Preparation method of catalytic cracking catalyst

By using NaY molecular sieve and humic acid to form a filter cake layer in catalyst production to recover ammonium ions in ammonia nitrogen wastewater, and combining it with rare earth exchange liquid for ion exchange, the problem of ammonia nitrogen pollution in catalytic cracking catalyst production is solved and low sodium oxide is achieved. The catalyst preparation with high content and low water consumption meets the requirements of ammonia-free production and environmental protection.

CN118767972AActive Publication Date: 2024-10-15PETROCHINA CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310354325.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-15
Estimated Expiration
2043-04-04

AI Technical Summary

Technical Problem

Ammonia nitrogen pollution is serious during the production process of catalytic cracking catalysts, and it is difficult to achieve ammonia-free production with existing technology, resulting in high production costs and environmental pollution.

Method used

By beating NaY molecular sieve with humic acid to form a filter cake layer, the filter cake layer is used to recover ammonium ions in ammonia nitrogen wastewater, and combined with rare earth exchange liquid for ion exchange, reducing the use of ammonium salt and achieving low sodium oxide content and low water content of the catalyst. Consumption.

Benefits of technology

It effectively reduces the water consumption and ammonium salt consumption in the catalyst production process, realizes green production of the catalyst and direct wastewater discharge, meets the national first-level emission standards, and simplifies the operation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767972A_ABST
    Figure CN118767972A_ABST
Patent Text Reader

Abstract

The invention provides a catalytic cracking catalyst preparation method, which comprises: forming a NaY molecular sieve filter cake layer, loading a Y-type molecular sieve after ammonia nitrogen wastewater exchange on the NaY filter cake, and recovering excess ammonium ions in ammonia nitrogen wastewater through the alkaline characteristic of the NaY filter cake layer and the ammonium ion adsorption characteristic of the NaY molecular sieve, meanwhile, excessive ammonium ions can also exchange part of Na < + > of the NaY molecular sieve in the recycling process of the NaY molecular sieve layer, Na < + > of the NaY molecular sieve layer is effectively removed, and ammonium ions lost by ammonia-nitrogen wastewater are recycled through the adsorption effect and the ion exchange effect of the NaY molecular sieve, so that ammonium ion recycling is achieved. The humic acid added in the NaY molecular sieve slurry is a multi-element organic complex and is dissolved in a NaY molecular sieve system to form sodium humate, the sodium humate can limit migration of ammonium ions in filtrate through adsorption and exchange with the ammonium ions, and loss of the ammonium ions along with the filtrate is inhibited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of catalyst preparation, and in particular to a method for preparing a catalytic cracking catalyst. Background Art

[0002] As we all know, the petroleum refining industry is an important pillar of the national economy. It has a long industrial chain, a wide range of products, and is closely related to people's lives. The most important refining method in the process of petroleum refining is catalytic cracking technology. 70% of gasoline, 40% of diesel, and 35% of propylene required in my country come from catalytic cracking, and catalytic cracking catalysts are the core content of catalytic cracking.

[0003] In order to reduce the sodium oxide content in the catalyst, which has an important influence on the catalytic activity, selectivity and stability, ammonium salts are commonly used in the production process of catalytic cracking catalysts to reduce the sodium content in the catalyst and its active component zeolite molecular sieve. + Ion exchange is performed, for example, Chinese patents CN1210034A and US4357265 disclose a method for preparing a molecular sieve using ammonium salts for exchange. In order to improve the exchange degree of sodium ions, multiple ammonium exchanges and multiple washing methods are often used. The waste liquid after molecular sieve exchange and catalyst washing is high ammonia nitrogen wastewater, which increases the investment and maintenance cost of ammonia nitrogen removal equipment of enterprises, increases production costs and sewage treatment burdens, and in addition, ammonia nitrogen exchanged or adsorbed on molecular sieves or catalysts will enter the atmosphere during the intermediate roasting process, and will also cause air pollution. Therefore, reducing production costs and solving ammonia nitrogen pollution in the catalyst preparation process are also the key points and difficulties in the development of catalytic cracking catalysts.

[0004] CN103240113A discloses a method for preparing an in-situ crystallization catalyst that reduces ammonia nitrogen pollution, which includes adding polydimethyldiallyl ammonium chloride that can adjust the stacking mode between kaolin during spraying, and after obtaining the in-situ crystallization product, first using an acidic solution to clean the exchange environment of the exchange ions, and then through other steps of exchange and roasting to obtain a catalytic cracking catalyst. The method can reduce the amount of ammonium salt used by more than 15%, effectively alleviate the ammonia nitrogen pollution problem in the preparation process of the in-situ crystallization catalyst, and reduce the production cost and improve the reaction performance of the catalyst.

[0005] CN100404432C discloses a method for reducing ammonia nitrogen pollution in the process of zeolite modification, which includes exchanging sodium in zeolite with potassium compound in the process of zeolite modification, and further exchanging and modifying the zeolite with ammonium salt. The method does not increase the cost of zeolite modification, and the amount of ammonium salt used is reduced by about 50%, thereby reducing ammonia nitrogen pollution and the burden and investment in the process of ammonia nitrogen wastewater treatment. It is an environmentally friendly technology for modifying zeolite; the prepared zeolite and catalyst have a lower sodium oxide content, and the catalyst performance is basically unchanged or improved.

[0006] CN103028431A discloses a clean production process of a molecular sieve catalytic cracking catalyst, which adopts a conventional in-situ crystallization method to prepare a modified molecular sieve or a molecular sieve catalytic cracking catalyst, and mixes the molecular sieve crystallization filtration mother liquor and / or the crystallization material washing water with the ammonia nitrogen wastewater generated in the molecular sieve exchange process as the spray washing liquid of the spray washing tower of the catalyst spray granulation tail gas, and adds the acidified aluminum salt or acid solution to the above-mentioned spray recovery liquid, gelling, filtering, filtrate discharge, and filter residue as a synthetic molecular sieve raw material. While preparing a qualified catalytic cracking catalyst product, the method can directly meet the discharge standards of the high ammonia nitrogen content wastewater generated in the process at a very low operating cost, and the silicon compounds in the wastewater can be fully recovered and recycled.

