Method for preparing sustainable aviation fuel based on biomass

Through the combined technology of modified molecular sieves and Co-Cu catalysts, the efficiency of converting biomass straw into ethanol is improved, the problem of low ethanol yield in the existing technology is solved, and more efficient ethanol production is achieved.

CN118767973AInactive Publication Date: 2024-10-15HENAN JUNHENG IND GRP BIOTECH CO LTD

Patent Information

Application Number
CN202410849095.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing process of producing aviation fuel from biomass straw, the ethanol yield is low, which leads to the need for further optimization of the efficiency and economic feasibility of the entire process.

Method used

Using a combination of modified molecular sieve catalyst and Co-Cu catalyst, the efficiency of converting syngas into ethanol is improved through the two-stage catalytic reaction of the modified molecular sieve catalyst at 200-240°C and the Co-Cu catalyst at 240-280°C. The modified molecular sieve catalyst is modified by template agents and Zn ions to form a special pore structure, and the Co-Cu catalyst provides a variety of active sites to promote the formation of C-C bonds.

Benefits of technology

It significantly improves the selectivity and yield of ethanol, optimizes the reaction path, reduces side reactions, improves the stability and durability of the overall catalytic system, and increases the yield of ethanol.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767973A_ABST
    Figure CN118767973A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing sustainable aviation fuel based on biomass, and belongs to the technical field of aviation fuel, the method comprises the following steps: firstly preparing biomass straw into synthesis gas, then preparing the synthesis gas into ethanol, then preparing the ethanol into ethylene, and finally preparing the ethylene into the aviation fuel. The method for preparing the ethanol from the synthesis gas comprises the following specific operation steps: S1, introducing the synthesis gas and dimethyl ether into a fixed bed reactor, and carrying out a catalytic reaction under the conditions of 200-240 DEG C and 2-10 MPa through a modified molecular sieve catalyst to obtain a first-grade product; in the synthesis gas, the volume ratio of CO to H2 is (1-5): 2; s2, enabling the primary product obtained in the step S1 to flow to a bimetallic catalyst, and performing catalytic reaction under the conditions of 240-280 DEG C and 8-15 MPa to obtain a secondary product; and S3, separating the secondary product obtained in S2 to obtain ethanol. According to the method, the ethanol yield in the step of preparing the ethanol from the synthesis gas can be remarkably improved in the process of preparing the aviation fuel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of aviation fuel, and in particular relates to a method for preparing sustainable aviation fuel based on biomass. Background Art

[0002] As a renewable resource, biomass straw is particularly important in the context of environmental protection and sustainable development. This technology can not only reduce dependence on fossil fuels and reduce carbon emissions, but also effectively utilize agricultural waste, with significant environmental and economic benefits.

[0003] There is a process flow for preparing aviation fuel from biomass straw, which is divided into four steps, namely: biomass straw is made into synthesis gas, synthesis gas is made into ethanol, ethanol is made into ethylene, and ethylene is made into aviation fuel. Among them, this step involves converting biomass into synthesis gas rich in carbon monoxide (CO), carbon dioxide (CO2) and hydrogen (H2) through gasification reaction; this technology has been widely studied and has mature application examples. The second step is that the conversion of synthesis gas into ethanol can be carried out by microbial fermentation or chemical catalysis. The third step is that ethanol can be dehydrated to produce ethylene, which is a relatively mature chemical process. The fourth step is that ethylene can be further converted into different types of liquid hydrocarbons, including alkanes that can be used for aviation fuel, through chemical reactions such as polymerization and hydrogenation; this process has a wide range of applications in the field of petrochemicals and the technology is relatively mature.

[0004] Although the above-mentioned entire process of converting biomass straw into aviation fuel is feasible in the existing technology, and some links have mature technical support, the efficiency, cost and economic feasibility of the entire process still need further optimization and empirical research. In particular, in the second step, in the process of generating ethanol from syngas, improving the ethanol yield is still the current research focus. Summary of the invention

[0005] In order to solve the problems existing in the background technology, the present invention provides a method for preparing sustainable aviation fuel based on biomass, which can significantly improve the ethanol yield during the preparation process.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing sustainable aviation fuel based on biomass, firstly, biomass straw is made into synthesis gas, then the synthesis gas is made into ethanol, then the ethanol is made into ethylene, and finally the ethylene is made into aviation fuel. The specific operation steps of synthesizing ethanol from synthesis gas are as follows:

[0008] S1, introducing synthesis gas and dimethyl ether into a fixed bed reactor, passing through a modified molecular sieve catalyst, and performing a catalytic reaction at 200-240° C. and 2-10 MPa to obtain a primary product; in the synthesis gas, the volume ratio of CO to H2 is (1-5):2;

[0009] S2, allowing the primary product obtained in S1 to flow to a bimetallic catalyst for catalytic reaction at 240-280°C and 8-15MPa to obtain a secondary product;

[0010] S3. Separate the secondary product obtained in S2 to obtain ethanol.

