Preparation method of catalytic cracking propylene assistant
Through the pulping technology of Y-type molecular sieve and humic acid combined with the ion exchange of phosphorus-containing wastewater, an efficient catalytic cracking propylene additive is formed, which solves the problem of phosphorus pollution in the production of catalytic cracking additives and realizes the recycling and utilization of phosphorus elements and additives. green production.
Patent Information
- Application Number
- CN202310356712.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-04-04
AI Technical Summary
Phosphorus pollution in the production process of catalytic cracking propylene additives is serious, and existing technology is difficult to effectively recycle, resulting in high wastewater treatment costs and affecting production efficiency and the environment.
Use Y-type molecular sieve and humic acid to form a filter cake, combine it with phosphorus-containing wastewater for ion exchange to form a Z-Y composite filter cake, and then mix it with inorganic oxides, clay and binders to spray-dry and form. After multiple ion exchanges and washing Obtain catalytic cracking propylene additives to achieve efficient recycling of phosphorus.
It reduces water consumption and phosphorus exchange liquid consumption in the additive production process, reduces production costs, realizes direct discharge of wastewater, and ensures green production of additives that meets environmental protection standards.
Smart Images

Figure CN118767981A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of auxiliary agent preparation, and in particular to a method for preparing a catalytic cracking propylene auxiliary agent. Background Art
[0002] Propylene is an extremely important organic chemical raw material, mainly used to produce chemicals such as polypropylene, acrylonitrile, propylene oxide, acrylic acid, and cumene. With the rapid development of the petrochemical industry, the demand for propylene is growing, and currently my country's propylene is in short supply. There are many process schemes for producing propylene in the petrochemical process, such as the traditional naphtha steam cracking method, the metathesis reaction technology of ethylene and butene, butene disproportionation reaction (CN1618512A, CN1618515A), propane dehydrogenation technology (such as CN1073893A), methanol to propylene technology, and catalytic cracking technology. Comparative analysis shows that the production of propylene through the fluidized catalytic cracking (FCC) process has the significant characteristics of low investment, wide adaptability of raw materials, and low cost, and has attracted more and more attention (US5318696A, US5997728A, US5236880A, US5472594A, CN1465527A, CN1796496A, CN1854254A). In the catalytic cracking process, the method of adding a promoter to increase propylene production is widely used because of its advantages of simple operation, flexible reaction, and little impact on the entire process.
[0003] USP5,997,728 discloses a method for catalytic cracking of heavy raw materials using a catalytic cracking aid containing a selective zeolite. The aid is formed by adding 12 to 40 weight percent of ZSM-5 zeolite to an amorphous matrix, the stock in the catalytic cracking system is at least 10 weight percent, and the proportion of ZSM-5 in the catalyst is not less than 3 weight percent. This method can significantly increase the yield of light olefins.
[0004] CN111760588A discloses a propylene production increasing catalytic cracking additive, characterized in that the additive contains 10 to 60 weight percent of ZSM-5 molecular sieve, 5 to 30 weight percent of binder, and 0.5 to 5 weight percent of phosphorus-containing cationic compound (P 2 O 5 The additive is compounded with the catalytic cracking main catalyst to significantly increase the yield of liquefied gas and propylene in the catalytic cracking reaction.
[0005] CN102188992B discloses a catalytic cracking aid for increasing propylene production in a refinery FCC unit and a preparation method thereof. The catalytic cracking aid comprises 20 to 35 parts by weight of a binder, 5 to 10 parts by weight of a sol, 2 to 8 parts by weight of an oxide and the remainder of a high-silicon ZSM-5 molecular sieve. The binder is aluminum oxide or silicon oxide. The sol is an acidic silica sol. The oxide is a metal oxide or a non-metal oxide. The catalytic cracking aid for increasing propylene production can significantly increase the propylene concentration in the liquefied gas without increasing the liquefied gas yield during use in a catalytic cracking FCC unit.
[0006] CN101450321A discloses a catalytic cracking additive for increasing propylene production, which contains 10-40 weight % of silicon binder in terms of silicon dioxide, 10-30 weight % of aluminum binder in terms of alumina, 0.5-35 weight % of molecular sieve, 5-60 weight % of clay, and 0.5-2 weight % of rare earth oxide, based on the total weight of the additive. The molecular sieve contains a selective molecular sieve, and the additive introduces an anticoagulation inhibitor and a silicon binder in two steps during the preparation process. The additive has a strong heavy oil cracking ability, is used for catalytic cracking, and has a high propylene yield.
[0007] CN102872902A discloses a catalytic cracking additive for increasing propylene production. The additive comprises, by total weight, 50-75% of high-silicon zeolite, 20-45% of a binder and 1-5% of an oxide; the high-silicon zeolite is a ZSM-5 type hydrogen-type zeolite, SiO 2 With Al 2 O 3 The molar ratio of the additive is 100 to 500; the binder is one of kaolin, alumina, silicon oxide, diatomaceous earth and sol or a combination thereof; the oxide is one of alkali metal oxide, rare earth metal oxide and non-metal oxide or a combination thereof. The additive is mixed with the FCC catalyst during the use of the catalytic cracking FCC unit, and can significantly increase the propylene concentration in the liquefied gas without increasing the liquefied gas yield.
[0008] CN112387302A discloses a catalytic cracking aid, a preparation method and application thereof, and a method for catalytic cracking of hydrocarbon oil. The catalytic cracking aid comprises high-silicon zeolite, mesoporous silica, a binder and a modifier; wherein the high-silicon zeolite is a hydrogen-type zeolite with an MFI framework structure, and the silicon-aluminum molar ratio SiO 2 / Al 2 O 3The ratio of the catalytic cracking additive to the catalytic cracking agent is not less than 100; the mesoporous silica is a one-dimensional straight-through-channel mesoporous silica material; the modifier is selected from at least one of alkaline earth metal oxides, rare earth metal oxides and non-metallic oxides. The catalytic cracking additive is used in the catalytic cracking process of hydrocarbon oil, and can increase the propylene concentration in the liquefied gas while ensuring the yield of the catalytic cracking liquefied gas.
[0009] CN112570017 A catalytic cracking catalyst and a preparation method thereof, comprising: mixing and slurrying pentacyclic zeolite, optional faujasite zeolite, natural minerals, zirconium aluminum composite sol and other inorganic oxide binders, and spray drying; wherein the zirconium aluminum composite sol preparation method comprises the following steps: (1) mixing a zirconium dioxide precursor and water, exchanging with anion exchange resin to obtain a first mixture, wherein the pH value of the first mixture is 2-5; (2) reacting an aluminum oxide precursor, optional water, acid and the first mixture to form a second mixture, wherein the pH value of the second mixture is preferably 2-5; and optionally (3) mixing the second mixture with a surfactant. The catalyst has good strength and is used for catalytic cracking of heavy oil. It can have higher cracking activity than the existing pentacyclic zeolite cracking catalyst, and has higher ethylene and propylene selectivity. In addition, it can also have a higher liquefied gas yield and / or a higher propylene yield.