[0007] Although the above methods greatly reduce the ammonia nitrogen wastewater in the catalytic cracking preparation process, ammonium ions are still introduced more or less, and it is impossible to achieve ammonia-free production. The ammonia nitrogen content of the filtrate in the ammonium exchange step is as high as 4000-10000 mg / kg, and even the ammonia nitrogen content in the washing water is 150-1500 mg / kg, while the national standard "Comprehensive Sewage Discharge Standard" requires that the primary discharge standard of ammonia nitrogen is 15 mg / kg and the secondary discharge standard is 50 mg / kg. Therefore, with the implementation of the new "Environmental Protection Law" and the improvement of citizens' environmental awareness, people are in urgent need of developing a new technology for preparing catalytic cracking catalysts with simple process, low cost and no ammonia in the production process.

[0008] Patent CN102795636B discloses an exchange modification method for reducing the sodium oxide content in Y-type molecular sieves, characterized in that the Y molecular sieve with a high sodium content is contacted with an aqueous solution containing an inorganic acid and an organic acid at 0-5°C for 0.5-3 hours, and then separated, washed, and dried to obtain a Y molecular sieve with a low sodium oxide content; wherein the weight ratio of H2O: molecular sieve is 11-18:1. In the process of significantly reducing the sodium oxide content in the Y molecular sieve, this method does not use ammonium salt at all, eliminates the ammonia nitrogen pollution problem from the source, and also significantly reduces the water consumption and wastewater discharge during the exchange process of the Y molecular sieve.

[0009] Patent CN102557070B discloses a method for removing sodium by exchange using organic carboxylic acid during the preparation of a Y-type molecular sieve, wherein NaY molecular sieve, organic carboxylic acid and a dispersion medium are mixed, stirred, filtered, washed and dried to obtain a NaHY molecular sieve; wherein the organic carboxylic acid is acetic acid; the raw material ratio is acetic acid / NaY molecular sieve = 0.15-0.6mmol / g, dispersion medium / NaY molecular sieve = 5-200 (w / w). The method of the present invention avoids the introduction of inorganic ammonium salt as a byproduct, reduces the generation of unnecessary inorganic salt byproducts during the exchange process, and reduces the impact of nitrogen-containing wastewater discharge on the environment.

[0010] Patent CN102794191B discloses a new method for preparing catalytic cracking catalysts without ammonia, in which the molecular sieve and catalyst exchange process is carried out in a mixed acid solution of inorganic acid and organic acid at low temperature and low acid concentration. The above method reduces the sodium oxide content in the catalyst, avoids ammonia nitrogen pollution in the molecular sieve exchange and catalyst washing process, and greatly reduces water consumption and wastewater treatment costs. The use of inorganic acid and organic acid to exchange and wash the molecular sieve and catalyst to reduce sodium is likely to destroy the molecular sieve crystal structure, resulting in poor crystallinity of the molecular sieve in the catalyst, reducing the thermal stability and hydrothermal stability of the catalyst; and this method needs to be exchanged at a temperature of 0-5°C, the operating conditions are harsh, and industrial operation is difficult.

[0011] Patent CN102553630A uses the traditional in-situ crystallization method to prepare NaY molecular sieve microspheres, and then contacts them with silicon tetrachloride gas at a weight ratio of 0.1-0.9:1, reacts at 150-500°C for 10 minutes to 6 hours, and washes the in-situ crystallized NaY zeolite microspheres with deionized water at 20-100°C to remove the residual Na + , Cl - 、Al 3+ The soluble by-products are then used to prepare a catalytic cracking catalyst containing a small-grain Y-type molecular sieve with a high silicon-aluminum ratio. However, the modified method still cannot avoid the disadvantages of difficult in-situ crystallization technology, high production cost, and difficulty in reducing the sodium content of the molecular sieve or catalyst.

[0012] Patent CN106732745B discloses a method for preparing a catalytic cracking catalyst, which is characterized in that the method contacts NaY molecular sieve raw powder with halogen-containing gas to carry out gas-phase ion exchange reaction, completes the sodium reduction and ultra-stabilization of the NaY molecular sieve raw powder in one step, and obtains a low-sodium high silicon-aluminum ratio molecular sieve. The method also compounds different types of clay ores and treats them with high-concentration acid to obtain acid-activated composite clay, then mixes the low-sodium high silicon-aluminum ratio molecular sieve and the acid-activated composite clay with a binder, rare earth, and decationized water, and then sprays and granulates them, and then solidifies them by roasting without washing or drying to obtain a finished catalytic cracking catalyst.

[0013] Halogen-containing gas (such as silicon tetrachloride) is used to contact Y-type molecular sieve or catalyst at high temperature. While removing aluminum, silicon fills into aluminum vacancies. The removed aluminum escapes in the form of aluminum chloride gas. At the same time, aluminum chloride reacts with sodium in the molecular sieve to form NaAlCl4 complex salt, and then sodium ions are removed by water washing or acid extraction. This process completely eliminates ammonia nitrogen pollution. However, silicon tetrachloride is hydrolyzed to form silica gel and hydrochloric acid. Silica gel is very easy to clog pipelines, and hydrochloric acid is extremely destructive to equipment and molecular sieves. At the same time, chlorine is highly corrosive and cannot be discharged into the atmosphere. It can only be absorbed by water for sewage discharge, which will cause the salt content in sewage to increase dramatically and waste chlorine.

[0014] Patent CN1840614A contacts one or more of the dried NaY, RENaY, REHY or REY molecular sieves with silicon tetrachloride according to a weight ratio of silicon tetrachloride: Y-type molecular sieve = 0.1-0.9:1, reacts at 100-600°C for 10 minutes to 6 hours, and removes more than 90% by weight of the sodium oxide from the Y-type molecular sieve after the gas-phase ion exchange reaction. The Y-type molecular sieve after the reaction is then directly mixed with a binder and clay for pulping, spray-formed, washed, filtered, and dried to obtain a finished catalytic cracking catalyst. The disadvantage of this method is that when the rare earth-containing Y-type molecular sieve is subjected to gas-phase ion exchange, the rare earth ions will be largely exchanged with silicon tetrachloride, reducing the utilization rate of the rare earths; at the same time, after the molecular sieve is ultra-stabilized after sodium reduction, it does not undergo a washing and exchange step, but is directly pulped and sprayed with other raw materials, which will result in the removal of harmful ions such as Na + NH4 + 、SO4 2- ions etc. re-enter the molecular sieve and catalyst.

