Aluminum member, aluminum resin composite, and method for producing aluminum resin composite

By forming nanoscale protrusions on the surface of the aluminum component and irradiating it with pulsed laser, the joint strength and acid resistance and hydrofluoric acid resistance of the aluminum resin composite are improved, and the acid resistance and hydrofluoric acid resistance of the aluminum resin composite in the existing technology are solved. The problem of insufficient acidity.

CN118769634AActive Publication Date: 2024-10-15PRIME PLANET ENERGY & SOLUTIONS INC +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410297530.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-10
Filing Date
2024-03-15
Publication Date
2024-10-15
Estimated Expiration
2044-03-15

AI Technical Summary

Technical Problem

The acid resistance and hydrofluoric acid resistance of existing aluminum resin composites during bonding are not high, resulting in separation problems between the resin component and the aluminum component, and insufficient joint strength.

Method used

By forming nanoscale protrusions with a diameter and height of less than 1 μm on the surface of the aluminum component, including amorphous alumina and α-alumina, and using pulse laser irradiation to form mesh-like protrusions, the bonding strength between the resin component and the aluminum component is improved. and resistance to acid and hydrofluoric acid.

Benefits of technology

Significantly improves the joint strength and acid resistance and hydrofluoric acid resistance of the resin component and the aluminum component, prevents separation in hydrochloric acid or lithium hexafluorophosphate non-aqueous electrolyte, and enhances the stability of the composite.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118769634A_ABST
    Figure CN118769634A_ABST
Patent Text Reader

Abstract

The invention relates to an aluminum member, an aluminum resin composite, and a method for manufacturing the aluminum resin composite. Provided are an aluminum member having excellent bonding strength, an aluminum resin composite, and a method for producing the aluminum resin composite. On the surface of an aluminum member (lid member (30), positive electrode terminal member (50)) comprising metallic aluminum, nano-scale protrusions (lid upper surface protrusion layer (F11), lid lower surface protrusion layer (F21), terminal side surface protrusion layer (F31), and terminal lower surface protrusion layer (F41)) each having a diameter and a height less than 1 [mu] m are closely arranged. Amorphous alumina and alpha-alumina are contained in a base end portion connected to the surface of the member.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The technical field disclosed in this specification relates to an aluminum member, an aluminum-resin composite, and a method for producing the aluminum-resin composite. Background Art

[0002] An aluminum-resin composite that joins an aluminum member and a resin member is known. In order to improve the joining strength between the aluminum member and the resin member, the surface of the aluminum member is roughened in advance. As a related prior art, for example, Patent Document 1 can be cited.

[0003] In Patent Document 1, in order to obtain an aluminum-resin composite, an aluminum member is first immersed in an etchant to roughen the surface of the aluminum member. As a result of the roughening treatment, fine irregularities are formed on the surface of the aluminum member.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2018-164989 Summary of the invention

[0007] Problems to be solved by the invention

[0008] When a conventional aluminum-resin composite is immersed in a liquid obtained by adding water to a non-aqueous electrolyte containing lithium hexafluorophosphate, the resin component is sometimes separated from the aluminum component. The reason is described below. Generally, a very thin oxide film is formed on the surface of the aluminum component. Therefore, in the aluminum-resin composite, the resin component is bonded to the aluminum component via the oxide film. In addition, hydrogen fluoride is generated in the above-mentioned liquid. Therefore, if the aluminum-resin composite is immersed in the above-mentioned liquid, the oxide film is decomposed by the hydrogen fluoride in the liquid. As a result, the resin component is separated from the aluminum component. In addition, when the aluminum-resin composite is immersed in hydrochloric acid, the oxide film is also decomposed by the hydrogen chloride in the liquid, and the resin component is separated from the aluminum component.

[0009] Therefore, it is believed that the acid resistance and hydrofluoric acid resistance of the previous aluminum resin composite are not high. In other words, the bonding strength of the bonding portion when the aluminum component and the resin component are bonded is insufficient. Therefore, it is hoped that the bonding strength of the bonding portion can be further improved.

[0010] The present invention has been made in view of the above-mentioned actual situation, and an object of the present invention is to provide an aluminum member, an aluminum-resin composite, and a method for producing the aluminum-resin composite, which are excellent in the bonding strength of the bonding portion when bonding with a resin member.

[0011] Means for solving problems

[0012] An aluminum component of one solution of the present invention which aims to solve the above-mentioned problems is a component made of metallic aluminum, on the surface of which nanoscale protrusions with a diameter and height of less than 1 μm are densely arranged, and the protrusions contain amorphous aluminum oxide and α-aluminum oxide at the base end connected to the surface of the component.

[0013] According to the aluminum component of the present invention, nanometer-level protrusions with diameters and heights of less than 1 μm are closely arranged on the surface of the component, so that the bonding strength of the joint portion when the resin component and the aluminum component are joined is improved by utilizing the anchoring effect. Furthermore, in the protrusion, the base end portion connected to the component surface contains not only amorphous aluminum oxide but also α-aluminum oxide with excellent chemical stability, so that the acid resistance and hydrofluoric acid resistance of the joint portion, and further the difficulty of separation of the resin component when immersed in hydrochloric acid or a liquid in which water is added to a non-aqueous electrolyte containing lithium hexafluorophosphate, are improved.

[0014] Moreover, another aspect of the present invention is an aluminum-resin composite in which a resin member is joined to the above-mentioned aluminum member.

[0015] Furthermore, according to another embodiment of the present invention, there is provided a method for manufacturing the above-mentioned aluminum resin composite, comprising: a protrusion forming process, wherein laser irradiation is performed on the surface of the component before the protrusion is formed to form the protrusion on the surface of the component; and an insert molding process, wherein, after the protrusion forming process, insert molding is used to form the resin component on the surface of the component. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a perspective view of a battery according to an embodiment.

[0017] Figure 2 for Figure 1 AA cross-section diagram.

[0018] Figure 3 A three-dimensional diagram of a positive terminal component.

[0019] Figure 4 For Figure 1 A three-dimensional view of a unit component extracted from a battery.

[0020] Figure 5A for Figure 4 BB cross-section diagram.

[0021] Figure 5B for Figure 4 CC cross-section diagram.

[0022] Fig. 6AIt is an explanatory diagram for explaining the bonding region between the upper surface of the cover member and the positive electrode resin member, and the region on the upper surface of the cover member that has been subjected to a roughening treatment.

[0023] Figure 6B It is an explanatory diagram for explaining the bonding region between the lower surface of the cover member and the positive electrode resin member, and the region on the lower surface of the cover member that has been subjected to a roughening treatment.

[0024] Fig. 7A It is an explanatory diagram for explaining a joining region between a side surface of a part of the positive electrode terminal member and the positive electrode resin member, and a region on the side surface of a part of the positive electrode terminal member that has been subjected to a roughening treatment.

[0025] Figure 7B It is an explanatory diagram for explaining the bonding region between the lower surface of the long straight portion of the positive electrode terminal member and the positive electrode resin member, and the region on the lower surface of the long straight portion of the positive electrode terminal member that has been roughened.

[0026] Figure 8 This is an image showing that the surface of an aluminum member is actually irradiated with pulse laser under the same conditions as the pulse laser irradiation of the roughened area, and a large number of protrusions at the nanoscale level are formed on the member surface and are densely arranged in a mesh shape.

[0027] Fig.9A This is an enlarged projection image of the cross-section sample obtained using TEM-EELS.

[0028] Fig. 9B A mapping image of chemical state A (chemical state analysis result) is shown.

[0029] Fig. 9C A mapping image of chemical state B (chemical state analysis result) is shown.

[0030] Fig.9D A mapping image showing chemical state C (chemical state analysis result) is shown.

[0031] Fig. 10A This is a graph of the EELS spectrum of Al-related compounds obtained from an analytical company.

[0032] Fig. 10B This is a graph of the EELS spectrum obtained from the cross-section sample.

[0033] Fig.11 This is a flow chart of a method for manufacturing a battery according to an embodiment.

[0034] Fig. 12A FIG. 1 is a diagram schematically showing a roughening process for the roughened area on the lower surface of the cover.

[0035] Fig. 12BA diagram schematically showing the roughening process of the roughened area on the side surface of the terminal.

[0036] Fig.13 A diagram schematically illustrating an insert molding process.

[0037] Fig.14A This is a table showing the results of the acid resistance test.

[0038] Fig. 14B This is a table showing the results of the hydrofluoric acid resistance test.