[0011] Further, in S1, the preparation method of the modified molecular sieve catalyst is as follows:

[0012] A1. Dissolve 21.6 g of NaOH in 640 mL of deionized water in a beaker, add 18.4 g of NaA1O2, slowly drop 544 g of 30 wt% silica sol aqueous solution while stirring, stir for 4 h, then add 1-1.5 g of mercerized molecular sieve powder and 1-1.2 g of template, continue stirring for 1 h to obtain a mixed solution;

[0013] A2, transfer the mixed solution obtained in A1 to a reaction kettle, heat to 145-155°C, keep warm for 3 days and then cool naturally, filter and wash the product until pH <9, dry at 100±2°C for 12h, heat to 545-555°C at a heating rate of 5°C / min, and calcine for 30-50min to obtain a solid product;

[0014] A3, pour the solid product obtained in A2 into NH4Cl solution, perform ion exchange, filter, perform ion exchange again, filter until the pH of the filtrate is ≈ 7, filter out the solid, and then calcine in a muffle furnace at 495-505°C to obtain hydrogen-type mordenite;

[0015] A4, put the hydrogen-type mordenite obtained in A3 into an ammonium fluorosilicate solution, stir at room temperature for 4 hours, filter and wash until the pH is neutral, dry and calcine to obtain a molecular sieve modification;

[0016] A5. Place the modified molecular sieve obtained in A4 into a 0.2 mol / L zinc nitrate solution at 60±2°C. 2+ After exchange, filtration and drying, the mixture is calcined at 495-505°C for 4 hours, pressed into tablets, and then adsorbed with pyridine for 12 hours to obtain a modified molecular sieve catalyst.

[0017] Furthermore, in A2, the reactor is a polytetrafluoroethylene-lined reactor.

[0018] Furthermore, in A3, the concentration of the NH4Cl solution is 0.1 mol / L, and the usage ratio of the solid product to the NH4Cl solution is 1 g:50 mL.

[0019] Furthermore, in A4, the concentration of the ammonium fluorosilicate solution is 0.2 mol / L, and the usage ratio of the hydrogen-type mordenite to the ammonium fluorosilicate solution is 1 g:50 mL.

[0020] Furthermore, in A4, the drying temperature is 100±2°C, and the drying time is 5-8h; the roasting temperature is 450-480°C, and the roasting time is 30-40min.

[0021] Furthermore, in S2, the bimetallic catalyst is a Co-Cu catalyst.

[0022] Furthermore, the preparation method of the Co-Cu catalyst is as follows:

[0023] B1. Dissolve 10g of Na2C2O4 in 350mL of deionized water, add 4.4g of copper nitrate trihydrate, stir until a dark blue transparent solution is obtained, seal and let stand at low temperature for 12h, wait until crystals are completely precipitated, filter, rinse with anhydrous ethanol, and dry in an oven at 50°C for 6h to obtain crystals;

[0024] B2, 3.0192g of cobalt nitrate hexahydrate, 12.6928g of zinc nitrate hexahydrate and 8.0028g of aluminum nitrate nonahydrate were dissolved in 200ml of deionized water to obtain a mixed salt solution a, 3.6259g of NaNO3 and 5.3764g of NaOH were dissolved in 200ml of deionized water to obtain a mixed salt solution b, the mixed salt solution a and the mixed salt solution b were vigorously stirred in a three-necked flask to obtain a pink slurry-like precipitate, and after continuing to vigorously stir for 5min, the temperature was raised to 100°C, and slowly stirred for crystallization for 12h, and after deionized water suction filtration and washing, it was washed with ethanol, and then placed in a 60°C vacuum oven to dry overnight, and ground to obtain a powder;

[0025] B3. Take the crystals obtained in B1 and the powder obtained in B2, mix them, prepare a 0.015 mol / L aqueous solution, add hydrotalcite powder, stir at room temperature for 12 h, filter and wash, vacuum dry at 60°C for 12 h, and grind to obtain a Co-Cu catalyst.

[0026] Furthermore, in B3, the crystals obtained in B1 and the powder obtained in B2 are mixed at a Co / Cu molar ratio of (1-2):1.

