion. The pores of traditional alumina carriers are small, which is not conducive to the diffusion of macromolecular reactants in residual oil. Therefore, it is necessary to develop alumina carriers with larger pores.

[0003] CN201510191156.7 discloses a heavy oil hydrogenation catalyst and a preparation method thereof. The catalyst comprises an alumina carrier composed of flaky polycrystalline γ-alumina and a hydrogenation active metal. The preparation method of the catalyst is as follows: adding a binder and an extrusion aid to the flaky γ-polycrystalline alumina raw powder, kneading, molding, drying and calcining to obtain an alumina carrier, and loading the active metal on the obtained alumina carrier by a conventional method. The preparation method of the flaky γ-polycrystalline alumina comprises the following steps: (1) mixing an inorganic aluminum salt, a low-carbon alcohol and / or water, and a low-carbon alkylene oxide uniformly to form a gel, and then aging the gel; (2) soaking the gel obtained in step (1) with a low-carbon alcohol, and then drying and calcining; (3) immersing the material obtained in step (2) in ammonia water for closed hydrothermal treatment, solid-liquid separation, and drying to obtain a flaky γ-polycrystalline alumina raw powder. This invention adjusts the pore structure of the carrier by adding flaky polycrystalline γ-alumina into the alumina carrier. However, the preparation process of flaky polycrystalline γ-alumina is relatively complicated. On the other hand, the matching degree between the active metal components and the catalyst pores needs to be further improved.

[0004] CN201910265729.4 discloses a preparation method of a hydrodemetallization catalyst. The preparation method of the hydrodemetallization catalyst of the present invention includes: (1) preparing rod-shaped alumina clusters; (2) impregnating the rod-shaped alumina clusters in step (1) with an impregnating solution containing a hydrogenation active component I and drying to obtain modified rod-shaped alumina clusters, and kneading, drying, and calcining the modified rod-shaped alumina clusters with pseudo-boehmite to obtain support I; (3) mixing the support I obtained in step (2) with ammonium bicarbonate and water, sealing and heat-treating, and drying and calcining the treated material to obtain support II; (4) impregnating the support II in step (3) with an impregnating solution containing a hydrogenation active component II, and drying and calcining the support to obtain a hydrodemetallization catalyst. This method adjusts the pore structure and active metal distribution of the catalyst by using rod-shaped alumina clusters modified with active components, thereby improving the activity of the catalyst. However, the pores formed by the accumulation of rod-shaped particles in the rod-shaped alumina clusters are relatively large, which is not conducive to the full exertion of the hydrogenation activity of the catalyst. Summary of the Invention

[0005] Aiming at the deficiencies in the prior art, the present invention provides a preparation method of a stepped pore desulfurization catalyst. The catalyst of the present invention has a stepped pore structure of macropores-mesopores. The hydrogenation reaction activity at the macropores is high, and the high hydrogenation reaction active sites are well matched with the pores of the catalyst. This catalyst has high hydrodemetallization and desulfurization activities during the heavy oil hydrogenation reaction process.

[0006] The preparation method of the stepped pore desulfurization catalyst of the present invention includes the following: (1) Preparing a first pseudo-boehmite with the following properties: 1.0 < P1 ≤ 1.3, 1.1 < P2 ≤ 1.5, P1 = D(120) / D(031), P2 = D(120) / D(020), where D represents the grain size of the crystal plane corresponding to the characteristic peak in the XRD spectrum of the pseudo-boehmite crystal grains; (2) Impregnating the first pseudo-boehmite with a first active component impregnating solution, and drying the impregnated material to obtain modified pseudo-boehmite; (3) Kneading and molding the modified pseudo-boehmite with a second pseudo-boehmite, and drying and calcining the molded product to obtain a modified alumina support; (4) Impregnating the modified alumina support with a second active component impregnating solution, and drying and calcining the impregnated material to obtain a stepped pore desulfurization catalyst.