[0039] Description of Reference Numerals

[0040] 1…battery, 10…housing, 20…main body member, 30…cover member, 33h…positive electrode insertion hole, 34h…negative electrode insertion hole, 50…positive electrode terminal member, 60…negative electrode terminal member, 70…positive electrode resin member, 80…negative electrode resin member, 100…protrusion, E1…cover upper surface bonding region, E2…cover lower surface bonding region, E3…terminal side bonding region, E4…terminal lower surface bonding region, F1…cover upper surface roughened region, F2…cover lower surface roughened region, F3…terminal side roughened region, F4…terminal lower surface roughened region DETAILED DESCRIPTION

[0041] Hereinafter, the embodiment of the present invention will be described with reference to the accompanying drawings. The battery 1 constituting the aluminum resin composite of the present invention is an example of a storage device, specifically, a square and sealed lithium-ion secondary battery mounted on vehicles such as hybrid vehicles, plug-in hybrid vehicles and electric vehicles. It should be noted that, hereinafter, the reference numerals X, Y, and Z related to the directions in the accompanying drawings limit the directions, indicating the left-right direction, the front-back direction, and the up-down direction. In addition, the reference numerals U, D, L, R, F, and B recorded at the positions of the arrows related to the directions limit the positions, indicating the upper side, the lower side, the left side, the right side, the front side, and the rear side. However, these directions and positions are limited for the convenience of explanation. Therefore, there is no limitation on the direction of the battery 1 to be set.

[0042] [Battery composition]

[0043] Figure 1 It is a three-dimensional diagram of the battery 1. Figure 2 for Figure 1 AA section diagram in. Figure 1 and Figure 2 As shown, the battery 1 includes a case 10 that seals the interior, an electrode body 40 accommodated in the case 10 , an electrolyte 3 and an insulating holder 5 , and a positive terminal member 50 and a negative terminal member 60 connected to the electrode body 40 .

[0044] The housing 10 is generally flat and has a bottomed rectangular parallelepiped shape. The housing 10 is composed of a main body member 20 and a cover member 30. In the present embodiment, the housing 10 is made of aluminum. However, the material of the housing 10 may also be an aluminum-based metal other than aluminum such as an aluminum alloy. In addition, the material of the housing 10 may also be a metal other than aluminum-based metals such as an iron-based metal. Furthermore, the cover member 30, the positive terminal member 50, and the negative terminal member 60 are examples of aluminum members of the present invention.

[0045] The main body member 20 is a square tube with a bottom. In addition, the main body member 20 has an opening 21. In other words, the main body member 20 has: a rectangular plate-shaped bottom 12, a pair of front side parts 13 and rear side parts 14 vertically erected from the edge of the front side F and the edge of the rear side B of the bottom 12, and a pair of left side parts 15 and right side parts 16 vertically erected from the end of the left side L and the end of the right side R of the bottom 12. The shape of the opening 21 is a rectangle with the left-right direction X as the long side direction and the front-back direction Y as the short side direction. The shape of the bottom 12 is a rectangular plate with the left-right direction X as the long side direction and the front-back direction Y as the short side direction. The shape of the front side part 13 and the rear side part 14 is a rectangular plate with the left-right direction X as the long side direction and the up-down direction Z as the short side direction. The shape of the left side part 15 and the right side part 16 is a rectangular plate with the up-down direction Z as the long side direction and the front-back direction Y as the short side direction.

[0046] Furthermore, the height (length in the vertical direction Z) of the front side portion 13 and the rear side portion 14 is the same as the height (length in the vertical direction Z) of the left side portion 15 and the right side portion 16. In addition, the height (length in the vertical direction Z) of the front side portion 13 and the rear side portion 14 and the length in the horizontal direction X of the front side portion 13 and the rear side portion 14 are considerably longer than the length in the front-back direction Y of the left side portion 15 and the right side portion 16. Therefore, hereinafter, with respect to the housing 10, the main body member 20 and the cover member 30, the horizontal direction X is sometimes referred to as the "length direction", the front-back direction Y is referred to as the "width direction", and the vertical direction Z is referred to as the "height direction".

[0047] The cover member 30 closes the opening 21 of the main body member 20. Specifically, the peripheral edge of the cover member 30 is laser welded to the top end of the upper side U of the front side portion 13, the rear side portion 14, the left side portion 15, and the right side portion 16 over the entire circumference. At the boundary portion between the top end of the main body member 20 and the peripheral edge of the cover member 30, a molten solidified portion 18 where the main body member 20 and the cover member 30 are melted and solidified is formed over the entire circumference by laser.

[0048] A safety valve 19 is provided slightly to the left L of the center of the cover member 30 in the left-right direction X. The safety valve 19 breaks and opens when the internal pressure of the housing 10 exceeds the valve opening pressure. A liquid injection hole 30k is formed slightly to the right R of the center of the cover member 30 in the left-right direction X, which penetrates the cover member 30 in the up-down direction Z. A sealing member 39 made of aluminum is fitted into the liquid injection hole 30k from the upper side U, thereby hermetically sealing the liquid injection hole 30k.

[0049] On one side of the cover member 30 in the left-right direction X ( Figure 1 , Figure 2 A positive electrode insertion hole 33h is formed near the end portion of the cover member 30 (the left side L in the figure) so as to penetrate the cover member 30 in the vertical direction Z. Figure 1 , Figure 2 Near the end portion (right side R in the middle), a negative electrode insertion hole 34h is formed that penetrates the cover member 30 in the up-down direction Z. The positive electrode insertion hole 33h and the negative electrode insertion hole 34h are formed into a rectangle with the left-right direction X as the long side direction and the front-back direction Y as the short side direction. In the positive electrode insertion hole 33h, the positive terminal member 50, which is longitudinally long as a whole (extending in one direction), is inserted from the upper side U along its length direction. In the negative electrode insertion hole 34h, the negative terminal member 60, which is longitudinally long as a whole (extending in one direction), is inserted from the upper side U along its length direction.

[0050] The positive electrode terminal member 50 is fixed to the cover member 30 via the positive electrode resin member 70 in a state of being insulated from the cover member 30. Therefore, the positive electrode terminal member 50 is supported by the cover member 30 via the positive electrode resin member 70. In the present embodiment, the positive electrode terminal member 50 is made of aluminum. However, the material of the positive electrode terminal member 50 can be appropriately set within the range that can be electrically connected to the positive electrode collector 41r of the electrode body 40 described later.

[0051] The negative electrode terminal member 60 is fixed to the cover member 30 via the negative electrode resin member 80 in a state of being insulated from the cover member 30. Therefore, the negative electrode terminal member 60 is supported by the cover member 30 via the negative electrode resin member 80. In the present embodiment, the negative electrode terminal member 60 is made of copper. However, the material of the negative electrode terminal member 60 can be appropriately set within the range that can be electrically connected to the negative electrode collector 42r of the electrode body 40 described later.

[0052] The electrode body 40 is a so-called "wound type" electrode body. In the electrode body 40, a strip-shaped positive electrode plate 41 and a strip-shaped negative electrode plate 42 are wound in a predetermined winding direction with a strip-shaped separator 43 sandwiched therebetween. As a result, the electrode body 40 as a whole is formed into a flat shape having horizontally long rectangular side surfaces extending in the vertical direction Z and the horizontal direction X at the front side F and the rear side B.

[0053] The positive electrode plate 41 has a collector foil (not shown) of the positive electrode and an active material layer (not shown) of the positive electrode carried by the collector foil. The collector foil of the positive electrode in the present embodiment is made of aluminum. However, the material of the collector foil of the positive electrode can be appropriately set within the range that can realize the function as the positive electrode of the lithium ion secondary battery. On the other hand, the negative electrode plate 42 has a collector foil (not shown) of the negative electrode and an active material layer (not shown) of the negative electrode carried by the collector foil. The collector foil of the negative electrode in the present embodiment is made of copper. However, the material of the collector foil of the negative electrode can be appropriately set within the range that can realize the function as the negative electrode of the lithium ion secondary battery.

[0054] In addition, a positive electrode collector portion 41r is formed in the electrode body 40. The positive electrode collector portion 41r is a portion where the collector foil of the positive electrode is exposed. The positive terminal lower side portion 52 of the positive terminal member 50 is bonded to the positive electrode collector portion 41r. Similarly, a negative electrode collector portion 42r is formed in the electrode body 40. The negative electrode collector portion 42r is a portion where the collector foil of the negative electrode is exposed. The negative terminal lower side portion 62 of the negative terminal member 60 is bonded to the negative electrode collector portion 42r. Therefore, the electrode body 40 is supported by the cover member 30 via the positive terminal member 50 and the negative terminal member 60.

[0055] Although detailed illustration is omitted, the positive electrode current collecting portion 41r is a portion protruding from the negative electrode plate 42 and the separator 43 in the axial direction of the electrode body 40, and only the positive electrode current collecting foil is wound. Similarly, the negative electrode current collecting portion 42r is a portion protruding from the positive electrode plate 41 and the separator 43 in the axial direction of the electrode body 40, and only the negative electrode current collecting foil is wound. In the present embodiment, the positive electrode current collecting portion 41r is formed at the end of the left side L of the electrode body 40. On the other hand, the negative electrode current collecting portion 42r is formed at the end of the right side R of the electrode body 40.