[0010] Phosphorus modification can significantly improve the cracking activity and stability of ZSM-5 zeolite additives.
[0011] USP6566293 discloses a cracking catalyst of phosphorus-modified ZSM-5 zeolite. The phosphorus-modified ZSM-5 is prepared by dispersing the zeolite in an aqueous solution of a phosphorus-containing compound having a pH value of above 4.5, so that the zeolite is loaded with at least 10% by weight of phosphorus (in terms of P 2 O 5 The catalyst is then slurried with the matrix and non-MFI structure zeolite components and spray-dried to form. The obtained catalyst has a high yield of light olefins for catalytic cracking.
[0012] CN1796497 discloses a catalytic cracking additive for increasing propylene production, characterized in that the additive is composed of 10-65 wt% of modified ZSM-5 molecular sieve, 0-60 wt% of clay, 15-70 wt% of inorganic oxide binder, 0.5-10 wt% of magnesium additive and 0.5-15 wt% of zinc additive on a dry basis, wherein the modified ZSM-5 molecular sieve is modified by phosphorus. The additive is applied in the catalytic cracking process, and can significantly increase the propylene concentration in the liquefied gas while increasing the yield of catalytic cracking liquefied gas and the octane number of catalytic cracking gasoline.
[0013] CN1049406C discloses a zeolite containing phosphorus and rare earth and having an MFI structure, and its anhydrous chemical composition is aRE2 O 3 ·bNa 2 O.Al 2 O 3 ·cP 2 O 5 dSiO 2 , wherein a=0.01-0.25, b=0.005-0.02, c=0.2-1.0, d=35-120. The zeolite has excellent hydrothermal activity stability and good selectivity for low-carbon olefins when used for high-temperature conversion of hydrocarbons.
[0014] CN1465527A discloses a MFI structure zeolite containing phosphorus and transition metals. The anhydrous chemical expression of the zeolite is (0-0.03) Na 2 O·(0.5-5)Al 2 O 3 ·(1.3-10)P 2 O 5 ·(0.7-15)M 2 O 3 ·(70-97)SiO 2 , wherein M is selected from one of transition metals Fe, Co and Ni. When the zeolite is applied to the catalytic cracking process of petroleum hydrocarbons, the yield and selectivity of C2-C4 olefins can be improved, and the yield of liquefied gas is higher.
[0015] In addition to phosphorus modification of ZSM-5 zeolite, it has also been reported that introducing phosphorus compounds into the matrix can improve the selectivity of the additive for propylene.
[0016] USP2002 / 0003103A1 discloses a catalytic cracking process for increasing the yield of propylene. The catalyst composition used contains not only large-pore USY zeolite, but also medium-pore zeolite such as ZSM-5 and an inorganic binder component with cracking performance. The inorganic binder component contains phosphorus, and its P / Al ratio is 0.1-10. The process can significantly increase the production of light olefins, especially increase the yield of propylene.
[0017] USP2002 / 0049133A1 discloses a catalyst with high zeolite content and high attrition resistance, which contains 30-85 wt% ZSM-5 zeolite, 6-24 wt% phosphorus (P 2 O 5 %, and less than 10 wt% Al 2 O 3 and the rest of clay and other components, wherein phosphorus exists in the matrix. The catalyst is used in catalytic cracking process to increase the yield of light olefins, especially propylene.
[0018] CN 100537030C discloses a catalyst auxiliary agent for increasing the propylene concentration of catalytic cracking liquefied gas, which contains, based on the weight of the auxiliary agent, 10-65 wt% of MFI structure zeolite, 0-20 wt% of non-MFI structure zeolite, 0-60 wt% of clay, 15-60 wt% of inorganic oxide binder in terms of oxide, 0.5-15 wt% of copper additive in terms of CuO and 0.5-15 wt% of P 2 O 5 The catalytic promoter is used in the catalytic cracking process of petroleum hydrocarbons to increase the yield of catalytic cracking liquefied gas and the octane number of catalytic cracking gasoline, and can significantly increase the propylene concentration in the liquefied gas.
[0019] CN102049284A discloses a catalytic cracking propylene additive, characterized in that the additive contains 30 to 80 weight percent of molecular sieves based on the total weight of the additive as 100%, wherein the content of ZSM-5 zeolite is 28 to 78 weight percent, and the additive contains 10 to 65 weight percent of clay, and the additive contains P, wherein P 2 O 5 5.0 to 20.0% by weight, preferably 7.0 to 15.0% by weight, La 2 O 3 The content of aluminum phosphate sol is 0-1.0 weight %; aluminum phosphate sol is used as a binder to improve the wear resistance of the additive, increase the solid content of the spray slurry, and avoid the chlorine content on the spray slurry and the additive. The activity of the prepared catalytic cracking propylene additive is significantly improved. When mixed with the main catalyst, it has less reduction in the activity of the main catalyst, can improve product distribution, has good dry gas and coke selectivity, and improves propylene yield.
[0020] CN107185586B discloses a catalytic cracking aid for producing more propylene and isopentene, and a preparation method and application thereof. The catalytic cracking aid for producing more propylene and isopentene comprises, on a dry basis, based on the total weight of the catalytic cracking aid, 15-45 wt% of alkali-modified ZSM-5 molecular sieve; 1-20 wt% of USY molecular sieve; 1-10 wt% of beta zeolite; 3-25 wt% of P 2 O 5 ; 3-25 wt% of inorganic oxides; and the balance of clay. The catalytic cracking aid for producing more propylene and isopentene can promote the shape-selective isomerization cracking reaction of gasoline components above C8 in catalytic cracking gasoline, can simultaneously increase the yields of propylene and isopentene, and increase the propylene content in the incremental liquefied gas (△ propylene / △ liquefied gas).