[0007] In the method of the present invention, in the first pseudo-boehmite prepared in step (1), D(120) represents the grain size of the crystal plane corresponding to the (120) peak in the XRD spectrum of the pseudo-boehmite grain, and D(120) is 75-105Å; D(031) represents the grain size of the crystal plane corresponding to the (031) peak in the XRD spectrum of the pseudo-boehmite grain, and D(031) is 70-90Å; D(020) represents the grain size of the crystal plane corresponding to the (020) peak in the XRD spectrum of the pseudo-boehmite grain, and D(031) is 70-90Å; Grain size, D (020) is 60-70Å; the 120 peak refers to the characteristic peak of 2θ of 25.5-29.9° in the XRD spectrum; the 031 peak refers to the characteristic peak of 2θ of 36.3-40.5° in the XRD spectrum; the 020 peak refers to the characteristic peak of 2θ of 12.0-16.2° in the XRD spectrum, D = Kλ / (Bcosθ), K is the Scherrer constant, λ is the diffraction wavelength of the target material, B is the half-peak width of the diffraction peak, and θ is the diffraction angle; In the method of the present invention, the preparation method of the first pseudo-boehmite is as follows: the calcined nitric acid is crushed and sieved to obtain a powdery material, the powdery material is immersed in a propylene oxide solution for sealed heat treatment, and the treated material is dried to obtain the first pseudo-boehmite; the first pseudo-boehmite is a flaky structure.

[0008] In the above-mentioned preparation method of the first pseudo-boehmite, the roasting temperature is 450-650°C, and the roasting time is 4-8 hours. The particle size of the powdered material is greater than 100 mesh, preferably greater than 200 mesh. The mass concentration of the propylene oxide solution is 2.5%-12%, preferably 4%-8%, and the mass ratio of the propylene oxide solution to the aluminum oxide is 3:1-10:1, preferably 4:1-8:1. The hydrothermal treatment is carried out in a closed container, and the closed container is preferably an autoclave. The hydrothermal treatment temperature is 110-180°C, preferably 120-160°C, and the treatment time is 4-8 hours. The pressure in the sealed container during the hydrothermal treatment is the autogenous pressure. The drying temperature is 100-160°C, and the drying time is 2-8 hours.

[0009] In the method of the present invention, the first active component impregnation solution described in step (2) is a W-Ni-P solution containing WO3 and NiO, the WO3 content in the solution is 1-5g / 100mL, the NiO content is 0.2-1g / 100mL, the amount of impregnation solution is such that the material is completely immersed, the impregnation time is 1-4 hours, the drying temperature is 100-160°C, and the drying time is 2-8 hours.

[0010] In the method of the present invention, the second pseudo-boehmite described in step (3) can be a pseudo-boehmite prepared by any method, such as acid precipitation method, alkali precipitation method, alcohol aluminum hydrolysis method, etc., preferably a pseudo-boehmite with a pore size of 10-20 nm, more preferably a pseudo-boehmite with a pore content of 10-20 nm accounting for more than 40% of the total pore volume.

[0011] In the method of the present invention, the mass ratio of the modified flaky pseudo-boehmite to the second pseudo-boehmite in step (3) is 1:4-2:3.

[0012] In the method of the present invention, the kneading molding described in step (3) is carried out by conventional methods in the art. During the molding process, conventional molding aids such as peptizers, extrusion aids, etc. may be added as needed. The peptizer is one or more of hydrochloric acid, nitric acid, sulfuric acid, acetic acid, oxalic acid, etc. The mass concentration of the peptizer is 0.5%-2%, and the amount of the peptizer depends on the molding effect; the extrusion aid is sesbania powder, and the amount added is 1%-3% of the final alumina carrier weight. The drying temperature is 100-160°C, and the drying time is 6-10 hours; the calcination temperature is 550-750°C, and the calcination time is 4-6 hours; the calcination is carried out in an oxygen-containing atmosphere, preferably in an air atmosphere.

[0013] In the method of the present invention, the second active component impregnation solution described in step (4) is a solution containing MoO3 and NiO, the MoO3 concentration in the solution is 8.5g / 100mL-15.5g / 100mL, and the NiO concentration is 2.0g / 100mL-3.8g / 100mL. The impregnation is carried out in equal volumes. The drying conditions of the impregnated material are 80-120°C for 4-8 hours, and the calcination conditions are 400-550°C for 4-8 hours.

[0014] The step-pore desulfurization catalyst prepared by the method of the invention is suitable for residual oil hydrodesulfurization and demetallization treatment reactions.

[0015] Compared with the prior art, the present invention has the following advantages: (1) The present invention first prepares a first pseudo-boehmite, which has high crystallinity, a uniform flaky particle structure and is interwoven and stacked to form a large number of 50-150 nm pores. The flaky grains support each other, which can ensure that the pores formed by the stacking are not easily destroyed when the carrier is formed. Therefore, when the flaky pseudo-boehmite is used as a raw material to prepare an alumina carrier, the macropore content of the carrier can be effectively increased.