[0027] This application has the following beneficial effects:

[0028] 1. In the preparation of modified molecular sieve catalysts, the addition of templates helps to form a specific pore structure in the molecular sieve, thereby enhancing the selectivity and yield of the target product ethanol; by converting Na-type mordenite into hydrogen-type mordenite, the number and strength of the acid sites of the catalyst can be increased, thereby improving the catalytic activity and ethanol yield; the introduction of Zn ions can improve the ethanol selectivity by changing the acidity and adsorption properties of the molecular sieve; ammonium fluorosilicate, as a strong acid, can react with aluminum in the molecular sieve to form a soluble aluminum-fluorine complex, thereby achieving a dealumination effect, reducing the non-framework aluminum content in the molecular sieve, and increasing its hydrophobicity and stability, which is beneficial for the synthesis gas to ethanol reaction, because higher hydrophobicity helps the selectivity and yield of ethanol; in the dealumination process, fluoride ions can form stronger bonds with silicon in the molecular sieve, which helps to maintain the crystallinity and stability of the molecular sieve; dealumination will also change the pore size and pore volume of the molecular sieve, which helps to adjust the adsorption performance and catalytic activity of the molecular sieve, and a more suitable pore structure can provide a more effective reaction path, promote ethanol formation, and increase ethanol yield.

[0029] 2. In the preparation of Co-Cu catalyst, the presence of cobalt and copper provides different types of active sites. Cobalt can promote the activation and chain growth reaction of CO, while copper helps the hydrogenation reaction. This complementarity makes the entire reaction process more efficient. The electronic interaction between cobalt and copper can modulate the electronic properties of the catalyst surface, thereby affecting the adsorption and conversion of reaction intermediates and improving the selectivity of ethanol. The addition of hydrotalcite powder enhances the catalyst's adsorption capacity for CO by providing surface alkaline sites, promotes the formation of CC bonds, and thus increases the ethanol yield.

[0030] 3. The modified molecular sieve catalyst and the Co-Cu catalyst play a role in different reaction paths. The former provides active sites in the initial stage of syngas conversion, while the latter may play a leading role in the subsequent CC bond formation and chain growth process. This graded catalysis helps to optimize the entire syngas-to-ethanol reaction path, reduce side reactions, and improve the selectivity and yield of ethanol. Moreover, the addition of the Co-Cu catalyst may also help to improve the stability and durability of the overall catalytic system and resist aging and poisoning that may occur during the reaction. Experimental verification shows that the modified molecular sieve catalyst and the Co-Cu catalyst jointly promote the reaction process of syngas-to-ethanol and synergistically improve the ethanol yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a comparative trend chart of ethanol yields from synthesis gas in Examples 1-5 of the present invention and Comparative Examples 1-4. DETAILED DESCRIPTION

[0032] The present application is further described in detail below with reference to the embodiments.

[0033] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.

[0034] Example 1: A method for preparing sustainable aviation fuel based on biomass, firstly, biomass straw is made into synthesis gas, then the synthesis gas is made into ethanol, then the ethanol is made into ethylene, and finally the ethylene is made into aviation fuel. The specific operation steps of synthesizing ethanol from synthesis gas are as follows:

[0035] S1. Synthesis gas and dimethyl ether are introduced into a fixed bed reactor, and a catalytic reaction is carried out at 220°C and 6MPa over a modified molecular sieve catalyst to obtain a primary product; in the synthesis gas, the volume ratio of CO to H2 is 1:1.

[0036] Wherein, the preparation method of the modified molecular sieve catalyst is as follows:

[0037] A1. Dissolve 21.6g of NaOH in 640mL of deionized water in a beaker, then add 18.4g of NaA1O2, slowly drop 544g of 30wt% silica sol aqueous solution while stirring, stir for 4h, then add 1.2g of mercerized molecular sieve powder and 1.1g of template agent, continue stirring for 1h to obtain a mixed solution. Mercerized molecular sieve powder was purchased from Jiangxi Xintao Technology Co., Ltd. The template agent is tetraethylammonium hydroxide.

[0038] A2, transfer the mixed solution obtained in A1 to a polytetrafluoroethylene-lined reactor, heat to 150°C, keep warm for 3 days and then cool naturally, filter and wash the product until pH <9, dry at 100±2°C for 12h, heat to 550°C at a heating rate of 5°C / min, and calcine for 40min to obtain a solid product.

[0039] A3. Pour the solid product obtained in A2 into an aqueous solution of NH4Cl with a concentration of 0.1 mol / L, with the ratio of the solid product to the NH4Cl solution being 1 g:50 mL, and perform ion exchange. After filtration, perform ion exchange again, and filter until the pH of the filtrate is ≈ 7 to filter out the solid, which is then calcined at 500°C in a muffle furnace to obtain hydrogen-type mordenite.