[0056] In addition, the electrode body 40 is separated from the bottom 12, the front side 13, the rear side 14, the left side 15 and the right side 16 of the main member 20 and the cover member 30 by a certain distance. Moreover, an insulating support 5 for reliably maintaining insulation is arranged between the electrode body 40 and the main member 20. As for the shape and material of the insulating support 5, as long as it can be arranged between the electrode body 40 and the main member 20 and the electrode body 40 can be insulated from the main member 20, it can be appropriately set. In the present embodiment, the insulating support 5 is composed of a strip film of polypropylene (PP) as a synthetic resin. In addition, the insulating support 5 is formed in a bag shape. Moreover, the bag-shaped insulating support 5 wraps the electrode body 40 in a state where the upper side U is open. That is, the insulating support 5 insulates the inner surface of the bottom 12, the front side 13, the rear side 14, the left side 15 and the right side 16 of the main member 20 and the outer surface of the electrode body 40 opposite to the main member 20.

[0057] The positive electrode resin member 70 is made of a thermoplastic resin, specifically, polyphenylene sulfide (PPS) in the present embodiment. Moreover, the positive electrode resin member 70 is joined to the cover member 30 and the positive terminal member 50, respectively. By joining the positive electrode resin member 70 to the cover member 30 and the positive terminal member 50, the cover member 30, the positive terminal member 50 and the positive electrode resin member 70 are integrated, and therefore, the battery 1 including the integrated product constitutes a composite formed of aluminum and resin. In addition, the positive electrode resin member 70 insulates the cover member 30 and the positive terminal member 50 while sealing them airtightly. That is, the positive electrode resin member 70 functions as an insulating member and a sealing member between the cover member 30 and the positive terminal member 50. Furthermore, the material of the positive electrode resin component 70 can be appropriately set as long as it can insulate the cover component 30 and the positive terminal component 50 while sealing them airtightly, and can also be joined to the cover component 30 and the positive terminal component 50 respectively. It can be other types of resins such as other types of thermoplastic resins, thermosetting resins, etc.

[0058] The negative electrode resin member 80 is made of a thermoplastic resin, specifically, polyphenylene sulfide (PPS) in the present embodiment. Moreover, the negative electrode resin member 80 is joined to the cover member 30 and the negative terminal member 60, respectively. By joining the negative electrode resin member 80 to the cover member 30 and the negative terminal member 60, the cover member 30, the negative terminal member 60 and the negative electrode resin member 80 are integrated, and therefore, the battery 1 including the integrated product constitutes a composite body formed by metal and resin. In addition, the negative electrode resin member 80 insulates the cover member 30 and the negative terminal member 60 while sealing them airtightly. That is, the negative electrode resin member 80 functions as an insulating member and a sealing member between the cover member 30 and the negative terminal member 60. Furthermore, the material of the negative electrode resin member 80 can be appropriately set as long as it can insulate the cover member 30 and the negative terminal member 60 while sealing them airtightly and can be joined to the cover member 30 and the negative terminal member 60 respectively. It can be other types of resins such as other types of thermoplastic resins, thermosetting resins, etc.

[0059] Next, the shape of the positive electrode terminal member 50 will be described. Figure 3 is a three-dimensional diagram of the positive terminal component 50. Figure 3 As shown, the positive terminal member 50 includes a positive terminal upper portion 51, a positive terminal lower portion 52, and a positive terminal intermediate portion 53. In the battery 1, the positive terminal upper portion 51 is relatively arranged on the upper side U, and the positive terminal lower portion 52 is relatively arranged on the lower side D.

[0060] The positive terminal upper side portion 51 has a constant L-shaped cross-sectional shape in one direction. As a detail of the cross-sectional shape of the positive terminal upper side portion 51, compared with one straight line portion of the L-shaped, the other straight line portion is longer. Therefore, the rectangular plate-shaped portion of the positive terminal upper side portion 51 corresponding to the longer straight line portion in the L-shaped cross-sectional shape is called "long straight line portion 51a", and the portion extending vertically from one edge of the long straight line portion 51a is called "short straight line portion 51b".

[0061] It should be noted that, in the following description of the positive terminal member 50, for convenience, the symbol for defining the direction is used. Figure 3 The reference numerals O, P, and Q shown in the figure. The reference numerals O, P, and Q respectively represent “the direction in which the L-shaped cross-sectional shape of the positive terminal upper side portion 51 extends constantly”, “the direction along the straight line of the long straight line portion 51a”, and “the direction along the straight line of the short straight line portion 51b”. In addition, the reference numerals O, P, and Q indicating directions are hereinafter referred to as “the first direction O”, “the second direction P”, and “the third direction Q”, respectively. Furthermore, in the description of the positive terminal member 50, the side in the third direction Q where the positive terminal upper side portion 51 is arranged is sometimes referred to as the “upper side”, and the side in the third direction Q where the positive terminal lower side portion 52 is arranged is sometimes referred to as the “lower side”.

[0062] The lower side portion 52 of the positive terminal is formed perpendicularly to the long straight portion 51a as a whole. The shape of the lower side portion 52 of the positive terminal is a rectangular plate with the third direction Q as the long side direction and the second direction P as the short side direction. In addition, in the first direction O, a part of the lower side portion 52 of the positive terminal converges to the inner side of the upper side portion 51 of the positive terminal, and another part overflows to the outer side of the upper side portion 51 of the positive terminal. Furthermore, in the second direction P, a part of the lower side portion 52 of the positive terminal converges to the inner side of the upper side portion 51 of the positive terminal, and another part overflows to the outer side of the upper side portion 51 of the positive terminal.

[0063] The positive terminal middle portion 53 is a crank shape as a whole, connecting the positive terminal upper side portion 51 and the positive terminal lower side portion 52. The shape of the positive terminal middle portion 53 seen from the second direction P is a rectangle with the first direction O as the long side direction and the third direction Q as the short side direction. In addition, the length of the first direction O of the positive terminal middle portion 53 is longer than the length of the first direction O of the positive terminal lower side portion 52. Moreover, the side surface of the positive terminal lower side portion 52 on the side overflowing to the outside of the positive terminal upper side portion 51 in the first direction O is continuous with the side surface of the positive terminal middle portion 53 on the same side in the first direction O.

[0064] In addition, two surfaces of the positive terminal middle portion 53 that are perpendicular to the second direction P near the connection with the short straight portion 51b and two surfaces of the short straight portion 51b that are perpendicular to the second direction P are formed on the same plane. Hereinafter, the portion of the positive terminal middle portion 53 that is formed on the same plane with the two surfaces of the short straight portion 51b that are perpendicular to the second direction P is referred to as the "upper continuous portion 53a". Moreover, the surface 51x on the side of the positive terminal upper side portion 51 including the short straight portion 51b in the second direction P where the positive terminal lower side portion 52 is arranged is in the same plane as the surface 53ax on the same side of the upper continuous portion 53a. In addition, a curved portion 53b is formed on the side of the upper continuous portion 53a that is opposite to the short straight portion 51b in the third direction Q, and the curved portion 53b is bent in a crank shape toward the outside of the positive terminal upper side portion 51 along the second direction P.

[0065] In the present embodiment, the shape of the negative terminal member 60 is the same as that of the positive terminal member 50. Therefore, the description using the perspective view of the negative terminal member 60 is omitted, and the negative terminal member 60 has a negative terminal upper side portion 61, a negative terminal lower side portion 62, and a negative terminal middle portion 63 corresponding to the positive terminal upper side portion 51, the positive terminal lower side portion 52, and the positive terminal middle portion 53, similarly to the positive terminal member 50.

[0066] Next, the bonding structure of the positive electrode resin member 70 , the cover member 30 , and the positive electrode terminal member 50 , and the roughening treatment of the cover member 30 and the positive electrode terminal member 50 will be described. Figure 4 To constitute Figure 1 and Figure 2 A portion of the battery 1 shown in FIG. 1 is a diagram in which a unit member 1A composed of an integrated cover member 30 , a positive electrode terminal member 50 and a positive electrode resin member 70 , and a negative electrode terminal member 60 and a negative electrode resin member 80 is extracted and shown in a perspective view. Figure 5A for Figure 4 BB cross-section diagram, Figure 5B for Figure 4 CC cross-section diagram. Fig. 6A , 6B It is an explanatory diagram for explaining the bonding region between the cover member 30 and the positive electrode resin member 70 and the region in the cover member 30 subjected to the roughening treatment. Fig. 7A , 7B It is an explanatory diagram for explaining the joining region between the positive electrode terminal member 50 and the positive electrode resin member 70 and the region in the positive electrode terminal member 50 subjected to a roughening treatment.

