Gallium-based liquid alloy micro-nano motor and preparation method thereof

By preparing gallium-based liquid alloy micro-nano motors and using Ga and Au doping and ultrasonic dispersion technology to form the Janus structure, the problems of slow movement speed and uncertain preparation size of micro-nano motors in the existing technology have been solved, and a more efficient Improved athletic performance and activity.

CN118768561APending Publication Date: 2024-10-15SHANGHAI UNIV OF ENG SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410843810.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing Ga@Pt micro-nano motors have slow movement speeds and uncertain sizes during the preparation process, which results in difficult post-modification and insufficient movement performance.

Method used

Using the preparation method of gallium-based liquid alloy micro-nano motors, liquid Ga and Au powders are mixed at room temperature, briefly immersed in hydrochloric acid to form composite droplets, and then dispersed ultrasonically and sprayed with Pt on the glass sheet to form a Janus structure and optimize the proportion of doped precious metals. and craftsmanship to increase motor activity.

Benefits of technology

It effectively increases the movement speed of micro-nano motors, increases movement efficiency by 60% to 100%, and obtains higher activity and suitable size through process optimization, simplifying the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118768561A_ABST
    Figure CN118768561A_ABST
Patent Text Reader

Abstract

The invention discloses a gallium-based liquid alloy micro-nano motor and a preparation method thereof.The preparation method comprises the steps that liquid Ga powder and Au powder are stirred and mixed to be uniform at the room temperature, the mixture is temporarily soaked in hydrochloric acid to enable Au and Ga to be compounded, then ultrasonic scattering is conducted, LM-MNMs particles are obtained and laid on a clean carrier, Pt is sprayed in a sputtering mode, the particle size of the LM-MNMs particles is 1-5 micrometers, and the Pt content of the LM-MNMs particles is 1-5 micrometers. The obtained gallium-based liquid alloy micro-nano horse forms a Janus structure, the self-driving performance is changed by optimizing the proportion of doped precious metal and the technology, the movement speed of the micro-nano motor is increased, the preparation process is not complex, and the equipment requirement is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of alloy materials, and in particular relates to a gallium-based liquid alloy micro-nano motor and a preparation method thereof. Background Art

[0002] In a general Pt-based catalytic system, as the concentration of hydrogen peroxide increases, the catalytic decomposition rate will reach a saturation value. The catalytic decomposition rate can be characterized by the current density during the catalytic reaction. When liquid metal (Ga) is introduced, the catalytic decomposition rate tends to disappear at the saturation rate point as the concentration of H2O2 increases. Until the concentration of H2O2 reaches saturation, the Pt catalytic decomposition rate has no tendency to decrease, and is always in a state of linear growth with the increase of H2O2 concentration (Y.Wang., W.Duan., C.Zhou., et al. Phoretic Liquid Metal Micro Nanomotors as Intelligent Filler for Targeted Microwelding. Advanced Materials: 2019, 31, 1905067.). This is a new phenomenon brought about by Ga@Pt micro-nanomotors, which allows micro-nanomotors to spontaneously enrich in the high concentration area of ​​H2O2. At the same time, Ga itself is also a carrier with good biocompatibility and excellent modifiability, and has great potential applications in biological drug delivery applications.

[0003] In the existing technology, the movement speed of Ga@Pt micro-nano motor itself is not fast, and the most suitable manufacturing size has not been confirmed in the preparation process. If the size is too small, the difficulty of subsequent modification will increase, and if the size is too large, the movement performance will be difficult to improve and the activity will be insufficient. Summary of the invention

[0004] In view of the deficiencies in the prior art, the main purpose of the present invention is to provide a gallium-based liquid alloy micro-nano motor, form a Janus structure, change the self-driving performance, and thus increase the movement speed of the micro-nano motor.

[0005] Another object of the present invention is to provide a method for preparing the gallium-based liquid alloy micro-nano motor, and to optimize the ratio and process of doping with precious metals to improve the movement activity of the Ga-based liquid alloy micro-nano motor.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] In the first aspect, the present invention proposes a method for preparing a gallium-based liquid alloy micro-nano motor, comprising: stirring and mixing liquid Ga and Au powder evenly at room temperature, briefly immersing in hydrochloric acid to allow Au and Ga to recombine, and then ultrasonically breaking up to obtain LM-MNMs particles, spreading them on a clean carrier and spraying Pt to obtain the motor.

[0008] Preferably, the particle size of the LM-MNMs particles is 1-5 μm, more preferably 3 μm.