[0040] A4. The hydrogen-type mordenite obtained in A3 was added to a 0.2 mol / L ammonium fluorosilicate solution in a ratio of 1 g to 50 mL. The mixture was stirred at room temperature for 4 h, filtered and washed until the pH was neutral, dried at 100°C for 6 h, and calcined at 460°C for 35 min to obtain a modified molecular sieve.

[0041] A5. Place the modified molecular sieve obtained in A4 into a 0.2 mol / L zinc nitrate solution at 60°C. 2+After exchange, filtration and drying, the mixture was calcined at 500°C for 4 hours, pressed into tablets and passed through a 30-40 mesh sieve, and then adsorbed with pyridine for 12 hours to obtain a modified molecular sieve catalyst.

[0042] S2, the primary product obtained in S1 flows to the bimetallic catalyst, and the catalytic reaction is carried out at 260°C and 12MPa to obtain the secondary product. The fixed bed reactor containing the modified molecular sieve catalyst and the fixed bed reactor containing the bimetallic catalyst are connected in series.

[0043] Wherein, the bimetallic catalyst is a Co-Cu catalyst, and the preparation method of the Co-Cu catalyst is as follows:

[0044] B1. Dissolve 10g of Na2C2O4 in 350mL of deionized water, add 4.4g of copper nitrate trihydrate, stir until a dark blue transparent solution is obtained, seal and let stand at low temperature for 12h, wait until crystals are completely precipitated, filter, rinse with anhydrous ethanol, and dry in an oven at 50°C for 6h to obtain crystals;

[0045] B2, 3.02g of cobalt nitrate hexahydrate, 12.69g of zinc nitrate hexahydrate and 8.00g of aluminum nitrate nonahydrate were dissolved in 200ml of deionized water to obtain a mixed salt solution a, 3.63g of NaNO3 and 5.38g of NaOH were dissolved in 200ml of deionized water to obtain a mixed salt solution b, the mixed salt solution a and the mixed salt solution b were vigorously stirred in a three-necked flask to obtain a pink slurry-like precipitate, and after continuing to vigorously stir for 5min, the temperature was raised to 100°C, and slowly stirred for crystallization for 12h, and after deionized water suction filtration and washing, it was washed with ethanol, and then placed in a 60°C vacuum oven to dry overnight, and ground to obtain a powder;

[0046] B3. Take the crystals obtained in B1 and the powder obtained in B2, mix them according to the Co / Cu molar ratio of 1.5:1 to prepare a 0.015 mol / L mixed aqueous solution, add hydrotalcite powder, the amount of hydrotalcite powder added is 0.5% of the mixed aqueous solution, stir at room temperature for 12 hours, filter and wash, vacuum dry at 60°C for 12 hours, grind, and obtain a Co-Cu catalyst.

[0047] S3. Separate the secondary product obtained in S2 to obtain ethanol.

[0048] Example 2: The difference between this example and Example 1 is that in the preparation of the modified molecular sieve catalyst, the amounts of mercerized molecular sieve powder and template agent used are different: 1 g of mercerized molecular sieve powder and 1 g of template agent.

[0049] Specifically, the preparation method of the modified molecular sieve catalyst is as follows:

[0050] A1. Dissolve 21.6 g of NaOH in 640 mL of deionized water in a beaker, then add 18.4 g of NaA1O2, slowly drop 544 g of 30 wt% silica sol aqueous solution while stirring, stir for 4 h, then add 1 g of mercerized molecular sieve powder and 1 g of template, continue stirring for 1 h to obtain a mixed solution.

[0051] A2, transfer the mixed solution obtained in A1 to a polytetrafluoroethylene-lined reactor, heat to 150°C, keep warm for 3 days and then cool naturally, filter and wash the product until pH <9, dry at 100±2°C for 12h, heat to 550°C at a heating rate of 5°C / min, and calcine for 40min to obtain a solid product.

[0052] A3. Pour the solid product obtained in A2 into an aqueous solution of NH4Cl with a concentration of 0.1 mol / L, with the ratio of the solid product to the NH4Cl solution being 1 g:50 mL, and perform ion exchange. After filtration, perform ion exchange again, and filter until the pH of the filtrate is ≈ 7 to filter out the solid, which is then calcined at 500°C in a muffle furnace to obtain hydrogen-type mordenite.

[0053] A4. The hydrogen-type mordenite obtained in A3 was added to a 0.2 mol / L ammonium fluorosilicate solution in a ratio of 1 g to 50 mL. The mixture was stirred at room temperature for 4 h, filtered and washed until the pH was neutral, dried at 100°C for 6 h, and calcined at 460°C for 35 min to obtain a modified molecular sieve.