[0067] The positive electrode terminal member 50 is fixed to the cover member 30 via the positive electrode resin member 70 in a state where the first direction O is parallel to the left-right direction X and the positive electrode terminal lower side portion 52 is arranged on the rear side B. On the other hand, the negative electrode terminal member 60 is fixed to the cover member 30 via the negative electrode resin member 80 in a state where the first direction O is parallel to the left-right direction X and the negative electrode terminal lower side portion 62 is arranged on the front side F.

[0068] The upper surface 51ax of the long straight portion 51a is exposed on the upper side U. In addition, in the up-down direction Z, the upper surface 30x of the cover member 30 and the lower surface 51ay of the long straight portion 51a are arranged at approximately the same position. Furthermore, in the up-down direction Z, the lower surface 51by of the short straight portion 51b is arranged at a position slightly lower than the lower surface 30y of the cover member 30. Furthermore, when viewed from above (from the upper side U to the lower side D), the long straight portion 51a of the positive terminal member 50 inserted into the positive electrode insertion hole 33h is completely retracted into the inside of the positive electrode insertion hole 33h. Moreover, in the left-right direction X and the front-back direction Y, the long straight portion 51a is arranged at approximately the center of the positive electrode insertion hole 33h.

[0069] The positive electrode resin member 70 is formed from the upper end of the positive terminal upper side portion 51 to slightly above the lower end of the upper continuous portion 53a in the vertical direction Z. The positive electrode resin member 70 is used to seal the lid member 30 and the positive terminal member 50 in an airtight manner. As described later, in the present embodiment, the positive electrode resin member 70 is formed integrally by insert molding, but for convenience, the portion of the positive electrode resin member 70 above the upper surface 30x of the lid member 30 is referred to as the "positive electrode resin upper side portion 71", the portion below the lower surface 30y of the lid member 30 is referred to as the "positive electrode resin lower side portion 72", and the portion between the upper surface 30x and the lower surface 30y of the lid member 30, that is, the portion filled in the positive electrode insertion hole 33h is referred to as the "positive electrode resin middle portion 73".

[0070] The positive electrode resin upper portion 71 includes a positive electrode resin upper frame-shaped portion 71 a surrounding the long straight portion 51 a over the entire circumference, and a positive electrode resin upper protruding portion 71 b connected to the positive electrode resin upper frame-shaped portion 71 a .

[0071] The positive electrode resin upper frame-shaped portion 71a is formed into a rectangular frame shape when viewed from above. The distance from the inner edge to the outer edge of each straight portion of the positive electrode resin upper frame-shaped portion 71a, that is, the first width W1, is approximately the same. The positive electrode resin upper protrusion 71b is formed to protrude toward the right side R from a part of the range of the approximate center of the straight portion formed on the right side R of the positive electrode resin upper frame-shaped portion 71a. The shape of the positive electrode resin upper protrusion 71b is a rectangular plate with the left-right direction X as the long side direction and the front-to-back direction Y as the short side direction. The length of the positive electrode resin upper protrusion 71b in the left-right direction X and the length in the front-to-back direction Y are longer than the first width W1. Furthermore, the positive electrode resin upper protrusion 71b is located at a gate member GT (refer to Fig.13 ) part.

[0072] In addition, the positive electrode resin upper frame-shaped portion 71a is joined to a rectangular ring-shaped cover upper surface frame-shaped joining area E11 that surrounds the entire outer side surface of the long straight portion 51a and the edge of the positive electrode insertion hole 33h in the upper surface 30x of the cover member 30. The distance from the inner edge to the outer edge of each straight portion of the cover upper surface frame-shaped joining area E11, that is, the second width W2 is substantially the same. In addition, the positive electrode resin upper side protrusion 71b is joined to the upper surface of the cover member 30 over the entire bottom surface.

[0073] It should be noted that the area of ​​the upper surface 30x of the cover member 30 that is bonded to the positive electrode resin upper side protrusion 71b is hereinafter referred to as the "cover upper surface rectangular bonding area E12". The cover upper surface rectangular bonding area E12 is formed to protrude to the right side R from a part of the range of the substantially center of the straight line portion of the right side R in the cover upper surface frame-shaped bonding area E11. That is, the cover upper surface frame-shaped bonding area E11 and the cover upper surface rectangular bonding area E12 are connected to constitute the bonding area of ​​the upper surface 30x of the cover member 30 with the positive electrode resin member 70. Therefore, the cover upper surface frame-shaped bonding area E11 and the cover upper surface rectangular bonding area E12 are collectively referred to as the "cover upper surface bonding area E1".

[0074] The positive electrode resin lower side portion 72 is formed as a rectangular plate with the left-right direction X as the long side direction and the front-back direction Y as the short side direction. Inside the positive electrode resin lower side portion 72, the portion of the positive electrode terminal member 50 that overlaps with the positive electrode resin lower side portion 72 in the vertical direction Z is completely buried. Therefore, the positive electrode resin lower side portion 72 is integrally joined to the outer side surface of the portion of the positive terminal member 50 that overlaps with the short straight line portion 51b and the upper continuous portion 53a in the vertical direction Z.

[0075] In addition, the positive electrode resin lower side portion 72 is joined to the rectangular ring-shaped cover lower surface joint area E2 that surrounds the edge of the positive electrode insertion hole 33h in the lower surface 30y of the cover member 30 over the entire circumference. The distance from the inner edge to the outer edge of each straight line portion of the cover lower surface joint area E2 is substantially the same on the front side F and the rear side B, and substantially the same on the left side L and the right side R. Moreover, compared with the third width W3, which is the distance from the inner edge to the outer edge of the straight line portion on the front side F and the rear side B, the fourth width W4, which is the distance from the inner edge to the outer edge of the straight line portion on the left side L and the right side R, is wider.

[0076] The positive electrode resin middle portion 73 is connected to the positive electrode resin upper portion 71 and the positive electrode resin lower portion 72. In addition, the positive electrode resin middle portion 73 is filled in the positive electrode insertion hole 33h. Therefore, the positive electrode resin middle portion 73 is joined to the inner side surface of the positive electrode insertion hole 33h of the cover member 30 throughout the entire circumference. Furthermore, inside the positive electrode resin middle portion 73, the portion of the short straight portion 51b of the positive terminal member 50 that overlaps with the positive electrode resin middle portion 73 in the vertical direction Z is completely buried. Therefore, the positive electrode resin middle portion 73 is integrally joined to the outer side surface of the portion of the short straight portion 51b of the positive terminal member 50 that overlaps in the vertical direction Z.

[0077] Furthermore, the outer side surface of the long straight portion 51a of the positive terminal member 50 is entirely joined to the positive electrode resin upper frame-shaped portion 71a. In addition, in the positive terminal member 50, the outer side surface of the portion of the short straight portion 51b that overlaps with the positive electrode resin middle portion 73 and the positive electrode resin lower portion 72 in the up-down direction Z is entirely joined to the positive electrode resin middle portion 73 and the positive electrode resin lower portion 72. Furthermore, the outer side surface of the portion of the upper continuous portion 53a of the positive terminal member 50 that overlaps with the positive electrode resin lower portion 72 in the up-down direction Z is entirely joined to the positive electrode resin lower portion 72. Therefore, the area of ​​the positive terminal member 50 that is joined to the positive electrode resin member 70 in the side surface that crosses the positive terminal upper portion 51 and the upper continuous portion 53a to become the same plane is referred to as the "terminal side joining area E3" (refer to Fig. 7A ). In addition, the entire lower surface 51ay of the long straight portion 51a on one side of the positive terminal lower side portion 52 formed in the third direction Q of the positive terminal member 50, that is, the area joined to the positive electrode resin member 70 is referred to as the "terminal lower surface joining area E4" (refer to Figure 7B ).

[0078] Thus, there are a plurality of bonding regions with the positive electrode resin member 70 in the cover member 30 and the positive electrode terminal member 50. In order to improve the sealing performance, a roughening treatment using pulsed laser irradiation is performed in a specific region of the cover member 30 and the positive electrode terminal member 50 including the bonding region with the positive electrode resin member 70. Therefore, the roughening treatment is described.

[0079] The roughening treatment is applied to the cover upper surface roughened area F1 which completely surrounds and contains the cover upper surface bonding area E1 in the upper surface 30x of the cover member 30, and the cover lower surface roughened area F2 which completely surrounds and contains the cover lower surface bonding area E2 in the lower surface 30y of the cover member 30. In addition, in the positive terminal member 50, the roughening treatment is applied to the terminal side surface roughened area F3 which completely surrounds and contains the terminal side surface bonding area E3 in the entire side surface which is in the same plane as that of the upper side portion 51 of the positive terminal and the upper side continuous portion 53a, and the terminal lower surface bonding area E4 itself, that is, the terminal lower surface roughened area F4.