[0021] CN101474573B discloses a catalytic cracking aid with high propylene yield and a preparation method thereof, characterized in that it comprises the following components (wt%): polybasic organic acid modified ZSM-5 molecular sieve 10-60, Al 2O 3 10-40, P (in terms of P element) 1-20, rare earth element (in terms of RE2O3) 1-15, clay 5-40. The additive of the present invention is used in combination with various catalytic cracking catalysts and is suitable for heavy hydrocarbon oil and catalytic cracking raw material hydrocarbon oil from various sources; it has good selectivity for propylene, high catalytic cracking conversion rate, high liquefied gas output, and high propylene content in liquefied gas; at the same time, dry gas and coke are not increased. The preparation method thereof comprises the following steps: a. Preparation of phosphate aluminum liquid: according to P (in terms of P 2 O 5 (A) 2 O 3 =1-5:1 (mol ratio) of the phosphorus source compound and hydrated alumina are dissolved in deionized water, mixed and prepared into a phosphate aluminum gel with a solid content of 20-40wt%, stirred, and peptized at 20°C-60°C for 1-5 hours to obtain a phosphate aluminum liquid; b. Preparation of polybasic organic acid modified ZSM-5 molecular sieve: according to the formula, water is added to the ZSM-5 molecular sieve to prepare a slurry with a solid content of 10%, polybasic organic acid is added during stirring, and the reaction is stirred at 20-90°C for 1-5 hours, filtered, and the filter cake is washed with deionized water until the filtrate is neutral; c. The polybasic organic acid modified ZSM-5 molecular sieve prepared in step b is added with water to prepare a slurry with a solid content of 10%, and the polybasic organic acid is added during stirring. At 20-90°C, the reaction is stirred for 1-5 hours, filtered, and the filter cake is washed with deionized water until the filtrate is neutral; 5. Add water to the molecular sieve filter cake for pulping, then add the rare earth metal solution according to the formula, stir and react for 30-120 minutes, add ammonia water to adjust the pH value to precipitate the rare earth molecular sieve in the solution, and mix and pulp; d. Mixing and pulping: put the phosphate aluminum gel prepared in step a, the molecular sieve modified by the polybasic organic acid in step b and rare earthed by step c, clay and aluminum sol into a mixing pulping tank, mix and pulp for 1-2 hours, add hydrochloric acid to adjust the pH value to 3.0 while stirring, and continue to pulp for 30-60 minutes; e. Spray drying to form; f. Washing and drying: wash with deionized water to a pH value of 6-7, and dry at 80-120°C.
[0022] CN103254925B discloses a catalytic cracking additive for increasing propylene production, which comprises, by total weight of the additive, 20-60% of HZSM-5 molecular sieve, 5-25% of phosphate aluminum oxide, 6-12% of silica-alumina gel carrier, and the rest is kaolin; the HZSM-5 molecular sieve SiO 2 With Al 2 O 3 The molar ratio of the phosphorus aluminum oxide is (25-500):1; the phosphorus aluminum oxide is aluminum phosphate; and the silica aluminum gel carrier is silica aluminum gel. The catalytic cracking aid of the present invention is applied to the catalytic cracking process of petroleum hydrocarbons. While increasing the propylene yield and the gasoline octane number, it can significantly reduce the loss of the main product catalytic gasoline component. The preparation method thereof comprises the following steps: (1) preparing the phosphorus aluminum oxide: according to P 2 O 5 With Al 2O 3 Aluminum sol and ammonium phosphate are added to a certain amount of chemical water in a weight ratio of (2.5-3.0):1 to prepare phosphate aluminum gel with a solid content of 20-40%; (2) Preparation of silica-alumina gel: According to SiO 2 With Al 2 O 3 The aluminum sulfate solution is slowly added to the stirring water glass solution in a weight ratio of 2:1; (3) Mixing and beating: Add the phosphate aluminum gel to the beating tank, add the HZSM-5 molecular sieve, stir for 40-60 minutes, add kaolin, beat for 60 minutes, add the prepared silica aluminum gel, and continue beating for 30-60 minutes; (4) Drying and molding: Use spray drying molding method; (5) Calcination: Calcination at 400-600℃ for 4 hours; (6) Washing and drying: Wash once with chemical water, the washing temperature is 60℃, the water / agent ratio is (5-10):1, and after washing, dry at 110-120℃ to obtain the required auxiliary agent.
[0023] In the existing production process of catalytic cracking propylene additives, the additives need to be washed with water for multiple times after being formed. The total phosphorus content (measured in P) of the waste liquid after the additives are washed exceeds the limit of the "Comprehensive Sewage Discharge Standard" (GB8978-1996) (first-level standard: 0.5 mg / l; second-level standard: 1.0 mg / l). It is necessary to spend huge amounts of money to treat the phosphorus-containing wastewater before it can be discharged. Otherwise, it will cause serious pollution to the environment.
[0024] The existing technology mainly focuses on improving the cracking performance of catalytic cracking propylene additives and the phosphorus removal method of phosphorus-containing wastewater, but there is no relevant report on the recycling of phosphorus-containing wastewater of propylene additives. The existing technology uses adsorbents to adsorb phosphorus to meet the emission standards. This operation requires the adsorbent to be in contact with the wastewater for a long time, and the adsorbent must be regenerated regularly, which cannot meet the continuous production requirements of the propylene additive preparation process, and seriously affects the production capacity of the propylene additive.
[0025] Therefore, how to effectively improve the phosphorus utilization rate in the propylene additive production process and reduce the discharge of phosphorus-containing wastewater is an important measure for catalyst manufacturers to reduce costs and increase efficiency, and is also one of the key research topics for catalyst manufacturers. Summary of the invention
[0026] The purpose of the present invention is to provide a method for preparing a catalytic cracking propylene additive, so as to solve the problem of serious phosphorus pollution in the production process of the catalytic cracking propylene additive, realize direct discharge of wastewater on the existing additive production device without additional investment, and ensure the green production of the additive.
[0027] To achieve the above object, the present invention provides a method for preparing a catalytic cracking propylene additive, comprising the following steps:
[0028] 1) slurrying Y-type molecular sieve, humic acid and water to obtain Y-type molecular sieve slurry, filtering the Y-type molecular sieve slurry to form a Y-type molecular sieve filter cake layer, wherein the dry weight ratio of the humic acid to the Y-type molecular sieve is 0.001-0.05;
[0029] 2) Slurrying ZSM-5 molecular sieve and phosphorus-containing wastewater to obtain ZSM-5 molecular sieve slurry, filtering the ZSM-5 molecular sieve slurry through a Y-type molecular sieve filter cake layer to form a ZY composite filter cake layer, performing ion exchange on the ZY composite filter cake layer with a first phosphorus-containing exchange liquid, and then washing the ZY composite molecular sieve filter cake, wherein the weight ratio of the first phosphorus-containing exchange liquid to the ZSM-5 molecular sieve dry basis is 0.005-0.15 in terms of P;
[0030] 3) The ZY composite molecular sieve filter cake, inorganic oxide, clay, binder and water are mixed and slurried, spray dried and formed, and calcined to obtain additive microspheres, the additive microspheres are mixed and slurried with water, and then filtered to form microsphere filter cakes, and the microsphere filter cakes are ion exchanged with a second phosphorus-containing exchange liquid, and then washed and dried to obtain a catalytic cracking propylene additive, wherein the weight ratio of the second phosphorus-containing exchange liquid to the dry basis of the microspheres is 0.005-0.10 in terms of P.
[0031] In the present invention, the slurrying conditions of the Y-type molecular sieve and water in step 1) are well known to those skilled in the art, and the content of the Y-type molecular sieve in the slurry is generally 100-300 g / L. The temperature of the slurry can be 10-100°C, preferably 50-90°C. The spray drying molding and calcination curing conditions in step 3) are well known to those skilled in the art, such as the drying temperature is from room temperature to 200°C, preferably 100-150°C, the calcination curing temperature is 300-600°C, preferably 400-500°C, and the calcination time is 10-200 minutes, preferably 30-60 minutes.