[0054] A5. Place the modified molecular sieve obtained in A4 into a 0.2 mol / L zinc nitrate solution at 60°C. 2+ After exchange, filtration and drying, the mixture was calcined at 500°C for 4 hours, pressed into tablets and passed through a 30-40 mesh sieve, and then adsorbed with pyridine for 12 hours to obtain a modified molecular sieve catalyst.

[0055] Example 3: The only difference between this example and Example 1 is that in the preparation of the modified molecular sieve catalyst, the amounts of mercerized molecular sieve powder and template agent used are different: 1.5 g of mercerized molecular sieve powder and 1.2 g of template agent.

[0056] Specifically, the preparation method of the modified molecular sieve catalyst is as follows:

[0057] A1. Dissolve 21.6 g of NaOH in 640 mL of deionized water in a beaker, then add 18.4 g of NaA1O2, slowly drop 544 g of 30 wt% silica sol aqueous solution while stirring, stir for 4 h, then add 1.5 g of mercerized molecular sieve powder and 1.2 g of template, continue stirring for 1 h to obtain a mixed solution.

[0058] A2. Transfer the mixed solution obtained in A1 to a polytetrafluoroethylene-lined reactor, heat to 150°C, keep warm for 3 days and then cool naturally. Filter and wash the product until pH <9, dry it at 100±2°C for 12h, heat it to 550°C at a heating rate of 5°C / min, and calcine it for 40min to obtain a solid product.

[0059] A3. Pour the solid product obtained in A2 into an aqueous solution of NH4Cl with a concentration of 0.1 mol / L, with the ratio of the solid product to the NH4Cl solution being 1 g:50 mL, and perform ion exchange. After filtration, perform ion exchange again, and filter until the pH of the filtrate is ≈ 7 to filter out the solid, which is then calcined at 500°C in a muffle furnace to obtain hydrogen-type mordenite.

[0060] A4. The hydrogen-type mordenite obtained in A3 was added to a 0.2 mol / L ammonium fluorosilicate solution in a ratio of 1 g to 50 mL. The mixture was stirred at room temperature for 4 h, filtered and washed until the pH was neutral, dried at 100°C for 6 h, and calcined at 460°C for 35 min to obtain a modified molecular sieve.

[0061] A5. Place the modified molecular sieve obtained in A4 into a 0.2 mol / L zinc nitrate solution at 60°C. 2+ After exchange, filtration and drying, the mixture was calcined at 500°C for 4 hours, pressed into tablets and passed through a 30-40 mesh sieve, and then adsorbed with pyridine for 12 hours to obtain a modified molecular sieve catalyst.

[0062] Example 4: The only difference between this example and Example 1 is that in the preparation of the Co-Cu catalyst, the molar ratio of Co / Cu is different: the molar ratio of Co / Cu is 1:1.

[0063] Specifically, the preparation method of the Co-Cu catalyst is as follows:

[0064] B1. Dissolve 10g of Na2C2O4 in 350mL of deionized water, add 4.4g of copper nitrate trihydrate, stir until a dark blue transparent solution is obtained, seal and let stand at low temperature for 12h, wait until crystals are completely precipitated, filter, rinse with anhydrous ethanol, and dry in an oven at 50°C for 6h to obtain crystals;

[0065] B2, 3.02g of cobalt nitrate hexahydrate, 12.69g of zinc nitrate hexahydrate and 8.00g of aluminum nitrate nonahydrate were dissolved in 200ml of deionized water to obtain a mixed salt solution a, 3.63g of NaNO3 and 5.38g of NaOH were dissolved in 200ml of deionized water to obtain a mixed salt solution b, the mixed salt solution a and the mixed salt solution b were vigorously stirred in a three-necked flask to obtain a pink slurry-like precipitate, and after continuing to vigorously stir for 5min, the temperature was raised to 100°C, and slowly stirred for crystallization for 12h, and after deionized water suction filtration and washing, it was washed with ethanol, and then placed in a 60°C vacuum oven to dry overnight, and ground to obtain a powder;

[0066] B3. Take the crystals obtained in B1 and the powder obtained in B2, mix them in a Co / Cu molar ratio of 1:1 to prepare a 0.015 mol / L mixed aqueous solution, add hydrotalcite powder, the amount of hydrotalcite powder added is 0.5% of the mixed aqueous solution, stir at room temperature for 12 h, filter and wash, vacuum dry at 60°C for 12 h, and grind to obtain a Co-Cu catalyst.

[0067] Example 5: The only difference between this example and Example 1 is that in the preparation of the Co-Cu catalyst, the molar ratio of Co / Cu is different: the molar ratio of Co / Cu is 2:1.