[0015] In summary, the use of acid exchange and gas-phase ion exchange can reduce the discharge of ammonia nitrogen wastewater in the catalyst production process, but the acid exchange conditions are harsh and gas-phase ion exchange requires increased equipment investment. The above technical solutions cannot meet the requirements for direct discharge of ammonia nitrogen wastewater from existing catalyst production equipment.

[0016] Therefore, how to effectively improve the utilization rate of ammonium ions in the production process of existing catalyst equipment and reduce the discharge of ammonia nitrogen wastewater is an important measure for catalyst manufacturers to reduce costs and increase efficiency, and is also one of the key research topics for catalyst manufacturers. Summary of the invention

[0017] The purpose of the present invention is to provide a method for preparing a catalytic cracking catalyst, so as to solve the problem of serious ammonia nitrogen pollution in the production process of the catalytic cracking catalyst, realize direct discharge of catalyst wastewater on the existing catalyst production device without additional investment, and ensure the green production of the catalyst.

[0018] To achieve the above object, the present invention provides a method for preparing a catalytic cracking catalyst, comprising the following steps:

[0019] 1) Slurrying NaY molecular sieve, humic acid and water, filtering to form a NaY molecular sieve filter cake layer, wherein the dry weight ratio of humic acid to NaY molecular sieve is 0.001-0.05;

[0020] 2) Slurrying the Y-type molecular sieve and ammonia nitrogen wastewater to obtain a Y-type molecular sieve slurry, filtering the Y-type molecular sieve slurry through a NaY molecular sieve filter cake layer to obtain a composite filter cake layer, and then exchanging ions through a first ammonium salt exchange solution and / or a rare earth exchange solution, and washing with water to obtain a composite molecular sieve filter cake; the Y-type molecular sieve is a cross-linked and baked Y-type molecular sieve and / or a double cross-linked and baked Y-type molecular sieve, and the weight ratio of the ammonium salt in the first ammonium salt exchange solution to the total amount of the NaY molecular sieve dry basis and the Y-type molecular sieve dry basis is 0-0.2; the weight ratio of the rare earth in the rare earth exchange solution in terms of rare earth oxide to the total amount of the NaY molecular sieve dry basis and the Y-type molecular sieve dry basis is 0-0.10;

[0021] 3) Mixing the composite molecular sieve filter cake, inorganic oxide, clay, binder and water for slurrying, spray drying for forming, calcining for solidification to obtain catalyst microspheres, mixing the catalyst microspheres with water for slurrying, filtering, performing ion exchange with a second ammonium salt exchange solution, washing with water, and drying to obtain a catalytic cracking catalyst; wherein the weight ratio of the ammonium salt in the second ammonium salt exchange solution to the catalyst microspheres on a dry basis is 0.005-0.10.

[0022] In the preparation method of the catalytic cracking catalyst of the present invention, the sodium oxide content of the NaY molecular sieve is 9-15%.

[0023] The NaY molecular sieve in the present invention can be prepared according to the existing method or can be purchased commercially. Its preparation method is well known to those skilled in the art. For example, the NaY molecular sieve synthesis method provided in patent CN103449468B is as follows: water glass, sodium aluminate and deionized water are mixed, and aged at 15-70°C for 0.5 to 48 hours to obtain a crystallization directing agent; the crystallization directing agent, water glass, acidic aluminum salt and sodium aluminate solution are uniformly mixed to obtain a silica-alumina gel; the silica-alumina gel is crystallized at 80 to 140°C; the crystallization is carried out for 0.1 to 80 hours; peroxide is added to the crystallized silica-alumina gel, and the O2 in the peroxide is allowed to form. 2- The molar ratio of Al2O3 to the gel is 0.05-20, and the crystallization is continued for 5-20 hours to obtain.

[0024] The slurry conditions of NaY molecular sieve and water are well known to those skilled in the art, and the content of NaY molecular sieve in the slurry is generally 100-300 g / L. The temperature of the slurry can be 10-100°C, preferably 50-90°C.

[0025] In the preparation method of the catalytic cracking catalyst of the present invention, the humic acid is one or more of fulvic acid, palmitic acid and black humic acid.

[0026] In the method for preparing the catalytic cracking catalyst of the present invention, the ammonium salt is one or more of ammonium chloride, ammonium sulfate, ammonium oxalate, ammonium phosphate and ammonium bicarbonate, preferably ammonium chloride and / or ammonium sulfate.

[0027] In the preparation method of the catalytic cracking catalyst of the present invention, the rare earth is rare earth nitrate and / or chloride, and the rare earth is one or more of lanthanum, cerium, praseodymium, neodymium and yttrium.

[0028] In the preparation method of the catalytic cracking catalyst of the present invention, the cross-pyratory Y type molecular sieve is one or more of a cross-pyratory ultra-stable Y molecular sieve, a cross-pyratory rare earth Y molecular sieve, a cross-pyratory rare earth hydrogen Y molecular sieve and a cross-pyratory hydrogen Y molecular sieve; the double cross-pyratory Y type molecular sieve is one or more of a double cross-pyratory ultra-stable Y molecular sieve, a double cross-pyratory rare earth Y molecular sieve, a double cross-pyratory rare earth hydrogen Y molecular sieve and a double cross-pyratory hydrogen Y molecular sieve.

[0029] In the preparation method of the catalytic cracking catalyst of the present invention, the inorganic oxide is one or more of rare earth oxide, magnesium oxide and silicon oxide; the clay is one or more of kaolin, halloysite and montmorillonite; and the binder is one or more of aluminum sol, silica sol and pseudo-boehmite.

[0030] In the method for preparing the catalytic cracking catalyst of the present invention, the ammonia nitrogen wastewater in step 2) is the filtrate collected during the ion exchange process in step 2) and / or the filtrate collected during the ion exchange process in step 3), or it can be the ammonium-containing filtrate collected outside this process, preferably the filtrate collected during the ion exchange process in step 3).

[0031] In the method for preparing the catalytic cracking catalyst of the present invention, in step 2), the mass ratio of ammonia nitrogen wastewater to Y-type molecular sieve is 2-10, preferably 3-6.

[0032] The spray drying and calcination curing conditions in the present invention are well known to those skilled in the art, such as the drying temperature is from room temperature to 200°C, preferably 100-150°C, the calcination curing temperature is 300-600°C, preferably 400-500°C, and the calcination time is 10-200 minutes, preferably 30-60 minutes.