[0032] The preparation method of the catalytic cracking propylene additive of the present invention, the Y-type molecule is selected from USY, REY, HY, REHY, NH 4 One or more of Y and REUSY.
[0033] In the preparation method of the catalytic cracking propylene additive of the present invention, the humic acid is selected from one or more of fulvic acid, palmitic acid and black humic acid.
[0034] In the preparation method of the catalytic cracking propylene additive of the present invention, the ZSM-5 molecular sieve can be selected from ZSM-5 molecular sieves with different silicon-aluminum ratios, or can be the corresponding ZSM-5 molecular sieve modified by metal ions. Preferably, the metal ions are rare earth ions.
[0035] In the method for preparing the catalytic cracking propylene additive of the present invention, the mass ratio of the phosphorus-containing wastewater to the ZSM-5 molecular sieve is 2-10, preferably 3-6.
[0036] In the method for preparing the catalytic cracking propylene additive of the present invention, the phosphorus-containing wastewater is the filtrate collected after ion exchange of the microsphere filter cake with the second phosphorus-containing exchange liquid in step 3).
[0037] In the method for preparing the catalytic cracking propylene additive of the present invention, the first phosphorus-containing exchange liquid and the second phosphorus-containing exchange liquid are one or more of ammonium phosphate solution, diammonium hydrogen phosphate solution, diammonium dihydrogen phosphate solution and phosphoric acid.
[0038] In the method for preparing the catalytic cracking propylene additive of the present invention, the first phosphorus-containing exchange liquid is prepared by preparing the filtrate collected after ion exchange of the microsphere filter cake with the second phosphorus-containing exchange liquid in step 3).
[0039] In the preparation method of the catalytic cracking propylene additive of the present invention, the inorganic oxide is one or more of rare earth oxide, magnesium oxide and silicon oxide; the clay is one or more of kaolin, halloysite and montmorillonite; and the binder is one or more of aluminum sol, silica sol and pseudo-boehmite.
[0040] The preparation method of the catalytic cracking propylene additive of the present invention comprises steps 1) and 2) being carried out on a first horizontal belt filter, wherein the first horizontal bag filter comprises a Y-type molecular sieve filter cake forming zone, a ZMS-5 molecular sieve filter cake forming zone, a phosphorus exchange zone and a water washing zone connected in series; and step 3) being carried out on a second horizontal belt filter, wherein the second horizontal belt filter comprises a microsphere filter cake forming zone, a phosphorus exchange zone and a metal ion exchange zone connected in series.
[0041] Beneficial effects of the present invention:
[0042] The preparation method of the catalytic cracking propylene additive provided by the present invention first forms a Y-type molecular sieve filter cake layer, and then loads the ZSM-5 molecular sieve after the phosphorus-containing wastewater exchange on the Y-type molecular sieve filter cake, and the excess phosphorus in the filtrate is recovered by the Y-type molecular sieve filter cake layer, thereby reducing the loss of phosphorus. At the same time, the excess phosphorus can also modify the Y-type molecular sieve, and the thermal stability and hydrothermal stability of the Y-type molecular sieve are simultaneously improved. The humic acid added by the present invention is a multi-organic complex, which has the function of fixing phosphorus elements, so that the phosphorus element is not easy to be lost with the filtrate, and the phosphorus utilization rate is further improved. The preparation method of the catalytic cracking additive provided by the present invention recycles the phosphorus-containing wastewater of the additive microspheres for the molecular sieve ion exchange process, which can effectively reduce the water consumption and phosphorus exchange liquid consumption in the additive production process, and is conducive to reducing the production cost of the additive. Therefore, compared with the prior art, the preparation method of the catalytic cracking propylene additive provided by the present invention does not need to increase additional investment, and the wastewater direct discharge requirements can be achieved on the existing production equipment, and the operation process is simple, providing technical support for green production and energy saving and consumption reduction of catalyst enterprises. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 This is a flow chart of the molecular sieve phosphorus exchange process of the present invention;
[0044] Figure 2 The figure is a flow chart of the phosphorus exchange process of the auxiliary agent microspheres of the present invention.
[0045] Wherein, the reference numerals are:
[0046] 1, 5, 15, 16 beating tanks;
[0047] Pipelines 2, 6, 10, 13, 17, 21, 25;
[0048] 3. 18 filter cloth;
[0049] 4Y molecular sieve cake formation area
[0050] 7ZSM-5 molecular sieve filter cake formation area
[0051] 8.23 Liquid receiver
[0052] 9, 12, 20, 24 containers
[0053] 14, 26 washing area
[0054] 19 Microsphere filter cake formation area
[0055] 11, 22 ion exchange area
[0056] 27 Recovery of filtrate DETAILED DESCRIPTION
[0057] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention.
[0058] According to the method provided by the present invention, Figure 1 , Figure 2 The process flow shown implements the present invention.
[0059] 1. Formation of Y-type molecular sieve filter cake
[0060] The Y-type molecular sieve, humic acid and water at 10-100°C, preferably 50-90°C, are slurried, and the formed slurry is continuously loaded from the slurrying tank 1 to the filter cloth 3 of the horizontal vacuum belt filter through the pipeline 2, and the filter cloth moves continuously and enters the Y-type molecular sieve filter cake forming area 4. The liquid receiver 8 is located below the filter cloth 3, and the liquid receiver 8 is evacuated. Under the action of vacuum, the liquid in the slurry on the filter cloth 3 enters the liquid receiver 8 through the filter cloth 3. At the same time, the Y-type molecular sieve slurry on the filter cloth 3 forms a filter cake, and the loading speed of the Y-type molecular sieve slurry should ensure that the thickness of the Y-type molecular sieve filter cake formed is 0.5-1.5 cm, preferably 0.8-1.5 cm. The vacuum degree in the vacuum box 8 makes the filter cake surface free of cracks. The vacuum degree in the vacuum box 8 is generally 0.02-0.08 MPa, preferably 0.05-0.08 MPa.
[0061] 2. Formation of ZSM-5 molecular sieve filter cake
[0062] The 50-100°C ZSM-5 molecular sieve slurry is continuously loaded from the beating tank 5 to the Y-type molecular sieve filter cake layer of the horizontal vacuum belt filter through the pipeline 6, and moves with the filter cloth into the ZSM-5 molecular sieve filter cake forming area 7. The phosphorus-containing wastewater can be provided by the microsphere exchange process liquid receiver 23 described below, which can reduce the amount of water used and recover phosphorus in the filtrate of the catalyst microsphere ion exchange process to reduce the amount of sewage discharged. At the same time, the ZSM-5 molecular sieve slurry on the filter cloth 3 forms a filter cake, and the loading speed of the ZSM-5 molecular sieve slurry should ensure that the thickness of the ZSM-5 molecular sieve filter cake formed is 0.5-1.5 cm, preferably 0.8-1.5 cm.