[0016] (2) The present invention first uses the first active metal impregnation liquid to pre-impregnate the flaky pseudo-boehmite, thereby ensuring that the content of active metal components in the macropores formed by the accumulation of the flaky particles of the prepared catalyst is high and multiple components of Mo, W, and Ni, thereby increasing the number of active sites for the hydrogenation reaction during the hydrogenation reaction. At the same time, the pores formed by the accumulation of the flaky particles are uniform, so that the catalyst can exert high hydrogenation reaction activity while effectively avoiding the catalyst deactivation caused by metal deposition and carbon deposition at the active sites, thereby ensuring the long-term operation of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] FIG. 1 is a SEM image of the flaky pseudo-boehmite P1-1 prepared in Example 1.

[0018] FIG. 2 is an XRD spectrum of the flaky pseudo-boehmite P1-1 prepared in Example 1.

[0019] Figure 3 This is the SEM image of material P1-6 prepared in Comparative Example 3. Implementation

[0020] The technical scheme and technical effect of the present invention are further described below in conjunction with the embodiments, but are not limited to the following embodiments. In the present invention, wt% represents mass fraction.

[0021] BET method: N2 physical adsorption-desorption was used to characterize the pore structure of the carriers of the embodiment and the comparative example. The specific operation was as follows: The pore structure of the sample was characterized by using an ASAP-2420 N2 physical adsorption-desorption instrument. A small amount of sample was vacuum treated at 300°C for 3-4 hours, and finally the product was placed under liquid nitrogen low temperature (-200°C) for nitrogen adsorption-desorption test. The specific surface area was obtained according to the BET equation, and the pore volume and the distribution rate of pore diameters below 30nm were obtained according to the BJH model.

[0022] Scanning electron microscopy was used to characterize the microstructure of the alumina carrier. The specific operation was as follows: a JSM-7500F scanning electron microscope was used to characterize the microstructure of the carrier, with an accelerating voltage of 5 KV, an accelerating current of 20 µA, and a working distance of 8 mm.

[0023] Mercury intrusion method: A mercury intrusion instrument was used to characterize the pore diameter distribution of the carriers of the embodiment and the comparative example. The specific operation is as follows: The pore distribution of the sample was characterized using the American Micromeritics AutoPore 9500 fully automatic mercury intrusion instrument. After the sample was dried, it was weighed and loaded into the dilatometer, and degassed for 30 minutes under the vacuum conditions given by the instrument, and then loaded with mercury. The dilatometer was then placed in an autoclave and vented. Then, a pressure increase and pressure reduction test was performed. The mercury contact angle was 130°, and the mercury interfacial tension was 0.485N.cm -1 The distribution rate of pores with a diameter of more than 100 nm is measured by mercury intrusion porosimetry.

[0024] The most probable pore size determination: Take the material pore size as the horizontal coordinate and the rate of change of pore volume with pore size as the vertical coordinate to obtain the pore size differential distribution curve. The peak value in the curve is the most probable pore size.

[0025] The GB / T 34099-2017 standard method was used to determine the Ni and V contents in oil products.

[0026] V+Ni removal rate % = (metal V+Ni content of crude oil - metal V+Ni content of product) / metal V+Ni content of crude oil × 100%.

[0027] Relative demetallization rate: Determine the demetallization rate of a certain catalyst, define its relative demetallization rate as 100%, and the impurity removal rate of other catalysts / defined catalyst impurity removal rate × 100% is the relative deimpurity removal rate.

[0028] Preparation of active metal modified flake pseudo-boehmite material HP: Example 1

[0029] Weigh an appropriate amount of aluminum nitrate and place it in a crucible and roast it at 500℃ for 6.5 hours. The particles were crushed and sieved to obtain particles with a size of 200 mesh or larger. 100 g of the sieved particles were weighed, 500 g of a 6.5% propylene oxide aqueous solution was added, and magnetic stirring was performed for 30 minutes. The mixture was then transferred to an autoclave and sealed, and heated at 145°C for 5.5 hours. After cooling, the solid material was filtered, washed, and dried at 140°C for 5 hours to obtain flaky pseudo-boehmite P1-1. The microstructure of the sample was observed to be flaky grain accumulation by scanning electron microscopy. The scanning electron microscopy image is shown in FIG. Figure 1 , XRD pattern see Figure 2 , P1=1.12, P2=1.29, D(120) is 84Å, D(031) is 75Å, and D(020) is 65Å.