[0033] The method for preparing the catalytic cracking catalyst of the present invention comprises steps 1) and 2) being carried out on a first horizontal belt filter, wherein the first horizontal bag filter comprises a NaY molecular sieve filter cake layer forming zone, a composite filter cake layer forming zone, an ion exchange zone and a water washing zone connected in series; and step 3) being carried out on a second horizontal belt filter, wherein the second horizontal belt filter comprises a filter cake forming zone, an ion exchange zone and a water washing zone connected in series.

[0034] Beneficial effects of the present invention:

[0035] The method for preparing a catalytic cracking catalyst provided by the present invention comprises the following steps: firstly forming a NaY molecular sieve filter cake layer, then loading a Y-type molecular sieve after exchanging ammonia nitrogen wastewater on the NaY filter cake, and recovering excess ammonium ions in the ammonia nitrogen wastewater by using the alkalinity characteristics of the NaY filter cake layer and the characteristics of the NaY molecular sieve for adsorbing ammonium ions; at the same time, the excess ammonium ions can also be exchanged for part of the NaY molecular sieve Na during the recycling process of the NaY molecular sieve layer. + , effectively remove Na from the NaY molecular sieve layer + , the adsorption and ion exchange of NaY molecular sieve recover the ammonium ions lost in the ammonia nitrogen wastewater to achieve the recycling of ammonium ions. The humic acid added to the NaY molecular sieve slurry of the present invention is a multi-organic complex, which is dissolved in the NaY molecular sieve system to form sodium humate. Sodium humate can limit the migration of ammonium ions in the filtrate through adsorption and exchange with ammonium ions, and inhibit the loss of ammonium ions with the filtrate. The catalytic cracking catalyst preparation method provided by the present invention recovers the catalyst microsphere ammonia nitrogen wastewater for the molecular sieve ion exchange process, which can effectively reduce the water consumption and ammonium salt consumption in the catalyst production process, and is conducive to reducing the production cost of the catalyst. Therefore, compared with the prior art, the preparation method of the catalytic cracking catalyst provided by the present invention does not require additional investment, and the wastewater direct discharge requirements can be achieved on the existing production equipment, and the operation process is simple, providing technical support for green production and energy saving and consumption reduction of catalyst enterprises. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a flow chart of the molecular sieve ion exchange process of the present invention;

[0037] Figure 2 The figure is a flow chart of the ion exchange process of the catalyst microspheres of the present invention.

[0038] Wherein, the reference numerals are:

[0039] 1, 5, 15, 16 beating tanks;

[0040] Pipelines 2, 6, 10, 13, 17, 21, 25;

[0041] 3. 18 filter cloth;

[0042] 4 NaY filter cake formation area

[0043] 7 Y-type molecular sieve filter cake formation area

[0044] 8.23 Liquid receiver

[0045] 9, 12, 20, 24 containers

[0046] 14, 26 washing area

[0047] 19 Microsphere filter cake formation area

[0048] 11, 22 ion exchange area

[0049] 27 Recover filtrate DETAILED DESCRIPTION

[0050] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention.

[0051] According to the method provided by the present invention, Figure 1 , Figure 2 The process flow shown implements the present invention.

[0052] 1. Formation of NaY filter cake

[0053] NaY molecular sieve, humic acid and water at 10-100°C, preferably 50-90°C, are slurried, and the formed slurry is continuously loaded from the slurry tank 1 to the filter cloth 3 of the horizontal vacuum belt filter through the pipeline 2, and the filter cloth moves continuously and enters the NaY filter cake forming area 4. The liquid receiver 8 is located below the filter cloth 3, and the liquid receiver 8 is evacuated. Under the action of vacuum, the liquid in the slurry on the filter cloth 3 enters the liquid receiver 8 through the filter cloth 3. At the same time, the NaY slurry on the filter cloth 3 forms a filter cake, and the loading speed of the NaY slurry should ensure that the thickness of the formed NaY filter cake is 0.5-1.5 cm, preferably 0.8-1.5 cm. The vacuum degree in the vacuum box 8 ensures that there is no crack on the surface of the filter cake. The vacuum degree in the vacuum box 8 is generally 0.02-0.08 MPa, preferably 0.05-0.08 MPa.

[0054] 2. Formation of Y-type molecular sieve filter cake

[0055] The Y-type molecular sieve and the ammonia nitrogen wastewater are slurried, and the 50-100°C Y-type molecular sieve slurry is continuously loaded from the slurrying tank 5 to the NaY filter cake layer of the horizontal vacuum belt filter through the pipeline 6, and moves into the Y-type molecular sieve filter cake forming area 7 with the filter cloth. The ammonia nitrogen wastewater can be provided by the microsphere exchange process liquid receiver 23 described below, which can reduce the amount of water on the one hand, and can also recover the ammonium in the filtrate of the catalyst microsphere ion exchange process to reduce the sewage discharge. At the same time, the Y-type molecular sieve slurry on the filter cloth 3 forms a filter cake, and the loading speed of the Y-type molecular sieve slurry should ensure that the thickness of the cross molecular sieve filter cake is 0.5-1.5 cm, preferably 0.8-1.5 cm.

[0056] 3. Molecular sieve ion exchange

[0057] As the filter cloth 3 moves, the filter cake formed in the NaY filter cake forming area 4 and the Y-type molecular sieve filter cake forming area 7 enters the ion exchange area 11, and an ammonium salt exchange solution and / or a rare earth exchange solution at a temperature of 20-100° C., preferably 30-90° C., is added from the container 9 through the pipeline 10. Under the action of vacuum, the ammonium salt exchange solution and / or the rare earth exchange solution perform ion exchange while passing through the filter cake.

[0058] 4. Molecular sieve washing

[0059] The washing method is well known to those skilled in the art. The filter cake obtained in the ion exchange zone 11 enters the water washing zone 14, and deionized water is added from the container 12 through the pipeline 13. The weight ratio of deionized water to molecular sieve is generally 1-15, preferably 2-10, and the temperature of the deionized water is 20-100° C., preferably 30-90° C. Under the action of vacuum, the liquid passes through the filter cake to wash away the residual ions, especially the anions, in the filter cake.

[0060] 5. Catalyst microsphere molding and curing

[0061] The washed composite molecular sieve filter cake enters the pulping tank 15, where inorganic oxides, clay, binder and water are added to mix and pulp, spray-formed, and calcined to obtain solidified catalyst microspheres.