[0068] Specifically, the preparation method of the Co-Cu catalyst is as follows:

[0069] B1. Dissolve 10g of Na2C2O4 in 350mL of deionized water, add 4.4g of copper nitrate trihydrate, stir until a dark blue transparent solution is obtained, seal and let stand at low temperature for 12h, wait until crystals are completely precipitated, filter, rinse with anhydrous ethanol, and dry in an oven at 50°C for 6h to obtain crystals;

[0070] B2, 3.02g of cobalt nitrate hexahydrate, 12.69g of zinc nitrate hexahydrate and 8.00g of aluminum nitrate nonahydrate were dissolved in 200ml of deionized water to obtain a mixed salt solution a, 3.63g of NaNO3 and 5.38g of NaOH were dissolved in 200ml of deionized water to obtain a mixed salt solution b, the mixed salt solution a and the mixed salt solution b were vigorously stirred in a three-necked flask to obtain a pink slurry-like precipitate, and after continuing to vigorously stir for 5min, the temperature was raised to 100°C, and slowly stirred for crystallization for 12h, and after deionized water suction filtration and washing, it was washed with ethanol, and then placed in a 60°C vacuum oven to dry overnight, and ground to obtain a powder;

[0071] B3. Take the crystals obtained in B1 and the powder obtained in B2, mix them in a Co / Cu molar ratio of 2:1 to prepare a 0.015 mol / L mixed aqueous solution, add hydrotalcite powder, the amount of hydrotalcite powder added is 0.5% of the mixed aqueous solution, stir at room temperature for 12 h, filter and wash, vacuum dry at 60°C for 12 h, and grind to obtain a Co-Cu catalyst.

[0072] Comparative Example 1: The difference between this comparative example and Example 1 is that the modification of ammonium fluorosilicate is deleted in the preparation of the modified molecular sieve catalyst.

[0073] Specifically, the preparation method of the modified molecular sieve catalyst is as follows:

[0074] A1. Dissolve 21.6g of NaOH in 640mL of deionized water in a beaker, then add 18.4g of NaA1O2, slowly drop 544g of 30wt% silica sol aqueous solution while stirring, stir for 4h, then add 1.2g of mercerized molecular sieve powder and 1.1g of template agent, continue stirring for 1h to obtain a mixed solution. Mercerized molecular sieve powder was purchased from Jiangxi Xintao Technology Co., Ltd. The template agent is tetraethylammonium hydroxide.

[0075] A2, transfer the mixed solution obtained in A1 to a polytetrafluoroethylene-lined reactor, heat to 150°C, keep warm for 3 days and then cool naturally, filter and wash the product until pH <9, dry at 100±2°C for 12h, heat to 550°C at a heating rate of 5°C / min, and calcine for 40min to obtain a solid product.

[0076] A3. Pour the solid product obtained in A2 into an aqueous solution of NH4Cl with a concentration of 0.1 mol / L, with the ratio of the solid product to the NH4Cl solution being 1 g:50 mL, and perform ion exchange. After filtration, perform ion exchange again, and filter until the pH of the filtrate is ≈ 7 to filter out the solid, which is then calcined at 500°C in a muffle furnace to obtain hydrogen-type mordenite.

[0077] A4. Place the hydrogen-type mordenite obtained in A3 into a 0.2 mol / L zinc nitrate solution at 60°C. 2+ After exchange, filtration and drying, the mixture was calcined at 500°C for 4 hours, pressed into tablets and passed through a 30-40 mesh sieve, and then adsorbed with pyridine for 12 hours to obtain a modified molecular sieve catalyst.

[0078] Comparative Example 2: The difference between this comparative example and Example 1 is that the bimetallic catalyst is replaced.

[0079] Specifically, the preparation method of the replaced metal catalyst is as follows: In a beaker, 96.80g of copper nitrate trihydrate, 15.60g of zinc nitrate hexahydrate and 14.71g of aluminum nitrate nonahydrate are dissolved in 2000ml of deionized water to obtain a mixed metal nitrate aqueous solution. In another beaker, 72.62g of concentrated ammonia water is diluted with 1500ml of deionized water, and the ammonia aqueous solution is vigorously stirred at room temperature, and then the obtained mixed metal nitrate aqueous solution is slowly added to the ammonia aqueous solution for about 60min. Filter to obtain a precipitate, and adjust the pH value of the precipitate to 10.0 with another ammonia aqueous solution. After continuing to stir for 200min, stand and age for 36h. Then, wash the precipitate with deionized water until neutral and centrifuge. The obtained precipitate is dried in a 120℃ oven for 24h. After drying, the sample is placed in a muffle furnace, heated to 400℃ at a heating rate of 1℃ / min, and roasted for 5h to obtain a roasted sample. Then, 1.4 g of manganese nitrate tetrahydrate and 1.4 g of nickel nitrate tetrahydrate were dissolved in 50 ml of deionized water, and the manganese and nickel aqueous solutions were loaded onto the calcined sample by impregnation, and the excess solvent was evaporated at 80°C. The sample was dried in an oven at 120°C for 24 hours, and after drying, the sample was placed in a muffle furnace, heated to 400°C at a heating rate of 1°C / min, and calcined for 3 hours to obtain the product.