[0030] (2) Weigh an appropriate amount of the flaky pseudo-boehmite prepared in step (1), and impregnate it with a first active component impregnation solution having a WO3 concentration of 3.0 g / 100 mL and a NiO concentration of 0.7 g / 100 mL for 2 hours. After impregnation, the material is dried at 140° C. for 5 hours to obtain active metal-modified flaky pseudo-boehmite HP1-1.

[0031] (3) Weigh 100 g of the active metal modified flaky pseudo-boehmite HP1-1 prepared in step (2), 233 g of pseudo-boehmite P2 (prepared by the aluminum sulfate-sodium aluminate method, with pores of 10-20 nm accounting for 55% of the total pore volume), and 3.5 g of sesbania powder, mix the above materials evenly, then add an appropriate amount of 1% acetic acid solution, knead the mixture evenly, and extrude into strips. The shaped product is dried at 130°C for 8 hours and calcined at 600°C for 5 hours to obtain the active metal modified alumina carrier of the present invention.

[0032] (4) Weigh 50 g of the active metal-modified alumina carrier prepared in step (3), and spray the active metal-modified alumina carrier with a second active component impregnation solution having a MoO3 concentration of 13.1 g / 100 mL and a NiO concentration of 3.5 g / 100 mL in a saturated impregnation manner. The impregnated material is dried at 140° C. for 5 hours and calcined at 450° C. for 5 hours to obtain the step pore hydrogenation catalyst Cat-1 of the present invention. The catalyst properties are shown in Table 1. Example 2

[0033] Same as Example 1, except that the calcination temperature of aluminum nitrate in step (1) is 550°C, the calcination time is 5.5 hours, the concentration of propylene oxide is 5.4%, the amount of solution is 630 g, the hydrothermal treatment temperature is 135°C, the treatment time is 6.5 hours, and the obtained flaky pseudo-boehmite has P1=1.13, P2=1.31, D(120) is 93Å, D(031) is 82Å, and D(020) is 71Å. In step (2), the WO3 concentration in the first active component impregnation solution is 3.5g / 100mL, and the NiO concentration is 0.8g / 100mL. In step (3), the amount of pseudo-boehmite P2 added is 185g. In step (4), the MoO3 concentration in the second active component impregnation is 12.0 g / 100 mL, and the NiO concentration is 3.1 g / 100 mL, to obtain the step pore hydrogenation catalyst Cat-2 of the present invention. The catalyst properties are shown in Table 1. Example 3

[0034] Same as Example 1, except that the calcination temperature of aluminum nitrate in step (1) is 450°C, the calcination time is 7.5 hours, the concentration of propylene oxide is 4.3%, the amount of solution is 720 grams, the hydrothermal treatment temperature is 155°C, the treatment time is 4.5 hours, and the obtained pseudo-boehmite has a flaky grain size of P1=1.07, P2=1.33, D(120) is 89Å, D(031) is 83Å, and D(020) is 67Å. In step (2), the WO3 concentration in the first active component impregnation solution is 2.5g / 100mL, and the NiO concentration is 0.6g / 100mL. In step (3), the amount of pseudo-boehmite P2 added is 150 grams. In step (4), the MoO3 concentration in the second active component impregnation is 11.3 g / 100 mL, and the NiO concentration is 2.7 g / 100 mL, to obtain the step pore hydrogenation catalyst Cat-3 of the present invention. The catalyst properties are shown in Table 1. Example 4

[0035] Same as Example 1, except that the calcination temperature of aluminum nitrate in step (1) is 600°C, the calcination time is 4.5 hours, the concentration of propylene oxide is 7.5%, the amount of solution is 430 grams, the hydrothermal treatment temperature is 125°C, the treatment time is 7.5 hours, and the obtained pseudo-boehmite has a flaky grain size of P1=1.17, P2=1.28, D(120) is 96Å, D(031) is 82Å, and D(020) is 75Å. In step (2), the WO3 concentration in the first active component impregnation solution is 4.0g / 100mL, and the NiO concentration is 1.0g / 100mL. In step (3), the amount of pseudo-boehmite P2 added is 300 grams. In step (4), the MoO3 concentration in the second active component impregnation is 13.5 g / 100 mL, and the NiO concentration is 4.2 g / 100 mL, to obtain the step pore hydrogenation catalyst Cat-4 of the present invention. The catalyst properties are shown in Table 1.