[0062] 6. Formation of microsphere filter cake

[0063] The solidified catalyst microspheres are put into the beating tank 16, water is added for beating, and the microsphere slurry is continuously loaded from the beating tank 16 to the filter cloth 18 of the horizontal vacuum belt filter through the pipeline 17, and the filter cloth is continuously moved and enters the microsphere filter cake forming area 19. The liquid receiver 23 is located below the filter cloth 18, and the liquid receiver 23 is evacuated. Under the vacuum effect, the liquid in the slurry on the filter cloth 18 enters the liquid receiver 23 through the filter cloth 18. At the same time, the microsphere slurry on the filter cloth 18 forms a filter cake, and the loading speed of the microsphere slurry should ensure that the thickness of the microsphere filter cake formed is 0.5-2.0 cm, preferably 0.8-1.5 cm. The vacuum degree in the vacuum box 23 is generally 0.02-0.08 MPa, preferably 0.03-0.08 MPa.

[0064] 7. Catalyst microsphere ammonium exchange

[0065] As the filter cloth 18 moves, the filter cake formed in the microsphere filter cake forming area 19 enters the ion exchange area 22, and an ammonium salt solution with a temperature of 20-100° C., preferably 30-90° C., is added from the container 20 through the pipeline 21. Under the action of vacuum, the ammonium salt solution passes through the filter cake while performing ion exchange.

[0066] 8. Catalyst microsphere washing

[0067] The washing method is well known to those skilled in the art. Deionized water is added from container 24 through pipeline 25 to the microsphere filter cake obtained in ion exchange zone 22, and washed in water washing zone 26. The weight ratio of deionized water to microspheres is generally 1-15, preferably 2-10, and the temperature of deionized water is 20-100° C., preferably 30-90° C. Under the action of vacuum, the liquid passes through the filter cake, and the residual ions in the filter cake are washed away to obtain the recovered filtrate 27.

[0068] The following example uses a Buchner funnel filter device to conduct experiments to illustrate the method provided by the present invention. Since the Buchner funnel filter device also undergoes the stages of filter cake formation, ion exchange and washing, but these steps are performed separately, they are equivalent to the continuous process on the belt filter.

[0069] Source of raw materials:

[0070] 1) NaY molecular sieve: industrial product, produced by Lanzhou Petrochemical Company, with a crystallinity of 94%, a silicon-aluminum ratio of 5, and a Na2O content of 14.3%; cross-baked ultra-stable Y molecular sieve: produced by Lanzhou Petrochemical Company, with a Na2O content of 4.1% and a unit cell constant of 24.55 angstroms;

[0071] Double cross-linking and one roasting ultra-stable Y molecular sieve: produced by Lanzhou Petrochemical Company, Na2O content is 1.5%, unit cell constant is 24.54 angstroms;

[0072] Cross-baked hydrogen Y molecular sieve: produced by Lanzhou Petrochemical Company, with a Na2O content of 4.6% and a unit cell constant of 24.65 angstroms;

[0073] Double cross-linked and one baked hydrogenated Y molecular sieve: produced by Lanzhou Petrochemical Company, with a Na2O content of 1.3% and a unit cell constant of 24.65 angstroms;

[0074] Double cross-baked rare earth Y molecular sieve: produced by Lanzhou Petrochemical Company, Na2O content is 1.1%, RE2O3 content is 14.8%, unit cell constant is 24.66 angstroms;

[0075] Kaolin, halloysite, montmorillonite, silica sol, pseudoboehmite and alumina sol were all from Lanzhou Petrochemical Company.

[0076] 2) Fulvic acid, palmitic acid, humic acid, ammonium chloride, ammonium sulfate, ammonium oxalate, ammonium phosphate, ammonium bicarbonate, lanthanum chloride, cerium nitrate, yttrium oxide, magnesium oxide, and white carbon black: analytically pure, all chemical reagents.

[0077] Specific analysis method:

[0078] 1) Molecular sieve sodium oxide content: analyzed by X-ray fluorescence spectrometry.

[0079] 2) Ammonia nitrogen content in the filtrate: detected by Nessler's reagent spectrophotometry.

[0080] Comparative Example 1

[0081] The samples were prepared according to patent CN103028431A.

[0082] The NaY type molecular sieve is filtered and washed with water through a belt filter, the crystallization mother liquor and the crystallization material washing water are collected, the filter cake is exchanged with ammonium (ammonium chloride and NaY molecular sieve dry basis ratio is 0.05:1) twice and the sodium is removed by intermediate roasting to obtain a modified Y molecular sieve with a sodium oxide content of 1.2%; the modified Y molecular sieve: kaolin: aluminum sol (calculated as aluminum oxide): yttrium oxide are mixed into a gel in a ratio of 35:54:10:1, with a solid content of 38%, and finally granulated by spraying in a spray granulation tower to obtain catalytic cracking catalyst microspheres, and then the microspheres are ammonium exchanged on a belt filter, wherein the amount of ammonium chloride is such that the weight ratio of ammonium chloride to microspheres is 0.08, the filter cake has a sodium oxide content of 0.2%, and the filter cake is flash dried to obtain a catalytic cracking catalyst product. The exchange filtrate mixed liquid A was collected, and the ammonia nitrogen content was 5962 μg / g. Crystallization material water and part of the crystallization mother liquor were added to the exchange filtrate mixed liquid to make the pH value of the mixed liquid 12.5. The mixed liquid was then used as the spray washing liquid of the spray washing tower of the spray granulation tower tail gas. The temperature of the spray recovery liquid was 92°C, and the ammonia nitrogen content was 185 μg / g. The sulfated aluminum sulfate solution was then added to the elution recovery liquid to make its pH value 9.5. After aging for 1 hour, the silica-alumina gel was obtained by filtration, and the ammonia nitrogen content of the filtrate was 21 μg / g.

[0083] Comparative Example 2

[0084] The samples were prepared according to patent CN102794191B.