[0009] Preferably, the method for preparing the gallium-based liquid alloy micro-nano motor comprises the following steps:

[0010] (1) Pure Ga and nano-Au powders are mixed and doped according to a ratio, and mechanically stirred to obtain a mixture;

[0011] (2) the mixture is completely immersed in hydrochloric acid, and after the mixture is completely formed into spherical droplets, excess hydrochloric acid is absorbed to obtain liquid metal composite droplets;

[0012] (3) The liquid metal composite droplets are first washed with ethanol for more than three times, and then immersed in ethanol for probe ultrasonic dispersion to obtain a LM-MNMs ethanol suspension;

[0013] (4) The glass slide was first cleaned with ethanol, then pretreated with O2 plasma, and then LM 2.5-10 mg / cm 2 The LM-MNMs ethanol suspension is spread on the glass sheet in a ratio of , to form a monolayer of particles, and then the glass sheet is placed in a vacuum environment until the ethanol evaporates naturally;

[0014] (5) Taking out the glass sheet, sputtering and spraying Pt on it in a Pt environment, and then placing it in clean water for water bath ultrasound, collecting the particles in water and storing them, thereby obtaining a gallium-based liquid alloy micro-nanomotor suspension.

[0015] More preferably, in step (1), the purity of Ga is greater than 99.999%, the particle size of the nano-Au powder is not greater than 500 nm, the purity is 99.9%, and the mass ratio of Au to Ga is 0.1 to 1:100.

[0016] More preferably, in step (1), the mechanical stirring time is 3 to 8 minutes, and the amount of the mixed powder prepared at one time does not exceed 5 g.

[0017] More preferably, in step (2), the concentration of the hydrochloric acid is 2 mol / L.

[0018] More preferably, in step (3), the power of the probe ultrasound is 300 W, and the dispersion time is 1 to 5 min, more preferably 3 min.

[0019] More preferably, in step (5), the time of sputtering spraying Pt is 100 to 200 s, and the power of water bath ultrasound is less than 80 W.

[0020] In a second aspect, the present invention further provides a gallium-based liquid alloy micro-nano motor, which is prepared by the preparation method of the gallium-based liquid alloy micro-nano motor.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. By doping a small amount of Au and pre-alloying it with Ga, its self-driving performance is changed, and the movement speed of the micro-nano motor is effectively improved. The efficiency can be increased by 60% to 100%. The preparation process is not complicated and the equipment requirements are low.

[0023] 2. The process of preparing gallium-based liquid alloy micro-nanomotors of the present invention is optimized, wherein the ultrasonic dispersion time of the probe directly affects the basic size of LM-MNMs, the proportion of the doped Au component directly affects the activity enhancement ability of LM-MNMs, and the LM-MNMs ethanol suspension is spread on a glass sheet to form a single layer of particles, which can obtain the Janus structure of the gallium-based liquid alloy micro-nanomotor, which is the prerequisite for allowing the micro-nanomotor to move. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Flow chart of the preparation process of gallium-based liquid alloy micro-nanomotor in the embodiment.

[0025] Figure 2 3 is a morphology distribution diagram of the gallium-based liquid alloy micro-nano motor in the embodiment.

[0026] Figure 3 This is the particle size distribution diagram of the gallium-based liquid alloy micro-nanomotor after ultrasound in the embodiment.

[0027] Figure 4 : This is the XRD diagram of the gallium-based liquid alloy micro-nano motor in the embodiment.

[0028] Figure 5 It is the DSC graph of the gallium-based liquid alloy micro-nano motor in the embodiment.

[0029] Figure 6 : It is the Zeta potential diagram of the gallium-based liquid alloy micro-nano motor in the embodiment.

[0030] Figure 7 This is a comparison chart of the self-electrophoretic propulsion speed of 0.5% Au-doped gallium-based liquid alloy micro-nanomotor in different concentrations of H2O2 in the embodiment. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention will be described in detail below in combination with the embodiments of the present invention and the accompanying drawings. However, the following embodiments are only used to understand the present invention and cannot limit the present invention.

[0032] Example 1

[0033] This embodiment follows Figure 1 The process flow shown is to prepare a gallium-based liquid alloy micro-nano motor, and the steps are as follows:

[0034] (1) Pure Ga (>99.999%) and nano-Au powder (≤500nm, 99.9%) were mixed at a mass ratio of 0.5% (Au:Ga=0.5%), and mechanically stirred for 5 min (the amount prepared at one time should not exceed 5 g).

[0035] (2) Add 2 mol / L hydrochloric acid to the stirred mixture to completely immerse the mixture. After the mixture completely forms spherical liquid metal composite droplets, use a dropper to absorb the surrounding hydrochloric acid.

[0036] (3) After washing the liquid metal composite droplet with ethanol (>99%) for more than three times, the droplet is immersed in ethanol.

[0037] (4) The liquid metal composite droplets were dispersed by probe ultrasound (300 W) for 3 min. The particle size obtained by the dispersion was controlled to be about 3 μm, and an ethanol suspension of LM-MNMs was obtained.