[0063] 3. Composite Molecular Sieve Ion Exchange
[0064] As the filter cloth 3 moves, the filter cake formed in the Y-type molecular sieve filter cake forming area 4 and the ZSM-5 filter cake forming area 7 enters the ion exchange area 11, and a phosphorus exchange liquid with a temperature of 20-100° C., preferably 30-90° C., is added from the container 9 through the pipeline 10. Under the action of vacuum, the phosphorus exchange liquid performs ion exchange while passing through the filter cake.
[0065] 4. Composite Molecular Sieve Washing
[0066] The washing method is well known to those skilled in the art. The filter cake obtained in the ion exchange zone 11 enters the water washing zone 14, and deionized water is added from the container 12 through the pipeline 13. The weight ratio of deionized water to the composite molecular sieve is generally 1-15, preferably 2-10, and the temperature of the deionized water is 20-100° C., preferably 30-90° C. Under the action of vacuum, the liquid passes through the filter cake to wash away the residual ions, especially the anions, in the filter cake.
[0067] 5. Forming and curing of additive microspheres
[0068] The washed composite molecular sieve filter cake enters the pulping tank 15, where inorganic oxides, clay, binder and water are added, mixed and pulped, sprayed and formed, and calcined and solidified to obtain additive microspheres.
[0069] 6. Formation of microsphere filter cake
[0070] The curing aid microspheres are put into the beating tank 16, water is added for beating, and the microsphere slurry is continuously loaded from the beating tank 16 to the filter cloth 18 of the horizontal vacuum belt filter through the pipeline 17, and the filter cloth is continuously moved and enters the microsphere filter cake forming area 19. The liquid receiver 23 is located below the filter cloth 18, and the liquid receiver 23 is evacuated. Under the vacuum effect, the liquid in the slurry on the filter cloth 18 enters the liquid receiver 23 through the filter cloth 18. At the same time, the microsphere slurry on the filter cloth 18 forms a filter cake, and the loading speed of the microsphere slurry should ensure that the thickness of the microsphere filter cake formed is 0.5-2.0 cm, preferably 0.8-1.5 cm. The vacuum degree in the vacuum box 23 is generally 0.02-0.08 MPa, preferably 0.03-0.08 MPa.
[0071] 7. Additive Microsphere Phosphorus Exchange
[0072] As the filter cloth 18 moves, the filter cake formed in the microsphere filter cake forming area 19 enters the ion exchange area 22, and a phosphorus exchange liquid with a temperature of 20-100° C., preferably 30-90° C., is added from the container 20 through the pipeline 21. Under the action of vacuum, the phosphorus exchange liquid passes through the filter cake while performing ion exchange.
[0073] 8. Auxiliary microsphere washing
[0074] The washing method is well known to those skilled in the art. The filter cake obtained in the ion exchange zone 22 enters the water washing zone 26. Deionized water is added from the container 24 through the pipeline 25 to the microsphere filter cake obtained in the ion exchange zone 22. The weight ratio of deionized water to microspheres is generally 1-15, preferably 2-10, and the temperature of the deionized water is 20-100° C., preferably 30-90° C. Under the action of vacuum, the liquid penetrates the filter cake to wash away the residual ions in the filter cake.
[0075] The following example uses a Buchner funnel filter device to conduct experiments to illustrate the method provided by the present invention. Since the Buchner funnel filter device also undergoes the stages of filter cake formation, ion exchange and washing, but these steps are performed separately, they are equivalent to the continuous process on the belt filter.
[0076] Source of raw materials:
[0077] 1) USY molecular sieve: produced by Lanzhou Petrochemical Company, Na 2 The O content is 0.9%, and the unit cell constant is 24.36 angstroms;
[0078] REY molecular sieve: produced by Lanzhou Petrochemical Company, Na 2 O content is 1.1%, RE2O3 content is 14.8%, unit cell constant is 24.66 angstroms;
[0079] HY molecular sieve: produced by Lanzhou Petrochemical Company, Na 2 The O content is 1.5%, and the unit cell constant is 24.39 angstroms;
[0080] NH 4 Y molecular sieve: produced by Lanzhou Petrochemical Company, Na 2 The O content is 1.2%, and the unit cell constant is 24.41 angstroms;
[0081] REHY molecular sieve: produced by Lanzhou Petrochemical Company, Na 2 O content is 1.3%, RE2O3 content is 1.5%, unit cell constant is 24.45 angstroms;
[0082] REUSY molecular sieve: produced by Lanzhou Petrochemical Company, Na 2 O content is 0.8%, RE2O3 content is 0.9%, unit cell constant is 24.39 angstroms;
[0083] Fe-ZSM-5 molecular sieve: produced by Lanzhou Petrochemical Company, molar ratio (SiO 2 / Al 2 O 3 ) is 40;
[0084] Zn-ZSM-5 molecular sieve: produced by Lanzhou Petrochemical Company, molar ratio (SiO 2 / Al 2 O 3 ) is 300;
[0085] La-ZSM-5 molecular sieve: produced by Lanzhou Petrochemical Company, molar ratio (SiO 2 / Al 2 O 3 ) is 100;
[0086] Kaolin, halloysite, montmorillonite, silica sol, pseudoboehmite and alumina sol were all from Lanzhou Petrochemical Company.
[0087] 2) Fulvic acid, palmitic acid, humic acid, phosphoric acid, ammonium phosphate, diammonium hydrogen phosphate, monoammonium phosphate, yttrium oxide, magnesium oxide, and white carbon black: analytically pure, all are chemical reagents.
[0088] Specific analysis method:
[0089] Phosphorus content in the filtrate: detected by ICP (Inductive Coupled Plasma Emission Spectrometer).
[0090] Comparative Example 1
[0091] The samples were prepared according to patent CN101474573B.
[0092] a. Preparation of phosphate aluminum liquid: 0.65 kg (dry basis) pseudo-boehmite and 2.52 kg of 85% orthophosphoric acid were dissolved in deionized water, mixed and prepared into a phosphate aluminum gel with a solid content of 30wt%, stirred, and peptized at 20 ℃-60 ℃ for 1-5 hours; to obtain a phosphate aluminum liquid;
[0093] b. Preparation of polybasic organic acid modified ZSM-5 molecular sieve: Weigh 4 kg of ZSM-5 molecular sieve, add water to prepare a slurry with a solid content of 10%, add 3 kg of oxalic acid while stirring, stir at a temperature of 20-90 ° C, react for 1-5 hours, filter, and wash the filter cake with deionized water until the filtrate is neutral;
[0094] c. Rare earth treatment: The polyacid-modified ZSM-5 molecular sieve filter cake prepared in step b was slurried with water and prepared into a molecular sieve slurry with a solid content of 20% by weight, and YCl 3 Solution 0.3 kg (according to Y 2 O 3 ), stirring and reacting for 30-120 minutes, adding ammonia water to adjust the pH to 11, so that the rare earth molecular sieve in the solution is precipitated, and mixing and slurrying;
[0095] d. Mixing and beating: put the phosphate aluminum gel prepared in step a, the molecular sieve modified by the polybasic organic acid in step b and rare earthed by step c, 2.5 kg of kaolin, and 1.16 kg of aluminum sol into a mixing and beating tank, mix and beat for 1-2 hours, add hydrochloric acid to adjust the pH value to 3.0 while stirring, and continue beating for 30-60 minutes;
[0096] e. Spray drying molding;
[0097] f. Washing and drying: Wash with deionized water until the pH value of the washing water is between 6 and 7, dry at 80-120°C, collect the microsphere filtrate A and the additive finished product D1, wherein the phosphorus content of the microsphere filtrate A is 123 mg / L.