[0036] Comparative Example 1 The same method as in Example 1 was used, except that the propylene oxide in step (1) was replaced by the same amount of ethylene oxide. After the hydrothermal treatment, no lamellar grains were observed in the microstructure of the material P1-5. A comparative catalyst Cat-5 was obtained. The catalyst properties are shown in Table 1.

[0037] Comparative Example 2 The same as Example 1, except that the aluminum nitrate in step (1) is replaced by aluminum sulfate, and the solid material particles are dissolved after hydrothermal treatment, and the product is not separated.

[0038] Comparative Example 3 The same as Example 1, except that the aluminum nitrate in step (1) was replaced by aluminum chloride. No lamellar grains were observed in the microstructure of the material P1-6 after hydrothermal treatment. P1=1.09, P2=1.46, D(120) was 76Å, D(031) was 70Å, and D(020) was 52Å. The SEM image is shown in Figure 3 , a comparative catalyst Cat-6 was prepared, and the catalyst properties are shown in Table 1.

[0039] Comparative Example 4 The same method as Example 1 was used except that the impregnation process in step (2) was omitted. Instead, a one-step impregnation method was used to prepare a comparative catalyst Cat-7 having the same active metal loading. The catalyst properties are shown in Table 1.

[0040] Table 1 Catalyst properties Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 3 Comparative Example 4 catalyst Cat-1 Cat-2 Cat-3 Cat-4 Cat-5 Cat-6 Cat-7 <![CDATA[Specific surface area, m 2 / g]]> 213 193 181 232 168 151 198 Pore ​​volume, mL / g 0.93 0.91 0.95 0.94 0.81 0.76 0.92 <![CDATA[MoO3 content, wt%]]> 12.9 11.7 11.5 13.2 13.1 13.3 12.8 NiO content, wt% 3.8 3.5 2.9 4.3 3.9 4.1 3.8 <![CDATA[WO3 content, wt%]]> 1.3 1.7 1.4 1.4 1.2 1.4 1.3 10-30nm pore content, v% 59.3 57.6 55.1 61.1 62.5 61.2 58.1 50-100nm pore content, v% 17.3 18.9 22.6 15.4 3.5 1.7 17.9

[0041] The catalytic performance of the step-pore desulfurization catalysts (Cat-1-Cat-7) prepared in the above examples and comparative examples was evaluated by the following method: Using a certain residual oil as raw material, the metal (Ni+V) content in the raw oil is 113μg / g, and the sulfur content is 0.26wt%. The catalytic performance of the stepped pore hydrogenation catalyst Cat-1-Cat-6 was evaluated on a 200mL small evaluation device. The reaction conditions are as follows: reaction temperature 385℃, pressure 14.0MPa, liquid hourly volume space velocity 0.70h -1 The volume ratio of hydrogen to oil was 800. The content of each impurity in the generated oil was determined after 3000 hours of reaction, and the impurity removal rate was calculated. The evaluation results are shown in Table 2.

[0042] Table 2 Comparison of catalyst hydrogenation performance Catalyst No. Cat-1 Cat-2 Cat-3 Cat-4 Cat-5 Cat-6 Cat-7 Relative demetallization (V+Ni) rate, % 126 135 138 123 100 93 116 Relative desulfurization rate, % 129 126 128 133 100 95 120 It can be seen from the data in Table 2 that, compared with the comparative catalyst, the catalyst prepared by the method of the present invention has higher hydrodemetallization activity and hydrodesulfurization activity.

Claims

1. A method for preparing a step-pore desulfurization catalyst, characterized in that It includes the following contents: (1) preparing a first pseudo-boehmite with the following properties: 1.0 < P1 ≤ 1.3, 1.1 < P2 ≤ 1.5, P1 = D(120) / D(031), P2 = D(120) / D(020), where D represents the grain size of the crystal plane corresponding to the characteristic peak in the XRD spectrum of the pseudo-boehmite grains; (2) impregnating the first pseudo-boehmite with a first active component impregnating solution, and drying the impregnated material to obtain a modified pseudo-boehmite; (3) kneading and molding the modified pseudo-boehmite with a second pseudo-boehmite, and drying and calcining the molded product to obtain a modified alumina support; (4) impregnating the modified alumina support with a second active component impregnating solution, and drying and calcining the impregnated material to obtain a hierarchical pore hydrogenation catalyst.