[0080] Comparative Example 3: The difference between this comparative example and Example 1 is that the hydrotalcite powder is deleted in the preparation of the bimetallic catalyst.

[0081] Specifically, the bimetallic catalyst is a Co-Cu catalyst, and the preparation method of the Co-Cu catalyst is as follows:

[0082] B1. Dissolve 10g of Na2C2O4 in 350mL of deionized water, add 4.4g of copper nitrate trihydrate, stir until a dark blue transparent solution is obtained, seal and let stand at low temperature for 12h, wait until crystals are completely precipitated, filter, rinse with anhydrous ethanol, and dry in an oven at 50°C for 6h to obtain crystals;

[0083] B2, 3.02g of cobalt nitrate hexahydrate, 12.69g of zinc nitrate hexahydrate and 8.00g of aluminum nitrate nonahydrate were dissolved in 200ml of deionized water to obtain a mixed salt solution a, 3.63g of NaNO3 and 5.38g of NaOH were dissolved in 200ml of deionized water to obtain a mixed salt solution b, the mixed salt solution a and the mixed salt solution b were vigorously stirred in a three-necked flask to obtain a pink slurry-like precipitate, and after continuing to vigorously stir for 5min, the temperature was raised to 100°C, and slowly stirred for crystallization for 12h, and after deionized water suction filtration and washing, it was washed with ethanol, and then placed in a 60°C vacuum oven to dry overnight, and ground to obtain a powder;

[0084] B3. Take the crystals obtained in B1 and the powder obtained in B2, mix them in a Co / Cu molar ratio of 1.5:1 to prepare a 0.015 mol / L mixed aqueous solution, stir at room temperature for 12 h, filter and wash, vacuum dry at 60°C for 12 h, and grind to obtain a Co-Cu catalyst.

[0085] Comparative Example 4: The difference between this comparative example and Example 1 is that: in the preparation of the modified molecular sieve catalyst, the same changes as in Comparative Example 1 are made; and in the preparation of the bimetallic catalyst, the same changes as in Comparative Example 3 are made.

[0086] Test examples: Test objects: Examples 1-5 and Comparative Examples 1-4.

[0087] Test item: ethanol yield (based on modified molecular sieve catalyst).

[0088] Test results: See Table 1.

[0089] Table 1. Test example data

[0090] Ethanol yield / g / kgcat / h Example 1 378.5 Example 2 365.7 Example 3 364.7 Example 4 371.9 Example 5 373.4 Comparative Example 1 311.8 Comparative Example 2 345.2 Comparative Example 3 332.7 Comparative Example 4 298.4

[0091] Result analysis: Based on the data in Table 1 and the Figure 1 It can be seen that in the process of preparing ethanol from synthesis gas of the present invention, the ethanol yield is as high as 378.5 g / kgcat / h (based on the modified molecular sieve catalyst) and is stable. Figure 1 It can be seen that in the process of preparing ethanol from synthesis gas of the present invention, the modified molecular sieve catalyst and the Co-Cu catalyst prepared by the present invention are used, both of which can improve the ethanol yield, and the two catalysts work synergistically.

[0092] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0093] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing sustainable aviation fuel based on biomass, firstly converting biomass straw into synthesis gas, then converting the synthesis gas into ethanol, then converting the ethanol into ethylene, and finally converting the ethylene into aviation fuel, characterized in that: The specific steps of producing ethanol from syngas are as follows: S1, introducing synthesis gas and dimethyl ether into a fixed bed reactor, passing through a modified molecular sieve catalyst, and performing a catalytic reaction at 200-240° C. and 2-10 MPa to obtain a primary product; in the synthesis gas, the volume ratio of CO to H2 is (1-5):2; S2, allowing the primary product obtained in S1 to flow to a bimetallic catalyst for catalytic reaction at 240-280°C and 8-15MPa to obtain a secondary product; S3. Separate the secondary product obtained in S2 to obtain ethanol.