[0080] The detailed conditions will be described later, and the roughening treatment of the cover upper surface roughening area F1, the cover lower surface roughening area F2, the terminal side roughening area F3, and the terminal lower surface roughening area F4 is performed by pulse laser irradiation. Moreover, in the cover upper surface roughening area F1, the cover lower surface roughening area F2, the terminal side roughening area F3, and the terminal lower surface roughening area F4, a large number of protrusions 100 are arranged in a mesh-like state in a dense state as a whole (arranged in a mesh-like state).

[0081] The so-called "a large number of protrusions are arranged in a dense state in a mesh shape" means that the protrusions 100 formed by pulse laser irradiation are arranged (standing in a forest) with a distance of at least less than the overall average value of the diameter of the protrusions between adjacent protrusions on the plane, and the gaps between the protrusions are also expanded two-dimensionally and connected to form a roughly grid shape. The roughly grid shape here includes planar shapes other than rectangles such as rhombuses, and is not particularly limited. In addition, the roughly grid shape can be uniform or uneven as a whole.

[0082] The protrusions 100 formed in the cover upper surface roughening region F1 and the cover lower surface roughening region F2 are products of fragmented particles generated by pulse laser irradiation on the surface of the cover member 30, which are combined in a beaded shape and extend in the height direction as a whole. Similarly, the protrusions 100 formed in the terminal side surface roughening region F3 and the terminal lower surface roughening region F4 are products of fragmented particles generated by pulse laser irradiation on the surface of the positive terminal member 50, which are combined in a beaded shape and extend in the height direction as a whole.

[0083] Furthermore, the so-called debris particles refer to particles with a diameter of less than 100 nm that fall on the surface near the pulse laser irradiation position and are formed by condensation of compounds formed by the reaction of metal vapor or metal atoms with atmospheric gas when the surface of a metal component is irradiated with a pulse laser to cause a part of the surface to evaporate explosively.

[0084] In addition, the entirety of the large number of protrusions 100 in the cover upper surface roughened region F1 is referred to as the "cover upper surface protrusion layer F11". Similarly, the entirety of the large number of protrusions 100 in the cover lower surface roughened region F2, the terminal side surface roughened region F3, and the terminal lower surface roughened region F4 are referred to as the "cover lower surface protrusion layer F21", "terminal side surface protrusion layer F31", and "terminal lower surface protrusion layer F41".

[0085] The diameter of a large number of protrusions 100 included in each protrusion layer F11 to F41 is 5 nm to 20 nm. In addition, the overall average value (average diameter) of the diameter of a large number of protrusions 100 included in each protrusion layer F11 to F41 is a nanometer level of less than 1 μm. "Nanometer level of less than 1 μm" is at the "nm" level, in other words, several nanometers to several hundred nanometers.

[0086] Furthermore, as an example of a method for calculating the average diameter of a large number of protrusions 100 contained in each protrusion layer F11 to F41, there is the following method. Initially, a cross-sectional sample of the joint portion of the cover member 30 and the positive terminal member 50 with the positive electrode resin member 70 is prepared using a predetermined cross-sectional sample preparation device (e.g., a cross-sectional polisher (registered trademark): manufactured by JEOL Ltd.). Next, the cross-sectional sample is observed using a field emission scanning electron microscope (FE-SEM). Then, the ridges of the protrusions 100 of the cover member 30 and the positive terminal member 50 in the cross-sectional sample are determined. Finally, based on the specific ridges, the average diameter of the large number of protrusions in the cross-sectional sample is measured.

[0087] The height of the large number of protrusions 100 contained in each protrusion layer F11 to F41 is 10 nm to 1000 nm. In addition, the overall average value (average height) of the height of the large number of protrusions 100 contained in each protrusion layer F11 to F41 is less than 1 μm in the nanometer level. However, the average height of the large number of protrusions 100 contained in each protrusion layer F11 to F41 is preferably 84 nm to 1000 nm.

[0088] Furthermore, as an example of a method for calculating the average height of a large number of protrusions 100 included in each protrusion layer F11 to F41, there is the following method. As this calculation method, a plate-shaped aluminum member is first prepared as a test piece. The test piece of the aluminum member is called an "average height test piece". Then, pulse laser irradiation is performed on the entire plane of the average height test piece under the same conditions as the pulse laser irradiation of each roughened area F1 to F4.

[0089] Next, a cross-sectional sample including a planar portion irradiated with a pulsed laser is prepared from the average height test piece using a predetermined cross-sectional sample preparation device (e.g., a cross-sectional polisher (registered trademark): manufactured by JEOL Ltd.). The cross-sectional sample is parallel to the thickness direction of the average height test piece. Next, a cross-sectional image of the cross-sectional sample is obtained using a scanning electron microscope (JEM ARM 200FDual-X: manufactured by JEOL Ltd.). The magnification of the cross-sectional image is 150,000 times.

[0090] Next, the cross-sectional area and bottom length of the protrusions in the cross-sectional image were measured using the image processing software "ImageJ". Then, the average height of the protrusions was calculated according to the following mathematical formula 1.

[0091] [Mathematical formula 1]

[0092] Average height of protrusions (nm) = cross-sectional area of ​​protrusions (nm 2 )÷base length (nm)

[0093] In fact, the surface of the aluminum component (component surface) was irradiated with pulse laser under the same conditions as the pulse laser irradiation of the roughening areas F1 to F4, and an image showing that a large number of protrusions at the nanometer level were formed on the component surface and were arranged in a dense mesh state is shown in FIG. Figure 8 .like Figure 8 As shown in FIG. 1 , a large number of protrusions with diameters and heights of nanometer level are arranged in a dense mesh-like state. Figure 8 The scale bar at the lower right corner of the lower image represents 30 nm.

[0094] Each protrusion layer F11 to F41 contains metallic aluminum, amorphous aluminum oxide, and α-aluminum oxide as a whole. Furthermore, at least the base end 100A of each protrusion layer F11 to F41, that is, the range from the base of the protrusion 100 to a height of 20 nm contains amorphous aluminum oxide and α-aluminum oxide.

[0095] The presence of metallic aluminum, amorphous aluminum oxide, and α-aluminum oxide in the protrusion 100 can be confirmed by elemental mapping. Specifically, first, a cross-sectional sample is prepared by the FIB (Focused Ion Beam) method from the surface of an aluminum component irradiated with a pulsed laser under the same conditions as the pulsed laser irradiation of the roughening areas F1 to F4. The cross-sectional sample contains the boundaries between the aluminum component and a large number of protrusions. Secondly, TEM-EELS (Transmission Electron Microscopy-Electron Energy Loss Spectroscopy) is used to obtain an enlarged projection image of the cross-sectional sample and the results of chemical state analysis.

[0096] Fig.9A This is an enlarged projection image of a cross-section sample obtained using TEM-EELS. Fig. 9B , 9C 9D is a mapping image of the chemical state contained in the cross-section sample obtained by TEM-EELS. Specifically, Fig. 9B To show the mapping image of chemical state A (chemical state analysis result), Fig. 9C To show the mapping image of chemical state B (chemical state analysis result), Fig.9D A mapping image showing chemical state C (chemical state analysis result) is shown.

[0097] Chemical state A is considered to be metallic aluminum, chemical state B is α-aluminum oxide, and chemical state C is considered to be amorphous aluminum oxide. These are based on the comparison of the EELS spectra of Al-related compounds obtained from an analytical company (Toray Research Center Co., Ltd.) in the past and the EELS spectra obtained from the cross-section sample this time. For reference, the spectra are shown in Fig. 10A , 10B .

[0098] Depend on Figure 9B to Figure 9D , the following can be inferred.

[0099] (1) In the protrusion 100 , metallic aluminum and aluminum oxide (amorphous aluminum oxide and α-aluminum oxide) are mixed as a whole.

[0100] (2) Amorphous aluminum oxide and α-aluminum oxide are mixed in the base end portion 100A of the protrusion 100. In other words, the area of ​​α-aluminum oxide / the area of ​​amorphous aluminum oxide>0.01.

[0101] (3) In the base end portion 100A of the protrusion 100 (range of 20 nm from the root), the area of ​​α-alumina is larger than the area of ​​amorphous alumina. In other words, more α-alumina is contained than amorphous alumina.

[0102] (4) Although the amount is small compared to amorphous aluminum oxide and α-aluminum oxide, metallic aluminum is contained in the base end portion 100A of the protrusion 100. The area of ​​aluminum oxide (amorphous aluminum oxide + α-aluminum oxide) / the area of ​​metallic aluminum + the area of ​​aluminum oxide > 90%.