[0085] The preparation of catalytic cracking catalyst comprises the following steps:

[0086] (1) Exchange washing of Y-type molecular sieve containing Na: Weigh 2.7 kg of acetic acid, add appropriate amount of cold water and stir to dissolve it, then add 8.1 kg of hydrochloric acid with a concentration of 36%, and then continue to add cold water to dilute the solution to 1000 L to prepare H + A mixed acid solution with a molar concentration of 0.17 mol / L, the solution temperature is controlled at 3.5±0.5°C, 71.4 kg of dry basis Y-type molecular sieve powder (weight ratio of water: dry basis molecular sieve powder = 14:1) is added during stirring, and then stirred at 3.5±0.5°C for 2 hours, and then the slurry is filtered, and the filter cake is rinsed with deionized water 5 times the weight of the dry basis Y-type molecular sieve powder;

[0087] (2) flash drying the product of step (1) and calcining at 550° C. for 3 hours;

[0088] (3) slurrying the product of step (2) at a ratio of molecular sieve dry basis: water = 1:3 to prepare a molecular sieve slurry;

[0089] (4) adding kaolin, aluminum sol and yttrium oxide to the molecular sieve slurry obtained in step (3) in a ratio of molecular sieve: kaolin: aluminum sol (calculated as aluminum oxide): yttrium oxide = 35:54:10:1 to prepare a catalyst mixed slurry;

[0090] (5) spray drying the slurry obtained in step (4) to prepare catalyst microspheres according to a conventional spray drying molding method for preparing catalytic cracking catalysts;

[0091] (6) Catalyst washing: weigh 540 g of acetic acid, add an appropriate amount of cold water and stir to dissolve it, then add 1620 g of hydrochloric acid with a concentration of 36%, and then continue to add cold water to dilute the solution to 1000 L to prepare a mixed acid solution with a H+ molar concentration of 0.034 mol / L. Control the solution temperature: 3.5±0.5°C, add 143 kg of dry catalyst microspheres prepared in step (5) (in the catalyst washing solution, the weight ratio of water: dry catalyst = 7:1) while stirring, then stir and wash at 3±0.5°C for 20 minutes, then filter, and rinse the filter cake with deionized water 5 times the weight of the catalyst;

[0092] (7) Drying the product gas stream of step (6) to obtain a catalytic cracking catalyst product D2. The sodium oxide content of the D2 sample is 0.1%.

[0093] Comparative Example 3

[0094] 1) The two-crosslinked and one-baked ultra-stable Y-type molecular sieve was mixed and slurried with ammonia nitrogen wastewater (exchange filtrate mixed solution A of comparative example 1), and the mass of the exchange filtrate mixed solution A was 5 times that of the NaY molecular sieve to prepare a two-crosslinked and one-baked ultra-stable Y-type molecular sieve slurry. The obtained two-crosslinked and one-baked ultra-stable Y-type molecular sieve slurry was heated to 70° C. and stirred for 1 h, poured into a Buchner funnel, and the filter bottle was evacuated to 0.07 MPa at the same time, and a one-crosslinked and one-baked Y-type molecular sieve filter cake with a thickness of 10 mm was formed on the filter cloth.

[0095] 3) When there is no liquid on the surface of the filter cake, immediately add a solution containing ammonium chloride at a temperature of 90°C. The addition speed ensures that no cracks are formed on the surface of the filter cake. The amount of ammonium chloride is such that the weight ratio of ammonium chloride to cross-baked Y-type molecular sieve is 0.10. When there is no liquid on the surface of the filter cake, immediately add deionized water at a temperature of 80°C to wash the filter cake. The weight ratio of deionized water to cross-baked Y-type molecular sieve is 5. Then remove the molecular sieve filter cake and collect filtrate B.

[0096] 4) adding kaolin, aluminum sol and yttrium oxide to the molecular sieve slurry obtained in step (3) in a ratio of molecular sieve: kaolin: aluminum sol (calculated as aluminum oxide): yttrium oxide = 35:54:10:1 to prepare a catalyst mixed slurry;

[0097] 5) The slurry obtained in step (4) is spray-dried to prepare catalyst microspheres according to a conventional spray-drying molding method for preparing catalytic cracking catalysts, and then calcined and solidified.

[0098] 6) Catalyst washing: The catalyst microspheres solidified in step 5) were mixed with water to prepare a slurry having a catalyst microsphere content of 110 g / L. The obtained slurry was heated to 60° C. and poured into a Buchner funnel. The filter bottle was evacuated to 0.06 MPa to form a filter cake with a thickness of 10 mm on the filter cloth.

[0099] 7) When there is no liquid on the surface of the filter cake in step 6), immediately add a solution containing ammonium chloride at a temperature of 90°C, and the amount of ammonium chloride is such that the weight ratio of ammonium chloride to microspheres is 0.08. When there is no liquid on the surface of the filter cake, immediately add deionized water at a temperature of 90°C to wash the filter cake, and the weight ratio of deionized water to microspheres is 5. Then remove the filter cake and collect the filtrate C, and dry it to obtain a catalyst sample D3, whose sodium oxide content is 0.1%, and the ammonia nitrogen content of the filtrate B is 1328ppm.

[0100] Example 1

[0101] 1) Mix NaY molecular sieve, fulvic acid and water to make a molecular sieve slurry with a molecular sieve content of 180 g / L, wherein the amount of fulvic acid added is 0.03:1 on a dry basis weight basis of fulvic acid to NaY molecular sieve. Heat the obtained molecular sieve slurry to 80°C and pour it into a Buchner funnel. At the same time, evacuate the filter bottle to 0.07 MPa to form a filter cake with a thickness of 10 mm on the filter cloth.

[0102] 2) The two-cross-baked ultra-stable Y-type molecular sieve was mixed and slurried with ammonia nitrogen wastewater (exchange filtrate mixed liquid A in Comparative Example 1), and the mass of the exchange filtrate mixed liquid A was 5 times that of the molecular sieve to prepare a two-cross-baked Y-type molecular sieve slurry. The obtained two-cross-baked Y-type ultra-stable molecular sieve slurry was heated to 70° C. and stirred for 1 h, and poured into a Buchner funnel on the NaY filter cake in step 1), and the filter bottle was vacuumed to 0.07 MPa at the same time, and a two-cross-baked ultra-stable Y-type molecular sieve filter cake with a thickness of 10 mm was formed on the filter cloth.

[0103] 3) When there is no liquid on the surface of the filter cake, immediately add a 90°C ammonium chloride solution at a speed that ensures that no cracks are formed on the surface of the filter cake. The amount of ammonium chloride is such that the weight ratio of ammonium chloride to the composite molecular sieve is 0.10. When there is no liquid on the surface of the filter cake, immediately add deionized water at 80°C to wash the filter cake. The weight ratio of deionized water to the molecular sieve is 5. Then remove the molecular sieve filter cake and collect the filtrate D.