2. The method for preparing sustainable aviation fuel based on biomass according to claim 1, characterized in that: In S1, the preparation method of the modified molecular sieve catalyst is as follows: A1. Dissolve 21.6 g of NaOH in 640 mL of deionized water in a beaker, add 18.4 g of NaA1O2, slowly drop 544 g of 30 wt% silica sol aqueous solution while stirring, stir for 4 h, then add 1-1.5 g of mercerized molecular sieve powder and 1-1.2 g of template, continue stirring for 1 h to obtain a mixed solution; A2, transfer the mixed solution obtained in A1 to a reaction kettle, heat to 145-155°C, keep warm for 3 days and then cool naturally, filter and wash the product until pH <9, dry at 100±2°C for 12h, heat to 545-555°C at a heating rate of 5°C / min, and calcine for 30-50min to obtain a solid product; A3, pour the solid product obtained in A2 into NH4Cl solution, perform ion exchange, filter, perform ion exchange again, filter until the pH of the filtrate is ≈ 7, filter out the solid, and then calcine in a muffle furnace at 495-505°C to obtain hydrogen-type mordenite; A4, put the hydrogen-type mordenite obtained in A3 into an ammonium fluorosilicate solution, stir at room temperature for 4 hours, filter and wash until the pH is neutral, dry and calcine to obtain a molecular sieve modification; A5. Place the modified molecular sieve obtained in A4 into a 0.2 mol / L zinc nitrate solution at 60±2°C. 2+ After exchange, filtration and drying, the mixture is calcined at 495-505°C for 4 hours, pressed into tablets, and then adsorbed with pyridine for 12 hours to obtain a modified molecular sieve catalyst.

3. The method for preparing sustainable aviation fuel based on biomass according to claim 2, characterized in that: In A2, the reactor is a reactor lined with polytetrafluoroethylene.

4. The method for preparing sustainable aviation fuel based on biomass according to claim 2, characterized in that: In A3, the concentration of the NH4Cl solution is 0.1 mol / L, and the usage ratio of the solid product to the NH4Cl solution is 1 g:50 mL.

5. The method for preparing sustainable aviation fuel based on biomass according to claim 2, characterized in that: In A4, the concentration of the ammonium fluorosilicate solution is 0.2 mol / L, and the usage ratio of the hydrogen-type mordenite to the ammonium fluorosilicate solution is 1 g:50 mL.

6. The method for preparing sustainable aviation fuel based on biomass according to claim 2, characterized in that: In A4, the drying temperature is 100±2°C, and the drying time is 5-8h; the roasting temperature is 450-480°C, and the roasting time is 30-40min.

7. The method for preparing sustainable aviation fuel based on biomass according to claim 1, characterized in that: In S2, the bimetallic catalyst is a Co-Cu catalyst.

8. The method for preparing sustainable aviation fuel based on biomass according to claim 7, characterized in that: The preparation method of the Co-Cu catalyst is as follows: B1. Dissolve 20g of Na2C2O4 in 700mL of deionized water, add 8.8g of copper nitrate trihydrate, stir until a dark blue transparent solution is obtained, seal and let stand at low temperature for 12h, wait until crystals are completely precipitated, filter, rinse with anhydrous ethanol, and dry in an oven at 50°C for 6h to obtain crystals; B2, 6.04g of cobalt nitrate hexahydrate, 25.40g of zinc nitrate hexahydrate and 16.00g of aluminum nitrate nonahydrate were dissolved in 400ml of deionized water to obtain a mixed salt solution a, 7.25g of NaNO3 and 10.75g of NaOH were dissolved in 400ml of deionized water to obtain a mixed salt solution b, the mixed salt solution a and the mixed salt solution b were vigorously stirred in a three-necked flask to obtain a pink slurry-like precipitate, and after continuing to vigorously stir for 5min, the temperature was raised to 100°C, and slowly stirred for crystallization for 12h, after deionized water suction filtration and washing, washed with ethanol, and then placed in a 60°C vacuum oven to dry overnight, ground to obtain a powder; B3. Take the crystals obtained in B1 and the powder obtained in B2, mix them, prepare a 0.015 mol / L aqueous solution, add hydrotalcite powder, stir at room temperature for 12 h, filter and wash, vacuum dry at 60°C for 12 h, and grind to obtain a Co-Cu catalyst.

9. The method for preparing sustainable aviation fuel based on biomass according to claim 8, characterized in that: In B3, the crystals obtained in B1 and the powder obtained in B2 are mixed at a Co / Cu molar ratio of (1-2):1.

Citation Information

Patent Citations

  • Equally distributed CoCu catalyst for preparing ethyl alcohol and higher alcohol through synthesis gas

    CN105903472A

  • Method for producing zeolite

    CN113950460A

  • Method for co-producing methanol and ethanol from synthesis gas

    CN115557829A

  • Method of transforming biomass into hydrocarbon

    US9738909B1

Cited By

  • Method for producing sustainable aviation fuel by utilizing straws

    CN120624076A

  • A method for producing sustainable aviation fuel from straw

    CN120624076B