[0103] In addition, the resin (polyphenylene sulfide) of the positive electrode resin member 70 is impregnated in the base end portion 100A (root portion) of the protrusion 100. In other words, the positive electrode resin member 70 is joined to the cover member 30 and the positive electrode terminal member 50 at the base end portion 100A (root portion) of the protrusion 100. The positive electrode resin member 70 is joined to the cover member 30 and the positive electrode terminal member 50 at the base end portion 100A (root portion) of the protrusion 100, and the positive electrode resin member 70 is also joined to the cover member 30 and the positive electrode terminal member 50 at the tip end portion 100B of the protrusion 100.

[0104] Furthermore, the bonding structure and use of the negative electrode resin member 80, the cover member 30 and the negative electrode terminal member 60 Figure 5A , Figure 5B , Fig. 6A , Figure 6B and Fig. 7A , Figure 7B The above-described positive electrode resin member 70 is configured similarly to the joint structure of the cover member 30 and the positive electrode terminal member 50. In addition, the joint area between the cover member 30 and the negative electrode resin member 80 and the joint area between the negative electrode terminal member 60 and the negative electrode resin member 80 are roughened and used. Figure 5A to Figure 7B The above-described roughening treatments for the lid member 30 and the positive electrode terminal member 50 are configured similarly.

[0105] [Battery Manufacturing]

[0106] Next, regarding the method for manufacturing the battery 1, refer to Fig.11 The manufacturing method of the battery 1 includes a component preparation step S1, a protrusion forming step S2, an insert molding step S3, a cap assembly finishing step S4, a closing step S5, a welding step S6, a liquid injection and sealing step S7, and an initial charging and aging step S8.

[0107] In the component preparation step S1, the cover member 30, the positive electrode terminal member 50, and the negative electrode terminal member 60 are prepared. Specifically, the liquid injection hole 30k, the positive electrode insertion hole 33h, the negative electrode insertion hole 34h, and the safety valve 19 are formed in the aluminum plate by a conventional general processing method, thereby obtaining the cover member 30. In addition, the aluminum plate is obtained by a conventional general processing method. Figure 3 A positive electrode terminal member 50 of the shape shown is obtained. Furthermore, a negative electrode terminal member 60 of the same shape as the positive electrode terminal member 50 is obtained from a copper plate by a conventional general processing method.

[0108] Following the component preparation step S1, the protrusion forming step S2 is performed. In the protrusion forming step S2, the surface of the cover member 30, which can become the cover upper surface roughening region F1 and the cover lower surface roughening region F2 in a state where the protrusion has not yet been formed, is irradiated with a pulsed laser, thereby forming the cover upper surface roughening region F1 and the cover lower surface roughening region F2. Similarly, in the protrusion forming step S2, the surface of the positive terminal member 50, which can become the terminal side surface roughening region F3 and the terminal lower surface roughening region F4 in a state where the protrusion has not yet been formed, is irradiated with a pulsed laser, thereby forming the terminal side surface roughening region F3 and the terminal lower surface roughening region F4.

[0109] As an example of the irradiation conditions of the pulsed laser irradiation in the protrusion forming step S2, the energy density of the laser irradiation per pulse is set to 24 J / cm in the case of aluminum. 2 In the case of copper, it becomes 32 J / cm 2 . And, for example, for aluminum, the wavelength is set to 1060 nm, the average output power is set to 25 W, the pulse period is set to 40 μs, the pulse width is set to 50 ns, the spot diameter is set to 63 μm, the conveying speed is set to 1450 mm / s, and the line spacing is set to 0.059 mm. Fig. 12A , 12B The figure schematically shows the trajectory of pulse laser irradiation when the pulse laser is irradiated on the cover lower surface roughened region F2 and the terminal side surface roughened region F3 in the protrusion forming step S2.

[0110] like Fig. 12A As shown, for the cover lower surface roughened region F2, on one side of the cover lower surface roughened region F2 along the left-right direction X ( Fig. 12A The top of the left L) Fig. 12A The side recorded as the "starting point" in the forward and backward direction Y is carried out on one side ( Fig. 12A Then, the pulse laser is irradiated to the other side (B) along the left-right direction X at a set line spacing (0.059 mm). Fig. 12A The right side R in the middle is staggered, and the other side ( Fig. 12A Then, the laser beam is directed to the other side (F) along the left-right direction X at a set line spacing (0.059 mm). Fig. 12A The right side R in the middle is offset, and the forward and backward direction Y is performed again on one side ( Fig. 12A After that, the pulsed laser irradiation is repeated until the pulsed laser irradiation traveling to one side or the other side in the front-rear direction Y reaches the other side (the side) of the roughened area F2 on the lower surface of the cover along the left-right direction X. Fig. 12A The top of the right side R) ( Fig. 12A The side recorded as the “end point” in FIG.

[0111] By irradiating the roughened area F2 of the lower surface of the cover with pulsed laser under the above conditions, protrusions 100 containing metallic aluminum, amorphous aluminum oxide and α-aluminum oxide and having a diameter and height of nanometer level are densely arranged in a mesh shape on the surface of the cover member 30 composed of metallic aluminum.

[0112] Furthermore, the position where the pulse laser irradiation starts in the cover lower surface roughening area F2 ( Fig. 12A The side described as "starting point" in the text is not limited to Fig. 12A ,exist Fig. 12A The side described as the "end point" in the figure may also be the position where the pulse laser irradiation starts. In addition, the pulse laser irradiation of the roughened surface area F1 on the cover is also the same as Fig. 12A The pulse laser irradiation on the cover lower surface roughened region F2 shown in the figure is performed in the same manner. However, the pulse laser irradiation on the cover upper surface roughened region F1 and the pulse laser irradiation on the cover lower surface roughened region F2 may be performed in different manners.

[0113] like Fig. 12B As shown, for the terminal side roughened region F3, at the top end ( Fig. 12B The positive terminal member 50 is irradiated with a pulsed laser that travels to one side in the first direction O of the positive terminal member 50 (the side recorded as the “starting point” in the figure). Next, the positive terminal member 50 is staggered to the other side along the third direction Q with a set line spacing (0.059 mm), and the pulsed laser irradiation that travels to the other side in the first direction O is performed. Then, the positive terminal member 50 is staggered to the other side along the third direction Q with a set line spacing (0.059 mm), and the pulsed laser irradiation that travels to one side in the first direction O is performed again. Thereafter, the pulsed laser irradiation is repeated until the pulsed laser irradiation that travels to one side or the other side of the first direction O reaches the top ( Fig. 12B The side recorded as the “end point” in FIG.

[0114] By subjecting the terminal side roughening region F3 to pulse laser irradiation under the above-mentioned conditions, protrusions 100 containing metallic aluminum, amorphous aluminum oxide and α-aluminum oxide and having a diameter and height of nanometer level are densely arranged in a mesh shape on the surface of the positive terminal member 50 composed of metallic aluminum.

[0115] Furthermore, the position where the pulse laser irradiation starts in the terminal side roughening area F3 ( Fig. 12BThe side described as "starting point" in the text is not limited to Fig. 12B ,exist Fig. 12B The side recorded as the "end point" in the figure can also be the starting point of pulse laser irradiation. In addition, the pulse laser irradiation of the roughened area F4 on the lower surface of the terminal is also the same as Fig. 12B The pulse laser irradiation for the terminal side roughening area F3 shown in the figure is performed in the same manner. However, the direction of the pulse laser irradiation at this time is the same as the laser irradiation for the terminal side roughening area F3, but the starting position and the ending position of the pulse laser irradiation become the top of one side and the top of the other side of the terminal lower surface roughening area F4 along the first direction O of the positive terminal member 50. Furthermore, the direction in which the pulse laser irradiation is staggered by a set line pitch (0.059 mm) becomes one side in the second direction P of the positive terminal member 50.

[0116] In the protrusion forming step S2, the pulse laser irradiation is performed on the bonding area of ​​the cover member 30 and the negative electrode resin member 80 around the negative electrode insertion hole 34h in a manner substantially similar to the case of the cover upper surface roughening area F1 and the cover lower surface roughening area F2, except for the energy density. Similarly, the pulse laser irradiation is performed on the bonding area of ​​the negative electrode terminal member 60 and the negative electrode resin member 80 in a manner substantially similar to the case of the terminal side surface roughening area F3 and the terminal lower surface roughening area F4, except for the energy density. Here, "substantially the same manner" refers to the area where the pulse laser irradiation is performed and the conditions of the pulse laser irradiation.

[0117] After the protrusion forming step S2, the insert molding step S3 is performed. In the insert molding step S3, the positive electrode resin member 70 and the negative electrode resin member 80 are formed, and the positive electrode resin member 70 is joined to the cover member 30 and the positive electrode terminal member 50 to form an integrated body, and the negative electrode resin member 80 is joined to the cover member 30 and the negative electrode terminal member 60 to form an integrated body. That is, the unit member 1A as an aluminum resin composite is manufactured. Fig.13 It is an explanatory diagram schematically showing the insert molding step S3 on the positive electrode terminal member 50 side.