[0038] (5) Take a glass slide, wash it twice with ethanol, pre-treat it with O2 plasma for more than 3 minutes, and then use LM 2.5-10 mg / cm 2 The suspension was spread out in a proportion of to form a single layer of particles.

[0039] (6) Place the glass slide in a vacuum environment and wait for the ethanol to evaporate naturally.

[0040] (7) A glass sheet with a single layer of LM-MNMs on its surface was sputter-coated with Pt for 150 s in a Pt environment using a sputtering machine (Kyky Technology, SBC-12).

[0041] (8) The glass sheet after spraying with Pt is placed in clean water, and the particles are collected into a small amount of water by water bath ultrasonic method (<80W) to obtain a gallium-based liquid alloy micro-nanomotor suspension.

[0042] The characterization results of the gallium-based liquid alloy micro-nano motor prepared in Example 1 are as follows: Figures 2 to 7 As shown in Figure 2, the electrophoretic propulsion speed of the gallium-based liquid alloy micro-nanomotor doped with 0.5% Au metal in different H2O2 concentrations is compared. Figure 7 shown.

[0043] Similarly, metal Ag and Cu can also be doped to prepare gallium-based liquid alloy micro-nano motors. According to tests, doping with precious metal elements Au and Ag can improve the movement efficiency of Ga-based liquid alloy micro-nano motors, with the improvement rate of Au being 60% to 100% and Ag being around 20%.

[0044] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a gallium-based liquid alloy micro-nano motor, It is characterized in that include: Liquid Ga and Au powder are stirred and mixed evenly at room temperature, and briefly immersed in hydrochloric acid to allow Au and Ga to recombine, and then ultrasonically dispersed to obtain LM-MNMs particles, which are then spread on a clean carrier and sputter-sprayed with Pt.

2. The method for preparing the gallium-based liquid alloy micro-nano motor according to claim 1, It is characterized in that The particle size of the LM-MNMs particles is 1 to 5 μm.

3. The method for preparing the gallium-based liquid alloy micro-nano motor according to claim 1 or 2, It is characterized in that The method for preparing the gallium-based liquid alloy micro-nano motor comprises the following steps: (1) Pure Ga and nano-Au powders are mixed and doped according to a ratio, and mechanically stirred to obtain a mixture; (2) the mixture is completely immersed in hydrochloric acid, and after the mixture is completely formed into spherical droplets, excess hydrochloric acid is absorbed to obtain liquid metal composite droplets; (3) The liquid metal composite droplets are first washed with ethanol for more than three times, and then immersed in ethanol for probe ultrasonic dispersion to obtain a LM-MNMs ethanol suspension; (4) The glass slide was first cleaned with ethanol and then with O 2 Plasma pretreatment, then LM 2.5~10mg / cm 2 The LM-MNMs ethanol suspension is spread on the glass sheet in a ratio of , to form a monolayer of particles, and then the glass sheet is placed in a vacuum environment until the ethanol evaporates naturally; (5) Taking out the glass sheet, sputtering and spraying Pt on it in a Pt environment, and then placing it in clean water for water bath ultrasound, collecting the particles in water and storing them, thereby obtaining a gallium-based liquid alloy micro-nanomotor suspension.

4. The method for preparing the gallium-based liquid alloy micro-nano motor according to claim 3, It is characterized in that In step (1), the purity of Ga is greater than 99.999%, the particle size of the nano Au powder is no greater than 500 nm, the purity is 99.9%, and the mass ratio of Au to Ga is 0.1 to 1:

100.

5. The method for preparing the gallium-based liquid alloy micro-nano motor according to claim 3, It is characterized in that In step (1), the mechanical stirring time is 3 to 8 minutes, and the amount of the mixed powder prepared at one time does not exceed 5 g.

6. The method for preparing the gallium-based liquid alloy micro-nano motor according to claim 3, It is characterized in that In step (2), the concentration of the hydrochloric acid is 2 mol / L.

7. The method for preparing the gallium-based liquid alloy micro-nano motor according to claim 3, It is characterized in that In step (3), the power of the probe ultrasound is 300 W, and the dispersion time is 1 to 5 minutes.

8. The method for preparing the gallium-based liquid alloy micro-nano motor according to claim 3, It is characterized in that In step (5), the sputtering spraying time of Pt is 100 to 200 seconds, and the power of water bath ultrasound is less than 80W.

9. A gallium-based liquid alloy micro-nano motor, It is characterized in that The gallium-based liquid alloy micro-nano motor is prepared by the preparation method of any one of claims 1 to 8.

Citation Information

Patent Citations

  • Preparing method for spherical micro-nano motor with alkali liquor as fuel drive

    CN110094314A

  • Magnetic control self-driven liquid metal micromotor and preparation method and application thereof

    CN113012887A

  • Functionalized enzyme-powered nanomotors

    EP3663257A1

  • Low melting gallium alloy

    JP1998158774A