2. The method according to claim 1, characterized in that: In the first pseudo-boehmite prepared in step (1), D(120) represents the grain size of the crystal plane corresponding to the (120) peak in the XRD spectrum of the pseudo-boehmite grains, and D(120) is 75 - 105 Å; D(031) represents the grain size of the crystal plane corresponding to the (031) peak in the XRD spectrum of the pseudo-boehmite grains, and D(031) is 70 - 90 Å; D(020) represents the grain size of the crystal plane corresponding to the (020) peak in the XRD spectrum of the pseudo-boehmite grains, and D(020) is 60 - 70 Å; the 120 peak refers to the characteristic peak with 2θ of 25.5 - 29.9º in the XRD spectrum; the 031 peak refers to the characteristic peak with 2θ of 36.3 - 40.5º in the XRD spectrum; the 020 peak refers to the characteristic peak with 2θ of 12.0 - 16.2º in the XRD spectrum, and D = Kλ / (Bcosθ), where K is the Scherrer constant, λ is the diffraction wavelength of the target, B is the half-peak width of the diffraction peak, and θ is the diffraction angle.

3. The method according to claim 1, characterized in that: The preparation method of the first pseudo-boehmite is as follows: pulverize and screen the roasted nitric acid to obtain a powdery material, immerse the powdery material in a propylene oxide solution for sealed heat treatment, and dry the treated material to obtain the first pseudo-boehmite; the first pseudo-boehmite has a flaky structure.

4. The method according to claim 3, characterized in that: In the preparation method of the first pseudo-boehmite, the roasting temperature is 450 - 650 °C, and the roasting time is 4 - 8 hours; the particle size of the powdery material is greater than 100 mesh, preferably greater than 200 mesh.

5. The method according to claim 3, characterized in that: In the preparation method of the first pseudo-boehmite, the mass concentration of the propylene oxide solution is 2.5% - 12%, and the mass ratio of the propylene oxide solution dosage to the aluminum-containing oxide is 3:1 - 10:1; the hydrothermal treatment is carried out in a closed container, the hydrothermal treatment temperature is 110 - 180 °C, preferably 120 - 160 °C, the treatment time is 4 - 8 hours, and the pressure in the sealed container during the hydrothermal treatment is the autogenous pressure.

6. The method according to claim 1, characterized in that: The first active component impregnation solution described in step (2) is a W-Ni-P solution containing WO3 and NiO, the WO3 content in the solution is 1-5g / 100mL, the NiO content is 0.2-1g / 100mL, the amount of impregnation solution is to completely immerse the material, the impregnation time is 1-4 hours, the drying temperature is 100-160°C, and the drying time is 2-8 hours.

7. The method according to claim 1, characterized in that: The second pseudo-boehmite in step (3) has a pore size of 10-20 nm, preferably a pseudo-boehmite in which the pore content of 10-20 nm accounts for more than 40% of the total pore volume.

8. The method according to claim 1, characterized in that: The mass ratio of the modified flaky pseudo-boehmite to the second pseudo-boehmite in step (3) is 1:4-2:

3.

9. The method according to claim 1, characterized in that: The second active component impregnation solution described in step (4) is a solution containing MoO3 and NiO, wherein the MoO3 concentration in the solution is 8.5g / 100mL-15.5g / 100mL, and the NiO concentration is 2.0g / 100mL-3.8g / 100mL. The impregnation is carried out in equal volumes. The material after impregnation is dried at 80-120°C for 4-8 hours and calcined at 400-550°C for 4-8 hours.

10. Use of a stepped pore desulfurization catalyst prepared by the method according to any one of claims 1 to 9 in a residual oil hydrodesulfurization and demetallization treatment process.

Citation Information

Patent Citations

  • Heavy oil hydrogenation catalyst and preparation method thereof

    CN106140180A

  • Mesoporous and macroporous catalyst with an active phase obtained by comulling, method for preparing same and use thereof for the hydrotreatment of residuum

    CN106660019A

  • Preparation method for hydrodemetallization catalyst

    CN107303490A

  • Preparation method of hydrodemetallization catalyst

    CN111774065A

  • Composite hierarchical pore catalysis-adsorption material and preparation method thereof

    CN115178234A