[0118] In the insert molding step S3, a mold DE is used. The mold DE has a lower mold DE1 arranged on the lower side and an upper mold DE2 arranged on the upper side. First, the lower mold DE1 and the upper mold DE2 are set so that the cover member 30, the positive terminal member 50 and the negative terminal member 60 are arranged at a predetermined position. At this time, the mold DE is used to integrally support the positive terminal member 50 inserted into the positive electrode insertion hole 33h, the negative terminal member 60 inserted into the negative electrode insertion hole 34h, and the cover member 30. In addition, the set lower mold DE1 and the upper mold DE2 form a space corresponding to the positive electrode resin member 70 and the negative electrode resin member 80.

[0119] In the insert molding process S3, the filling process S31 is first performed, and then the curing process S32 is performed. In the filling process S31, as shown in FIG. Fig.13 As shown, the molten resin MR, which is the material of the positive electrode resin member 70 and the negative electrode resin member 80, is injected from the gate member GT through the upper mold DE2 into the space formed by the lower mold DE1 and the upper mold DE2. At this time, for example, the molten resin MR is filled into the gaps between the large number of protrusions until it reaches the base of the protrusions.

[0120] The material of the positive electrode resin member 70 and the negative electrode resin member 80 contains polyphenylene sulfide as a main component. The material of the positive electrode resin member 70 and the negative electrode resin member 80 contains a glass filler. The linear expansion coefficient of the material of the positive electrode resin member 70 and the negative electrode resin member 80 is set between the linear expansion coefficient of copper (1.65) and the linear expansion coefficient of aluminum (2.31).

[0121] Then, after the molten resin MR is injected, the molten resin MR is appropriately cooled as a solidification step S32, thereby forming the positive electrode resin member 70 and the negative electrode resin member 80. Specifically, for example, in the filling step S31, the molten resin MR that fills the gaps between the large number of protrusions 100 included in the roughened regions F1 to F4 until it reaches the base of the protrusions 100 is solidified to form the positive electrode resin member 70 joined to the joining regions E1 to E4 including the roughened regions F1 to F4. Similarly, the negative electrode resin member 80 is also formed. Then, the upper mold DE2 is moved upward, and the unit member 1A consisting of the integrated cover member 30, the positive electrode resin member 70 and the positive terminal member 50, the negative electrode resin member 80 and the negative terminal member 60 is taken out from the lower mold DE1.

[0122] Following the insert molding process S3, the cover assembly completion process S4 is performed. In the cover assembly completion process S4, the cover assembly is completed. Specifically, the electrode body 40 is prepared, and the lower side portion 52 of the positive terminal and the lower side portion 62 of the negative terminal of the unit member 1A generated by the insert molding process S3 are welded to the positive electrode collecting portion 41r and the negative electrode collecting portion 42r of the electrode body 40, respectively. Then, the electrode body 40 in this state is surrounded (wrapped) with a bag-shaped insulating bracket 5. As a result, the cover assembly consisting of the cover member 30, the positive terminal member 50, the negative terminal member 60, the positive electrode resin member 70, the negative electrode resin member 80, the electrode body 40 and the insulating bracket 5 is completed.

[0123] After the cover assembly completion step S4, the closing step S5 is performed. In the closing step S5, the main body member 20 is prepared, and the portion below the cover member 30 including the electrode body 40 and the insulating bracket 5 in the cover assembly completed in the cover assembly completion step S4 is inserted into the main body member 20, and the opening 21 of the main body member 20 is closed by the cover member 30.

[0124] Following the closing step S5, the welding step S6 is performed. In the welding step S6, the top ends of the upper side U of the front side portion 13, the rear side portion 14, the left side portion 15, and the right side portion 16 of the main body member 20 in the vertical direction Z are laser welded to the peripheral edge of the cover member 30 over the entire circumference, thereby hermetically sealing the opening 21.

[0125] Following the welding step S6, the liquid injection and sealing step S7 is performed. In the liquid injection and sealing step S7, the electrolyte 3 is injected into the outer shell 10 through the liquid injection hole 30k, and the electrolyte 3 is immersed in the electrode body 40. Then, the sealing member 39 is inserted into the liquid injection hole 30k from the upper side U, and the sealing member 39 is welded to the cover member 30 over the entire circumference, so that the sealing member 39 and the cover member 30 are hermetically sealed.

[0126] After the liquid injection and sealing step S7, the charging and aging step S8 is performed. In the charging and aging step S8, a charging device (not shown) is connected to the battery 1 to perform initial charging on the battery 1. Then, the initially charged battery 1 is left for a predetermined time to perform aging on the battery 1. In this way, the battery 1 is completed.

[0127] Next, an experiment for verifying the acid resistance and hydrofluoric acid resistance of the joint between the aluminum component and the resin component is described. The experiment was conducted by the applicant of the present patent. In addition, the experiment is referred to as the "joint durability verification experiment". The joint durability verification experiment consists of the following three steps (1) to (3).

[0128] (1) Preparation of test specimens

[0129] (2) Implementation of acid resistance test

[0130] (3) Implementation of hydrofluoric acid resistance test

[0131] First, the preparation of (1) test specimens is described. The test specimens are the test objects for the joint durability verification experiment. The test specimens are formed by joining a plate-like aluminum component to a resin component. The resin component is made of polyphenylene sulfide (PPS). The plate-like aluminum component is made of metal aluminum. Among the plate-like aluminum components, there are aluminum components whose component surfaces are irradiated with pulsed laser under the irradiation conditions of the above-mentioned protrusion forming step S2, and aluminum components whose component surfaces are not irradiated with pulsed laser.

[0132] Hereinafter, the aluminum components irradiated with pulsed laser are referred to as "irradiated aluminum components", and the aluminum components not irradiated with pulsed laser are referred to as "non-irradiated aluminum components". In the joint durability verification experiment, three irradiated aluminum components and three non-irradiated aluminum components were prepared for the acid resistance test, and three irradiated aluminum components and three non-irradiated aluminum components were prepared for the hydrofluoric acid resistance test.

[0133] Each aluminum member was formed into a square shape in plan view as a whole, with each side of the square being 50 mm long and the thickness of the metal member being 0.5 mm.

[0134] In addition, a roughened area irradiated with pulsed laser light under the irradiation conditions of the above-mentioned protrusion forming step S2 is formed on the surface of each irradiated aluminum member on the side where the aluminum member is bonded to the resin member. The shape of the roughened area is a circle with a diameter of 20 mm. The center of the roughened area is roughly consistent with the center of the irradiated aluminum member. In the roughened area, a large number of protrusions 100 with diameters and heights at the nanometer level are formed in a mesh-like manner in a dense state in parallel, similar to the above-mentioned roughened areas F1 to F4.

[0135] Then, for each aluminum component, a resin component was joined by insert molding. The shape of the resin component was a circular plate. The diameter of the resin component was 16 mm, and the height of the resin component was 3 mm. Moreover, the center of the resin component was roughly consistent with the center of the aluminum component. In addition, in this experiment, the resin component was joined to the irradiated aluminum component within the range of the roughening area.

[0136] Next, (2) the acid resistance test is described. In the acid resistance test, the irradiated aluminum component and the non-irradiated aluminum component were immersed in 0.1 mol / L hydrochloric acid. Next, one irradiated aluminum component and one non-irradiated aluminum component were taken out 1 hour, 5 hours, and 24 hours after the start of immersion. Then, for each immersion time, one hour after taking out, it was confirmed whether the resin component was peeled off from the aluminum component.

[0137] Finally, (3) the hydrofluoric acid resistance test is described. In the hydrofluoric acid resistance test, first, a 1M LiPF 6 The irradiated aluminum component and the non-irradiated aluminum component were immersed in the product obtained by adding 1200 ppm of water to the electrolyte solution composed of EC / DEC=1:1. Then, one irradiated aluminum component and one non-irradiated aluminum component were taken out 1 hour, 5 hours, and 24 hours after the start of immersion. Then, for each immersion time, one hour after taking out, it was confirmed whether the resin component was peeled off from the aluminum component.

[0138] Fig.14A This is a table showing the results of (2) acid resistance test. Fig. 14B This is a table showing the results of (3) hydrofluoric acid resistance test. Fig.14A Table and Fig. 14B The table shows the relationship between the immersion time of each aluminum component and the presence or absence of peeling.

