Laminated film and method for producing laminated film
By using a resin composition of a photocurable resin and an organic solvent to form a compatible layer in the laminated film, and adjusting the characteristics of the bonding layer through Raman spectroscopy, the problem of insufficient bonding between the base layer and the surface layer in the prior art is solved. , realizing a laminated film with strong winding and high joint strength.
Patent Information
- Application Number
- CN202410393081.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-02-21
- Filing Date
- 2024-04-02
- Publication Date
- 2024-10-15
AI Technical Summary
In existing laminated films, the bonding layer between the base material layer and the surface layer fails to fully exert its bonding function in the form of a mixed layer, resulting in poor bonding effects.
A resin composition of a photocurable resin and an organic solvent is coated on the base material layer, and heat treatment is performed to mix cellulose triacetate and the photocurable resin with each other to form a compatible layer, and the bonding is adjusted by Raman spectroscopy. The relationship between layer thickness and peak intensity ensures TJ×IB/IA≥15.0μm to achieve sufficient bonding.
It achieves strong winding and sufficient bonding between the base material layer and the surface layer, improves the bonding strength and durability of the laminated film, and ensures that the bonding layer will not peel off after long-term exposure to light.
Smart Images

Figure CN118769647A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a laminated film and a method for producing the laminated film. Background Art
[0002] Conventionally, there is known a laminated film including a base layer, a surface layer disposed on the base layer, and a bonding layer disposed between the base layer and the surface layer to bond the base layer and the surface layer (for example, Patent Document 1 listed below).
[0003] Patent Document 1 described below discloses that the substrate layer (transparent substrate) is formed of a resin film containing cellulose triacetate, the surface layer (low refractive index layer) is formed of a curable resin composition containing an adhesive matrix containing an ionizing radiation curable material (e.g., an acrylic material, etc.), and the bonding layer (hard coating layer) is formed in the form of a mixed layer in which a part of the cellulose triacetate contained in the substrate layer (transparent substrate) and a part of the adhesive matrix contained in the surface layer (low refractive index layer) are mixed.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2013-205644 Summary of the invention
[0007] Problems to be solved by the invention
[0008] In the laminated film having the above-described structure, the bonding layer is required to have a function of sufficiently bonding the base layer and the surface layer.
[0009] However, studies on enabling the mixed layer serving as the bonding layer to exert a sufficient bonding function when the bonding layer is formed as a mixed layer of a part of the constituents of the base layer and a part of the constituents of the surface layer are not considered sufficient.
[0010] Therefore, an object of the present invention is to provide a laminated film in which a bonding layer formed as a mixed layer of a part of the constituents of a base layer and a part of the constituents of a surface layer can exhibit a sufficient bonding function, and to provide a method for producing the laminated film.
[0011] Solutions to the problem
[0012] The present inventors have conducted intensive studies and found that, in a laminated film in which a bonding layer is formed in the form of a mixed layer including a part of the constituent components of the substrate layer and a part of the constituent components of the surface layer, the thickness of the bonding layer is set to T μm, and when imaging Raman measurement based on Raman spectroscopy is performed on the bonding layer, the bonding layer has a wavelength of 1730 cm -1 The intensity of the peak at the top of the peak is set as I A , will be at wave number 1635cm -1 The intensity of the peak at the top of the peak is set as I B When the above T and the above I A And the above I B When a specific relationship is satisfied, the bonding layer can fully exert its bonding function.
[0013] Then, the present invention was conceived.
[0014] That is, the laminated film of the present invention comprises:
[0015] Base material layer,
[0016] a surface layer disposed on the substrate layer, and
[0017] a bonding layer disposed between the substrate layer and the surface layer to bond the substrate layer and the surface layer,
[0018] The substrate layer is formed of a resin film containing cellulose triacetate,
[0019] The surface layer is formed of a resin composition containing a photocurable resin.