[0104] 4) adding kaolin, aluminum sol and yttrium oxide to the molecular sieve slurry obtained in step (3) in a ratio of molecular sieve: kaolin: aluminum sol (calculated as aluminum oxide): yttrium oxide = 35:54:10:1 to prepare a catalyst mixed slurry;

[0105] 5) The slurry obtained in step (4) is spray-dried to prepare catalyst microspheres according to a conventional spray-drying molding method for preparing catalytic cracking catalysts, and then calcined and solidified.

[0106] 6) Catalyst washing: The catalyst microspheres solidified in step 5) were mixed with water to prepare a slurry having a catalyst microsphere content of 110 g / L. The obtained slurry was heated to 60° C. and poured into a Buchner funnel. The filter bottle was evacuated to 0.06 MPa to form a filter cake with a thickness of 10 mm on the filter cloth.

[0107] 7) When there is no liquid on the surface of the filter cake in step 6), immediately add a solution containing ammonium chloride at a temperature of 90°C, and the amount of ammonium chloride is such that the weight ratio of ammonium chloride to microspheres is 0.08. When there is no liquid on the surface of the filter cake, immediately add deionized water at a temperature of 90°C to wash the filter cake, and the weight ratio of deionized water to microspheres is 5. Then remove the filter cake and collect the filtrate E. The filter cake is dried to obtain a catalyst sample S1, whose sodium oxide content is 0.09%, and the ammonia nitrogen content of the filtrate D is 8ppm.

[0108] Example 2

[0109] The operation steps are the same as those in Example 1, except that:

[0110] Step 1) The NaY molecular sieve slurry content is 300 g / L, the weight ratio of humic acid added to NaY molecular sieve dry basis is 0.001:1, the slurry temperature is 15° C., the vacuum degree of the filter bottle is 0.08 MPa, and the filter cake thickness is 5 mm.

[0111] Step 2) The cross-baked ultra-stable Y-type molecular sieve is mixed with ammonia nitrogen wastewater (filtrate E) and slurried. The amount of filtrate E is twice that of the molecular sieve. The slurry temperature is 50° C., stirred for 2 hours, the vacuum degree of the filter bottle is 0.08 MPa, and the filter cake thickness is 15 mm.

[0112] Step 3) The weight ratio of lanthanum chloride (calculated as rare earth oxide) to the composite molecular sieve is 0.10. The temperature of deionized water is 100° C., and the weight ratio of deionized water to the molecular sieve is 1. Remove the molecular sieve filter cake and collect the filtrate F.

[0113] Step 4) Molecular sieve: halloysite: silica sol (calculated as silicon dioxide): magnesium oxide = 35:54:10:1.

[0114] Step 5) spray drying and curing.

[0115] Step 6) The catalyst microsphere content is 300 g / L, the slurry temperature is 80° C., the filter flask vacuum is 0.02 MPa, and the filter cake thickness is 5 mm.

[0116] Step 7) The weight ratio of ammonium oxalate to catalyst is 0.10, the temperature of deionized water is 20°C, and the weight ratio of deionized water to catalyst microspheres is 10. Then the filter cake is removed and the filtrate I is collected to obtain a catalyst sample S2, which has a sodium oxide content of 1.1% and a filtrate F ammonia nitrogen content of 6 ppm.

[0117] Example 3

[0118] The operation steps are the same as those in Example 1, except that:

[0119] Step 1) The content of NaY molecular sieve slurry is 100 g / L, the weight ratio of humic acid added to NaY molecular sieve dry basis is 0.05:1, the slurry temperature is 100° C., the vacuum degree of the filter bottle is 0.02 MPa, and the filter cake thickness is 15 mm.

[0120] Step 2) The double cross-baked rare earth Y molecular sieve is mixed with ammonia nitrogen wastewater (filtrate I) and slurried, the amount of filtrate I is 10 times that of the molecular sieve, the slurry temperature is 100°C, stirring is performed for 0.5h, the vacuum degree of the filter bottle is 0.02 MPa, and the filter cake thickness is 5 mm.

[0121] Step 3) The temperature is 20° C., and the weight ratio of ammonium phosphate to molecular sieve is 0.20. The temperature of deionized water is 20° C., and the weight ratio of deionized water to molecular sieve is 3. Remove the molecular sieve filter cake and collect the filtrate J.

[0122] Step 4) Molecular sieve: montmorillonite: pseudo-boehmite (calculated as alumina): white carbon = 35:54:10:1.

[0123] Step 5) spray drying and curing.

[0124] Step 6) The catalyst microsphere content is 100 g / L, the slurry temperature is 20° C., the filter flask vacuum is 0.08 MPa, and the filter cake thickness is 20 mm.

[0125] Step 7) The weight ratio of ammonium sulfate to catalyst is 0.005, the temperature of deionized water is 100°C, and the weight ratio of deionized water to catalyst microspheres is 7. Then the filter cake is removed and the filtrate K is collected to obtain a catalyst sample S3, whose sodium oxide content is 1.0%, and the ammonia nitrogen content of the filtrate J is 4 ppm.

[0126] Example 4

[0127] The operation steps are the same as those in Example 1, except that:

[0128] Step 1) The NaY molecular sieve slurry content is 180 g / L, the weight ratio of humic acid and fulvic acid added to the NaY molecular sieve dry basis is 0.05:1 respectively, the slurry temperature is 75° C., the vacuum degree of the filter bottle is 0.04 MPa, and the filter cake thickness is 8 mm.

[0129] Step 2) (two cross-linked and one hydrogenated Y molecular sieve + one cross-linked and one hydrogenated Y molecular sieve) was mixed with ammonia nitrogen wastewater (filtrate K) and slurried. The amount of filtrate K was 4 times that of the molecular sieve. The slurry temperature was 70° C. and stirred for 1.5 h. The vacuum degree of the filter bottle was 0.04 MPa and the filter cake thickness was 13 mm.

[0130] Step 3) The weight ratio of cerium nitrate (calculated as rare earth oxide) to molecular sieve is 0.05, the temperature of deionized water is 40° C., and the weight ratio of deionized water to molecular sieve is 8. Remove the molecular sieve filter cake and collect the filtrate L.

[0131] Step 4) Molecular sieve: kaolin: aluminum sol (calculated as alumina): yttrium oxide = 35:54:10:1.

[0132] Step 5) spray drying and curing.

[0133] Step 6) The catalyst microsphere content is 170 g / L, the slurry temperature is 60° C., the filter flask vacuum is 0.04 MPa, and the filter cake thickness is 18 mm.