[0098] Comparative Example 2
[0099] The samples were prepared according to patent CN102794194B.
[0100] The preparation of catalytic cracking aid comprises the following steps:
[0101] (1) Exchange and washing of NaZSM-5 molecular sieve: 8.7 kg of acetic acid was weighed, and an appropriate amount of cold water was added and stirred to dissolve. Then, 18.9 kg of nitric acid with a concentration of 20 wt % was added, and then cold water was added to dilute the solution to 1000 L to prepare a low concentration mixed acid solution. The solution temperature was controlled at 1±0.5°C. 125 kg of dry NaZSM-5 molecular sieve powder was added during stirring (in the molecular sieve exchange solution, H 2 The mixture was stirred at 1±0.5°C for 2 hours, and the slurry was filtered. The filter cake was rinsed with deionized water 5 times the weight of the NaZSM-5 molecular sieve powder.
[0102] (2) flash drying the product of step (1) and calcining at 550° C. for 3 hours;
[0103] (3) slurrying the product of step (2) at a ratio of molecular sieve dry basis: water = 1:3 to prepare a molecular sieve slurry;
[0104] (4) adding kaolin, aluminum sol, and yttrium oxide to the molecular sieve slurry obtained in step (3) in a ratio of molecular sieve: kaolin: aluminum sol (calculated as aluminum oxide): yttrium oxide = 50:27:20:3 to prepare an additive mixed slurry;
[0105] (5) spray drying the slurry obtained in step (4) to prepare additive microspheres according to a conventional spray drying molding method for preparing catalytic cracking propylene additives;
[0106] (6) Auxiliary agent washing: 1740 g of acetic acid was weighed, and an appropriate amount of cold water was added and stirred to dissolve. Then, 3780 g of nitric acid with a concentration of 20 wt % was added, and then cold water was added to dilute the solution to 1000 L to prepare a low concentration mixed acid solution. The solution temperature was controlled at 1±0.5° C., and 167 kg of dry catalytic cracking propylene auxiliary agent was added during stirring (in the auxiliary agent washing solution, H 2 O: catalytic cracking propylene aid dry weight ratio = 6: 1), then stirring and reacting at 1 ± 0.5 ° C for 2 hours, then filtering the slurry, and rinsing the filter cake with deionized water 5 times the dry weight of the catalytic cracking propylene aid;
[0107] (7) Drying the product gas stream of step (6) to obtain a finished product of a catalytic cracking propylene additive, which is denoted as D2.
[0108] Comparative Example 3
[0109] 1) The ZSM-5 molecular sieve obtained in step 2) of comparative example 2 was mixed with phosphorus-containing wastewater (microsphere filtrate A of comparative example 1) to prepare ZMS-5 molecular sieve slurry, and the mass of microsphere filtrate A was 5 times that of ZMS-5 molecular sieve. The obtained ZMS-5 molecular sieve slurry was heated to 70° C. and stirred for 1 h, poured into a Buchner funnel, and the filter bottle was evacuated to 0.07 MPa at the same time to form a ZMS-5 molecular sieve filter cake with a thickness of 10 mm on the filter cloth.
[0110] 3) When there is no liquid on the surface of the filter cake, immediately add a 90°C ammonium phosphate solution at a speed that ensures that no cracks are formed on the surface of the filter cake. The amount of ammonium phosphate is such that the weight ratio of P to ZMS-5 molecular sieve is 0.04. When there is no liquid on the surface of the filter cake, immediately add deionized water at 80°C to wash the filter cake. The weight ratio of deionized water to ZMS-5 molecular sieve is 5. Then remove the molecular sieve filter cake and collect the filtrate B.
[0111] 4) adding kaolin, aluminum sol and yttrium oxide to the molecular sieve slurry obtained in step (3) in a ratio of molecular sieve: kaolin: aluminum sol (calculated as aluminum oxide): yttrium oxide = 50:27:20:3 to prepare an additive mixed slurry;
[0112] 5) According to the conventional spray drying molding method for preparing auxiliary agents, the slurry obtained in step (4) is spray-dried to prepare auxiliary agent microspheres, and then calcined and solidified.
[0113] 6) Additive washing: The curing additive microspheres prepared in step 5) are mixed with water to prepare a slurry having an additive microsphere content of 110 g / L. The obtained slurry is heated to 60° C. and poured into a Buchner funnel. The filter bottle is evacuated to 0.06 MPa to form a filter cake with a thickness of 10 mm on the filter cloth.
[0114] 7) When there is no liquid on the surface of the filter cake in step 6), immediately add ammonium phosphate solution at a temperature of 90°C, and the amount of ammonium phosphate is such that the weight ratio of P to microspheres is 0.03. When there is no liquid on the surface of the filter cake, immediately add deionized water at a temperature of 90°C to wash the filter cake, and the weight ratio of deionized water to microspheres is 5. Then remove the filter cake and collect the filtrate C, dry it to obtain the additive sample D3, and the phosphorus content of the filtrate B is 158 mg / L.
[0115] Example 1
[0116] 1) Mix USY molecular sieve, fulvic acid and water to make a molecular sieve slurry with a molecular sieve content of 180 g / L, wherein the amount of fulvic acid added is 0.03:1 on a dry basis. Heat the obtained molecular sieve slurry to 80°C and pour it into a Buchner funnel. At the same time, evacuate the filter bottle to 0.07 MPa to form a filter cake with a thickness of 10 mm on the filter cloth.
[0117] 2) The ZSM-5 molecular sieve obtained in step 2) of comparative example 2 was mixed with the phosphorus-containing wastewater (microsphere filtrate A of comparative example 1) and slurried. The mass of microsphere filtrate A was 5 times that of the molecular sieve to prepare ZSM-5 molecular sieve slurry. The obtained ZSM-5 molecular sieve slurry was heated to 70° C. and stirred for 1 h. The slurry was poured onto the USY filter cake obtained in step 1) of the Buchner funnel. At the same time, the filter bottle was evacuated to 0.07 MPa to form a ZSM-5 molecular sieve filter cake with a thickness of 10 mm on the filter cloth.