[0139] like Fig.14A As shown in FIG. 2 , as a result of the acid resistance test (2), the irradiated aluminum component did not peel off, while the non-irradiated aluminum component peeled off after 24 hours of immersion. Fig. 14B As shown in (3), as a result of the hydrofluoric acid resistance test, the irradiated aluminum components did not peel off, while the non-irradiated aluminum components peeled off after being taken out after 24 hours of immersion. Therefore, the irradiated aluminum components are considered to have higher acid resistance and hydrofluoric acid resistance than the non-irradiated aluminum components in terms of the bonding portion with the resin component. Furthermore, although detailed descriptions are omitted, element mapping was performed using the above-mentioned FIB method and TEM-EELS for all irradiated aluminum components. As a result, the presence of α-alumina was confirmed in all irradiated aluminum components. In addition, for the non-irradiated aluminum components, an oxide film was formed on the surface of the component, and it was considered that α-alumina did not exist. Therefore, compared with the case where the protrusion does not contain α-alumina, when the protrusion contains α-alumina, the acid resistance and hydrofluoric acid resistance of the bonding portion with the resin component are higher.

[0140] As described above, a large number of protrusions 100 having a diameter and a height of less than 1 μm are closely arranged on the surface of the cover member 30 and the positive terminal member 50 made of metal aluminum, so that when the positive electrode resin member 70 is joined to the cover member 30 and the positive terminal member 50 by the anchor effect, the joining strength of the joint portion is improved. Furthermore, the base end portion 100A of the protrusion 100 connected to the member surface contains not only amorphous aluminum oxide but also α-alumina with excellent chemical stability, so that the acid resistance and hydrofluoric acid resistance of the joint portion and the resistance to peeling of the positive electrode resin member 70 when immersed in a liquid obtained by adding water to hydrochloric acid or a non-aqueous electrolyte containing lithium hexafluorophosphate are improved. In addition, the base end portion 100A of the large number of protrusions 100 contains more α-alumina than amorphous aluminum oxide. Therefore, the acid resistance and hydrofluoric acid resistance of the joint portion are further improved, and the resistance to separation of the positive electrode resin member 70 when immersed in a liquid obtained by adding water to hydrochloric acid or a non-aqueous electrolyte containing lithium hexafluorophosphate is further improved.

[0141] In addition, the gaps between the large number of protrusions 100 formed in the roughened areas F1 to F4 are filled with the positive electrode resin component 70. Therefore, as an aluminum-resin composite, the bonding strength of the bonding portion between the aluminum component and the resin component is improved, and at the same time, the acid resistance and hydrofluoric acid resistance of the bonding portion, and the difficulty of separation of the positive electrode resin component 70 when immersed in a liquid formed by adding water to hydrochloric acid or a non-aqueous electrolyte containing lithium hexafluorophosphate, are further improved.

[0142] Furthermore, by adopting the above-mentioned protrusion forming step S2, protrusions 100 containing α-alumina and having a diameter and height of nanometer level are formed in a mesh-like and densely arranged state, and by adopting the above-mentioned insert molding step S3, the positive electrode resin component 70 can be filled in the gaps between a large number of protrusions 100. Therefore, while the bonding strength of the bonding portion between the cover member 30 and the positive terminal member 50 and the positive electrode resin component 70 is improved, the acid resistance and hydrofluoric acid resistance of the bonding portion are further improved, and the difficulty of separation of the positive electrode resin component 70 when immersed in a liquid formed by adding water to hydrochloric acid or a non-aqueous electrolyte containing lithium hexafluorophosphate is further improved.

[0143] Furthermore, this embodiment is merely an example and does not limit the present invention in any way. Therefore, the present invention can be modified and altered in various ways without departing from the scope of the present invention. The following describes the improved and modified examples of this embodiment.

[0144] In this embodiment, a flat wound electrode body 40 is exemplified as the electrode body housed in the housing 10, but the electrode body may also be a stacked electrode body. In addition, in this embodiment, one electrode body is housed in the housing 10, but a plurality of electrode bodies may be housed in the housing 10.

[0145] In the present embodiment, the outer shell 10 is a flat rectangular parallelepiped with a bottom as a whole, but the shape of the outer shell 10 may be appropriately deformed and may be other shapes such as a cylindrical shape. In addition, the shape of one or both of the positive terminal member 50 and the negative terminal member 60 may be appropriately deformed. Similarly, the shape of one or both of the positive electrode resin member 70 and the negative electrode resin member 80 may be appropriately deformed. Furthermore, in the present embodiment, the shape of the positive terminal member 50 and the shape of the negative terminal member 60 may be the same or different. Similarly, in the present embodiment, the shape of the positive electrode resin member 70 is the same as the shape of the negative electrode resin member 80, but may be different.

[0146] In this embodiment, the battery 1 in which the lid member 30 and the positive electrode terminal member 50 made of metal aluminum are respectively joined to the positive electrode resin member 70 is included in the aluminum resin composite of the present invention, and the cell member 1A constituting the battery 1 is also included in the aluminum resin composite of the present invention.

[0147] In this embodiment, the present invention is applied to lithium-ion batteries, but it can be applied to any general power storage device, for example, the present invention can also be applied to nickel-hydrogen batteries and nickel-cadmium batteries. In addition, the use of the present invention is not limited to batteries, and can be widely applied to composites in which aluminum components and resin components are joined.

[0148] In the present embodiment, as the irradiation condition of the pulsed laser irradiation in the protrusion forming step S2, that is, the irradiation condition of the pulsed laser irradiation for forming protrusions containing metallic aluminum, amorphous aluminum oxide and α-aluminum oxide and having a diameter and height at the nanometer level arranged in a dense mesh state, the wavelength is set to 1060nm, but it can also be appropriately changed in the range of 1060 to 1080nm. Similarly, the spot diameter can be appropriately set in the range of 10 to 200μm. More preferably, the spot diameter can be appropriately set in the range of 50 to 100μm. Furthermore, the interval of irradiation involving laser irradiation can be set to + / -10% of the spot diameter.

[0149] In addition, according to Fig. 9C and Fig.9D In the base end portion of the protrusion (range from the root to 20 nm), the area of ​​α-alumina is larger than the area of ​​amorphous alumina. In other words, it is estimated that more α-alumina is contained than amorphous alumina, but the content ratio of amorphous alumina and the content ratio of α-alumina can be made roughly the same. Alternatively, more amorphous alumina can be made than α-alumina. However, from the viewpoint of acid resistance and hydrofluoric acid resistance, it is preferable to contain more α-alumina than amorphous alumina.

[0150] In the present embodiment, the resin member 70 for the positive electrode reaches the base ends (roots) of a large number of protrusions constituting the roughened regions F1 to F4, but for example, the resin member 70 for the positive electrode may be filled in the gaps between a large number of protrusions in a state where it reaches the top end of the protrusion as a whole, the portion between the top end and the middle, or the portion approximately in the middle or between the middle and the base end.

[0151] In the present embodiment, the roughened regions F1 and F2 are formed in the entire area of ​​the joining regions E1 and E2, but the roughened regions F1 and F2 may be formed in a part of the joining regions E1 and E2. However, in this case, the roughened regions F1 and F2 are preferably formed in the joining regions E1 and E2 in a ring shape in a manner that surrounds the positive electrode insertion hole 33h. In addition, the roughened regions F3 and F4 are formed in the entire area of ​​the joining regions E3 and E4, but the roughened regions F3 and F4 may be formed in a part of the joining regions E3 and E4. However, in this case, the roughened region F3 is preferably formed as a whole in the part of the middle portion 53 of the positive electrode terminal in the joining region E3. In addition, the roughened region F4 is preferably formed in a ring shape along the peripheral portion of the joining region E4.

Claims

1. An aluminum component, comprising metal aluminum, on the surface of which nanometer-scale protrusions with diameters and heights each less than 1 μm are densely arranged, wherein the protrusions contain amorphous aluminum oxide and α-aluminum oxide at the base end connected to the surface of the component.

2. The aluminum member according to claim 1, wherein The base end portion of the protrusion contains more α-aluminum oxide than amorphous aluminum oxide.

3. An aluminum-resin composite, comprising the aluminum member according to claim 1 or 2 to which a resin member is bonded.

4. A method for producing an aluminum-resin composite, the method for producing an aluminum-resin composite according to claim 3, comprising: a protrusion forming step, wherein the protrusion is formed on the surface of the member by irradiating the surface with laser light before the protrusion is formed; and An insert molding step, wherein, after the protrusion forming step, the resin member is formed on the member surface by insert molding.

Citation Information

Patent Citations

  • Method for producing a material composite composed of metal and plastic to form a plastic-metal hybrid component

    CN106715073A

  • Methods of manufacturing composite member and composite member

    JP2022057584A

  • Metal Formings

    JP5998303B1

  • Metal member, method for producing metal member, metal-resin joined body and method for producing metal-resin joined body

    US20200070477A1

  • Metal member, composite of metal member and resin member, and production method therefor

    WO2018092607A1