[0020] The bonding layer is formed in the form of a compatibility layer in which a part of the cellulose triacetate contained in the base layer and a part of the photocurable resin contained in the surface layer are compatible with each other.
[0021] The thickness of the bonding layer is T J μm,
[0022] When the bonding layer was subjected to imaging Raman measurement based on Raman spectroscopy at a wave number of 1730 cm -1 The intensity of the peak at which the peak top is observed is set as I A , will be at wave number 1635cm -1 The intensity of the peak at which the peak top is observed is set as I B hour,
[0023] The above T J , the above I A And the above I B Satisfies the following relationship:
[0024] T J×I B / I A ≥15.0μm.
[0025] In addition, the method for producing a laminated film of the present invention has the following characteristics:
[0026] forming a coating layer by coating a resin composition including a photocurable resin and an organic solvent capable of dissolving the cellulose triacetate on a base layer formed of a resin film including cellulose triacetate; and
[0027] The substrate layer and the coating layer are subjected to a heat treatment.
[0028] The heat treatment is performed so that the maximum temperature becomes 130° C. or higher. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a cross-sectional view showing the structure of the laminated film according to the present embodiment.
[0030] Figure 2A This is a cross-sectional view showing a process of forming the laminated film of this embodiment.
[0031] Figure 2B It is a cross-sectional view showing another process of forming the laminated film of this embodiment.
[0032] Figure 2C This is a cross-sectional view showing still another process of forming the laminated film according to this embodiment.
[0033] Figure 2D This is a cross-sectional view showing still another process of forming the laminated film according to the present embodiment.
[0034] Figure 3 It is a schematic diagram for explaining the method for producing the laminated film according to the present embodiment.
[0035] Explanation of symbols
[0036] 1. Substrate layer
[0037] 2 Surface layer
[0038] 3 Bonding layer
[0039] 10 Laminated Film DETAILED DESCRIPTION
[0040] [Laminated film]
[0041] Below, refer to Figure 1 A laminated film according to one embodiment of the present invention will be described. In the following, a laminated film according to a specific example of one embodiment of the present invention may be simply referred to as a laminated film according to the present embodiment.
[0042] The laminated film 10 of the present embodiment includes a base layer 1 , a surface layer 2 disposed on the base layer 1 , and a bonding layer 3 disposed between the base layer 1 and the surface layer 2 to bond the base layer 1 and the surface layer 2 together.
[0043] In the laminated film 10 of the present embodiment, the base layer 1 is formed of a resin film containing triacetyl cellulose (TAC).
[0044] In the laminated film 10 of the present embodiment, the surface layer 2 is formed of a resin composition containing a photocurable resin.
[0045] In the laminated film 10 of the present embodiment, the bonding layer 3 is formed as a compatibilizing layer in which part of the above-mentioned triacetyl cellulose (TAC) contained in the base layer 1 and part of the photocurable resin contained in the surface layer 2 are compatibilized together.
[0046] In the laminated film 10 of the present embodiment, the thickness of the bonding layer 3 is T J μm, and when imaging Raman measurement based on Raman spectroscopy was performed on the bonding layer 3, the wavelength was 1730 cm -1 The intensity of the peak at which the peak top is observed is set as I A , will be at wave number 1635cm -1 The intensity of the peak at which the peak top is observed is set as I B When the above T J , the above I A And the above I B The following relationship is satisfied.
[0047] Relational T J ×[I B / I A ]≥15.0μm
[0048] According to the laminated film having the above-described structure, the bonding layer formed as a mixed layer of a part of the constituent components of the base layer and a part of the constituent components of the surface layer can be made to exhibit a sufficient bonding function.
[0049] It should be noted that at the wave number 1730 cm -1 The peak intensity I of the peak at the top of the peak is observed A Originated from the carbon-oxygen double bond (C=O) of cellulose triacetate. At wave number 1635 cm -1 The peak intensity I of the peak at the top of the peak is observed B It is derived from the carbon-carbon double bond (C═C) of the photocurable resin.