[0118] 3) When there is no liquid on the surface of the filter cake, immediately add ammonium phosphate solution at a temperature of 90°C, and the addition speed ensures that no cracks are formed on the surface of the filter cake. The amount of ammonium phosphate is such that the weight ratio of P to ZSM-5 molecular sieve is 0.04. When there is no liquid on the surface of the filter cake, immediately add deionized water at a temperature of 80°C to wash the filter cake, and the weight ratio of deionized water to the composite molecular sieve is 5. Then remove the composite molecular sieve filter cake and collect the filtrate D, in which the dry basis mass ratio of the Y-type molecular sieve to the ZSM-5 molecular sieve is 6:94.
[0119] 4) adding kaolin, aluminum sol and yttrium oxide to the molecular sieve slurry obtained in step (3) in a ratio of molecular sieve: kaolin: aluminum sol (calculated as aluminum oxide): yttrium oxide = 50:27:20:3 to prepare an additive mixed slurry;
[0120] 5) According to the conventional spray drying molding method for preparing auxiliary agents, the slurry obtained in step (4) is spray-dried to prepare auxiliary agent microspheres, and then calcined and solidified.
[0121] 6) Additive washing: The curing additive microspheres prepared in step 5) are mixed with water to prepare a slurry having an additive microsphere content of 110 g / L. The obtained slurry is heated to 60° C. and poured into a Buchner funnel. The filter bottle is evacuated to 0.06 MPa to form a filter cake with a thickness of 10 mm on the filter cloth.
[0122] 7) When there is no liquid on the surface of the filter cake in step 6), immediately add ammonium phosphate solution at a temperature of 90°C, and the amount of ammonium phosphate is such that the weight ratio of P to microspheres is 0.03. When there is no liquid on the surface of the filter cake, immediately add deionized water at a temperature of 90°C to wash the filter cake, and the weight ratio of deionized water to microspheres is 5. Then remove the filter cake and collect the filtrate E, dry the filter cake to obtain the additive sample S1, and the phosphorus content of the filtrate D is 0.8 mg / L.
[0123] Example 2
[0124] The operation steps are the same as those in Example 1, except that:
[0125] Step 1) The content of REY molecular sieve slurry is 300 g / L, the weight ratio of humic acid added to REY molecular sieve dry basis is 0.001:1, the slurry temperature is 15° C., the vacuum degree of the filter bottle is 0.08 MPa, and the filter cake thickness is 5 mm.
[0126] Step 2) Fe-ZSM-5 molecular sieve and phosphorus-containing wastewater (filtrate E) are mixed and slurried, the amount of filtrate E is twice that of the molecular sieve, the slurry temperature is 50° C., stirring is performed for 2 hours, the vacuum degree of the filter bottle is 0.08 MPa, and the filter cake thickness is 15 mm.
[0127] Step 3) The amount of diammonium hydrogen phosphate is such that the weight ratio of P to ZSM-5 molecular sieve is 0.005. The temperature of deionized water is 100° C., and the weight ratio of deionized water to molecular sieve is 1. Remove the molecular sieve filter cake and collect the filtrate F.
[0128] Step 4) Molecular sieve: halloysite: silica sol (calculated as silicon dioxide): magnesium oxide = 35:54:10:1.
[0129] Step 5) spray drying and curing.
[0130] Step 6) The microsphere content is 300 g / L, the slurry temperature is 80° C., the filter flask vacuum is 0.02 MPa, and the filter cake thickness is 5 mm.
[0131] Step 7) The weight ratio of ammonium dihydrogen phosphate to the additive is 0.10, the temperature of deionized water is 20° C., and the weight ratio of deionized water to the additive microspheres is 10. Then the filter cake is removed and the filtrate I is collected to obtain the additive sample S2, and the phosphorus content of the filtrate F is 0.6 mg / L.
[0132] Example 3
[0133] The operation steps are the same as those in Example 1, except that:
[0134] Step 1) The molecular sieve slurry with a dry basis mass ratio of REUSY to HY of 1:1 has a content of 100 g / L, the weight ratio of humic acid added to the molecular sieve dry basis is 0.05:1, the slurry temperature is 100° C., the vacuum degree of the filter bottle is 0.02 MPa, and the filter cake thickness is 15 mm.
[0135] Step 2) Zn-ZSM-5 molecular sieve is mixed with phosphorus-containing wastewater (filtrate I) for slurrying, the amount of filtrate I is 10 times that of the molecular sieve, the slurry temperature is 100° C., stirring is performed for 0.5 h, the vacuum degree of the filter bottle is 0.02 MPa, and the filter cake thickness is 5 mm.
[0136] Step 3) The temperature is 20° C., and the weight ratio of diammonium hydrogen phosphate to molecular sieve is 0.15. The temperature of deionized water is 20° C., and the weight ratio of deionized water to molecular sieve is 3. Remove the molecular sieve filter cake and collect the filtrate J.
[0137] Step 4) Molecular sieve: montmorillonite: pseudo-boehmite (calculated as alumina): white carbon = 40:43:15:2.
[0138] Step 5) spray drying and curing.
[0139] Step 6) The content of the additive microspheres is 100 g / L, the slurry temperature is 20° C., the vacuum degree of the filter bottle is 0.08 MPa, and the filter cake thickness is 20 mm.
[0140] Step 7) The weight ratio of diammonium hydrogen phosphate to the additive is 0.005, the temperature of deionized water is 100° C., and the weight ratio of deionized water to the additive microspheres is 7. Then the filter cake is removed and the filtrate K is collected to obtain the additive sample S3, and the phosphorus content of the filtrate J is 0.4 mg / L.
[0141] Example 4
[0142] The operation steps are the same as those in Example 1, except that:
[0143] Step 1) NH 4 The dry basis mass ratio of Y to REHY is 1:3, the molecular sieve slurry content is 180 g / L, the weight ratio of humic acid and fulvic acid added to the molecular sieve dry basis is 0.03:1 respectively, the slurry temperature is 75°C, the vacuum degree of the filter bottle is 0.04 MPa, and the filter cake thickness is 8 mm.
[0144] Step 2) The rare earth ZSM-5 molecular sieve obtained in step c of comparative example 1 was mixed with phosphorus-containing wastewater (filtrate K) and slurried. The amount of filtrate K was 4 times that of the molecular sieve. The slurry temperature was 70°C. The mixture was stirred for 1.5 hours. The vacuum degree of the filter bottle was 0.04 MPa. The filter cake thickness was 13 mm.
[0145] Step 3) The weight ratio of phosphoric acid to molecular sieve is 0.01, the temperature of deionized water is 40° C., and the weight ratio of deionized water to molecular sieve is 8. Remove the molecular sieve filter cake and collect the filtrate L.
[0146] Step 4) Molecular sieve: kaolin: aluminum sol (calculated as alumina): yttrium oxide = 45:34.5:20:0.5.