[0134] Step 7) The weight ratio of (ammonium oxalate + ammonium bicarbonate) to the catalyst is 0.08. The temperature of deionized water is 60°C, and the weight ratio of deionized water to molecular sieve is 9. The filter cake is dried at 200°C and then calcined at 500°C for 1h, then the filter cake is removed and the filtrate M is collected to obtain a catalyst sample S4 having a sodium oxide content of 1.2% and an ammonia nitrogen content of 4ppm in the filtrate L.

[0135] It can be seen from the results of Examples S1 to S4 that the ammonia nitrogen content of the filtrate obtained by the method of the present invention is less than 15ppm, which meets the national first-level emission standards. Compared with Comparative Example 1, the operation process of the present invention is simple and the direct discharge of ammonia nitrogen wastewater can be directly realized on the existing catalyst preparation device. In Comparative Example 1, the wastewater generated by the molecular sieve synthesis and exchange process is used as the spray washing liquid of the catalyst spray granulation tail gas spray washing tower, and the ammonia nitrogen in the spray washing liquid is stripped and absorbed by the ammonia absorption tower to obtain a spray recovery liquid with low ammonia nitrogen content. It is stirred into gel with acidified aluminum salt or acid solution, filtered, and the filtrate is discharged; the ammonia absorption tower absorption liquid is used as a molecular sieve exchange liquid or ingredient, and the operation is cumbersome, and the ammonia nitrogen wastewater is still higher than the national first-level emission standard, and it cannot meet the direct discharge requirements. Compared with Comparative Example 2, the method of the present invention takes into account the feasibility of ammonia nitrogen wastewater treatment and production. Comparative Example 2 needs to be exchanged at a temperature of 0-5°C, the operating conditions are harsh, and the industrial operation is difficult, which cannot meet the actual production needs. The catalytic cracking catalyst filtrate prepared by the method provided by the present invention has low ammonia nitrogen content, does not need to be treated with ammonia nitrogen, can meet the direct discharge requirements, has good operability, and has a good industrial application prospect.

[0136] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a catalytic cracking catalyst, characterized in that: The following steps are involved: 1) Slurrying NaY molecular sieve, humic acid and water, filtering to form a NaY molecular sieve filter cake layer, wherein the dry weight ratio of humic acid to NaY molecular sieve is 0.001-0.05; 2) Slurrying the Y-type molecular sieve and ammonia nitrogen wastewater to obtain a Y-type molecular sieve slurry, filtering the Y-type molecular sieve slurry through a NaY molecular sieve filter cake layer to obtain a composite filter cake layer, and then exchanging ions through a first ammonium salt exchange solution and / or a rare earth exchange solution, and washing with water to obtain a composite molecular sieve filter cake; the Y-type molecular sieve is a cross-linked and baked Y-type molecular sieve and / or a double cross-linked and baked Y-type molecular sieve, and the weight ratio of the ammonium salt in the first ammonium salt exchange solution to the total amount of the NaY molecular sieve dry basis and the Y-type molecular sieve dry basis is 0-0.2; the weight ratio of the rare earth in the rare earth exchange solution in terms of rare earth oxide to the total amount of the NaY molecular sieve dry basis and the Y-type molecular sieve dry basis is 0-0.10; 3) Mixing the composite molecular sieve filter cake, inorganic oxide, clay, binder and water for slurrying, spray drying for forming, calcining for solidification to obtain catalyst microspheres, mixing the catalyst microspheres with water for slurrying, filtering, performing ion exchange with a second ammonium salt exchange solution, washing with water, and drying to obtain a catalytic cracking catalyst; wherein the weight ratio of the ammonium salt in the second ammonium salt exchange solution to the catalyst microspheres on a dry basis is 0.005-0.

10.

2. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: The sodium oxide content of the NaY molecular sieve is 9-15%.

3. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: The humic acid is one or more of fulvic acid, palmitic acid and humic acid.

4. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: The ammonium salt is one or more of ammonium chloride, ammonium sulfate, ammonium oxalate, ammonium phosphate and ammonium bicarbonate, preferably ammonium chloride and / or ammonium sulfate.

5. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: The rare earth is rare earth nitrate and / or chloride, and the rare earth is one or more of lanthanum, cerium, praseodymium, neodymium and yttrium.

6. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: The cross-pyratory Y type molecular sieve is one or more of a cross-pyratory ultra-stable Y molecular sieve, a cross-pyratory rare earth Y molecular sieve, a cross-pyratory rare earth hydrogen Y molecular sieve and a cross-pyratory hydrogen Y molecular sieve; the double cross-pyratory Y type molecular sieve is one or more of a double cross-pyratory ultra-stable Y molecular sieve, a double cross-pyratory rare earth Y molecular sieve, a double cross-pyratory rare earth hydrogen Y molecular sieve and a double cross-pyratory hydrogen Y molecular sieve.

7. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: The inorganic oxide is one or more of rare earth oxide, magnesium oxide and silicon oxide; the clay is one or more of kaolin, halloysite and montmorillonite; the binder is one or more of aluminum sol, silica sol and pseudo-boehmite.

8. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: The ammonia nitrogen wastewater in step 2) is the filtrate collected during the ion exchange process in step 2) and / or the filtrate collected during the ion exchange process in step 3).

9. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: In step 2), the mass ratio of ammonia nitrogen wastewater to Y-type molecular sieve is 2-10, preferably 3-6.

10. The method for preparing a catalytic cracking catalyst according to claim 1, characterized in that: Step 1) and step 2) are performed on a first horizontal belt filter, wherein the first horizontal bag filter comprises a NaY molecular sieve filter cake layer forming zone, a composite filter cake layer forming zone, an ion exchange zone and a water washing zone connected in series; and step 3) is performed on a second horizontal belt filter, wherein the second horizontal belt filter comprises a filter cake forming zone, an ion exchange zone and a water washing zone connected in series.

Citation Information

Patent Citations

  • Method for reducing ammonia nitrogen in industrial wastewater

    CN101519232A

  • Cleaner production process for molecular sieve catalytic cracking catalyst

    CN103028431A

  • Catalytic cracking catalyst for efficient conversion of heavy oil, and preparation method thereof

    CN103447063A

  • Preparation method of catalytic cracking catalyst

    CN106732745A

  • Ammonium ion exchange method of molecular sieve

    CN1448339A