[0147] Step 5) spray drying and curing.
[0148] Step 6) The content of the additive microspheres is 170 g / L, the slurry temperature is 60° C., the vacuum degree of the filter bottle is 0.04 MPa, and the filter cake thickness is 18 mm.
[0149] Step 7) The weight ratio of phosphoric acid to the auxiliary agent is 0.02. The temperature of deionized water is 60°C, and the weight ratio of deionized water to the auxiliary agent is 9. The filter cake is dried at 200°C and then calcined at 500°C for 1h, then the filter cake is removed and the filtrate M is collected to obtain an auxiliary agent sample S4, and the phosphorus content of the filtrate L is 0.5 mg / L.
[0150] Example 5
[0151] The industrial grade LDO-75 industrial catalyst was used as the main catalyst, and the additives prepared in Examples 1-4 and Comparative Examples 1-3 were mixed uniformly at a weight ratio of 95:5 to obtain a mixed catalyst, which was aged at 800°C for 10 hours with 100% steam. The catalytic performance of the mixed catalyst was evaluated on a fixed fluidized bed device using 3 million tons / year of catalytic raw materials from Lanzhou Petrochemical as the evaluation oil (properties are shown in Table 1). The blank is the evaluation result of the main catalyst without additives. The evaluation conditions are reaction temperature 500°C, regeneration temperature 700°C, and catalyst-oil ratio 4. The evaluation results are shown in Table 2.
[0152] Table 1 Catalytic raw material properties
[0153]
[0154] Table 2 Evaluation results of additives, %
[0155]
[0156] It can be seen from the results of Examples S1 to S4 that the phosphorus content of the filtrate obtained by the method of the present invention is less than 1 mg / l, which meets the national secondary emission standards. Compared with Comparative Example 1, the operation process of the present invention is simple and the direct discharge of wastewater can be achieved on the existing auxiliary agent preparation device. Compared with Comparative Example 2, the method of the present invention is operable in actual production. Comparative Example 2 requires exchange at a temperature of 0-5°C, harsh operating conditions, and great difficulty in industrial operation, which cannot meet actual production needs. It can be seen from the evaluation data that the auxiliary agent prepared by the method of the present invention can improve the propylene yield and propylene selectivity of the catalytic cracking catalyst, and the auxiliary agent filtrate prepared by the method provided by the present invention has a low phosphorus content, does not need to be treated, can meet the direct discharge requirements, and has good operability and has a good prospect for industrial application.
[0157] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a catalytic cracking propylene additive, characterized in that: The following steps are involved: 1) slurrying Y-type molecular sieve, humic acid and water to obtain Y-type molecular sieve slurry, filtering the Y-type molecular sieve slurry to form a Y-type molecular sieve filter cake layer, wherein the dry weight ratio of the humic acid to the Y-type molecular sieve is 0.001-0.05; 2) Slurrying ZSM-5 molecular sieve and phosphorus-containing wastewater to obtain ZSM-5 molecular sieve slurry, filtering the ZSM-5 molecular sieve slurry through a Y-type molecular sieve filter cake layer to form a ZY composite filter cake layer, performing ion exchange on the ZY composite filter cake layer with a first phosphorus-containing exchange liquid, and then washing the ZY composite molecular sieve filter cake, wherein the weight ratio of the first phosphorus-containing exchange liquid to the ZSM-5 molecular sieve dry basis is 0.005-0.15 in terms of P; 3) The ZY composite molecular sieve filter cake, inorganic oxide, clay, binder and water are mixed and slurried, spray dried and formed, and calcined to obtain additive microspheres, the additive microspheres are mixed and slurried with water, and then filtered to form microsphere filter cakes, and the microsphere filter cakes are ion exchanged with a second phosphorus-containing exchange liquid, and then washed and dried to obtain a catalytic cracking propylene additive, wherein the weight ratio of the second phosphorus-containing exchange liquid to the dry basis of the microspheres is 0.005-0.10 in terms of P.
2. The method for preparing the catalytic cracking propylene additive according to claim 1, characterized in that: The Y-type molecule is selected from one or more of USY, REY, HY, REHY, NH4Y and REUSY.
3. The method for preparing the catalytic cracking propylene additive according to claim 1, characterized in that: The humic acid is selected from one or more of fulvic acid, palmitic acid and humic acid.
4. The method for preparing the catalytic cracking propylene additive according to claim 1, characterized in that: The ZSM-5 molecular sieve is a ZSM-5 molecular sieve modified by metal ions, and preferably, the metal ions are rare earth ions.
5. The method for preparing the catalytic cracking propylene additive according to claim 1, characterized in that: The mass ratio of the phosphorus-containing wastewater to the ZSM-5 molecular sieve is 2-10, preferably 3-6.
6. The method for preparing the catalytic cracking propylene additive according to claim 1, characterized in that: The phosphorus-containing wastewater is the filtrate collected after ion exchange of the microsphere filter cake with the second phosphorus-containing exchange liquid in step 3).
7. The method for preparing a catalytic cracking propylene additive according to claim 1, characterized in that: The first phosphorus-containing exchange liquid and the second phosphorus-containing exchange liquid are one or more of ammonium phosphate solution, diammonium hydrogen phosphate solution, diammonium dihydrogen phosphate solution and phosphoric acid.
8. The method for preparing a catalytic cracking propylene additive according to claim 1, characterized in that: The first phosphorus-containing exchange solution is prepared by collecting the filtrate after ion exchange of the microsphere filter cake with the second phosphorus-containing exchange solution in step 3).
9. The method for preparing a catalytic cracking propylene additive according to claim 1, characterized in that: The inorganic oxide is one or more of rare earth oxide, magnesium oxide and silicon oxide; the clay is one or more of kaolin, halloysite and montmorillonite; the binder is one or more of aluminum sol, silica sol and pseudo-boehmite.
10. The method for preparing a catalytic cracking propylene additive according to claim 1, characterized in that: Step 1) and step 2) are performed on a first horizontal belt filter, wherein the first horizontal bag filter comprises a Y-type molecular sieve filter cake forming zone, a ZMS-5 molecular sieve filter cake forming zone, a phosphorus exchange zone and a water washing zone connected in series; and step 3) is performed on a second horizontal belt filter, wherein the second horizontal belt filter comprises a microsphere filter cake forming zone, a phosphorus exchange zone and a water washing zone connected in series.
Citation Information
Patent Citations
Process for the production of an anion exchanger, and a use of same
CA1169735A
Process for the production of distillates and lubricanting oils
CA2472906A1
Preparation method of inorganic-organic compound-type adsorbent based on clinoptilolite and application for removing Cr(VI) in industrial waste water
CN101797496A
Catalytic cracking catalyst for efficient conversion of heavy oil, and preparation method thereof
CN103447063A
Catalytic cracking catalyst for cracking coker gas oil and increasing production of liquefied gas and preparation method thereof
CN109304222A