[0050] Compatibility refers to the state in which different substances can be mixed together without separation.
[0051] Here, as described later, the laminated film 10 of the present embodiment is obtained by applying a resin composition containing a photocurable resin and an organic solvent capable of dissolving triacetyl cellulose (TAC) on the base layer 1 to form a coating layer, and then heat-treating the coating layer.
[0052] In the laminated film 10 of the present embodiment, the surface layer 2 and the bonding layer 3 are formed of the coating layer and triacetyl cellulose (TAC) diffused from the base material layer 1 into the coating layer.
[0053] More specifically, in the laminated film 10 of the present embodiment, the portion of the coating layer where the cellulose triacetate is not diffused constitutes the surface layer 2 , and the portion of the coating layer where the cellulose triacetate is diffused constitutes the bonding layer 3 .
[0054] In addition, in the bonding layer 3, the triacetyl cellulose from the base layer 1 and the photocurable resin from the coating layer are mixed with each other without separation, thereby constituting a compatible layer. That is, in the bonding layer 3, the triacetyl cellulose from the base layer 1 and the photocurable resin from the coating layer are strongly entangled with each other, thereby constituting a compatible layer.
[0055] As described above, the base material layer 1 is formed of a resin film containing triacetyl cellulose (TAC).
[0056] In the cellulose triacetate, all three hydroxyl groups present in the β-glucose unit constituting cellulose are acetylated. More specifically, all the secondary hydroxyl groups at the 2nd and 3rd positions and the primary hydroxyl group at the 6th position present in the β-glucose unit of the cellulose triacetate are acetylated.
[0057] As a commercial item of the resin film consisting of triacetyl cellulose, the trade name "TJ40UL" etc. manufactured by Fuji Film Corporation are mentioned, for example.
[0058] The glass transition temperature Tg of the above-mentioned cellulose triacetate (TAC) is 130°C.
[0059] The glass transition temperature Tg can be measured, for example, using a DSC device. More specifically, the glass transition temperature Tg can be determined from a DSC curve obtained when a sample (cellulose triacetate) is heated at a rate of 5°C / min while nitrogen is flowing from a temperature 30K or more lower than the expected glass transition temperature Tg to a temperature 30K or more higher.
[0060] The glass transition temperature Tg can be determined based on the method described in JIS K7121:1987 "Method for measuring glass transition temperature of plastics".
[0061] The resin film as the substrate layer 1 can be obtained, for example, by forming a resin composition containing triacetyl cellulose (TAC) into a film. When the resin composition is formed into a film, it is preferably not subjected to a stretching treatment. That is, the resin film is preferably a non-stretched film.
[0062] As described above, the surface layer 2 is formed of a resin composition containing a photocurable resin. Examples of the photocurable resin include resins that can cure the surface layer 2 by irradiation with active energy rays (hereinafter also referred to as active energy ray-curable resins).
[0063] Examples of active energy ray-curable resins include resins that are cured by irradiation with electron beams, ultraviolet rays, α rays, β rays, γ rays, or X rays, and ultraviolet-curable resins that are cured by irradiation with light such as ultraviolet rays are preferred.
[0064] In addition, the irradiation with active energy rays may be irradiation with light (light irradiation) including ultraviolet light or the like.
[0065] Examples of the photocurable resin include polyester resins, (meth)acrylic resins, urethane resins, amide resins, silicone resins, epoxy resins, and urethane (meth)acrylate resins.
[0066] Among them, as the photocurable resin, at least one of a (meth)acrylic resin and a urethane (meth)acrylate resin is preferably used, and a urethane (meth)acrylate resin is more preferably used.
[0067] In addition, as a commercial item of urethane (meth)acrylate type resin, the trade name "LUXYDIR 17-806" etc. made by DIC Corporation are mentioned, for example.
[0068] The photocurable resin may be a copolymer of an oligomer having a functional group and a monomer having a functional group.
[0069] Examples of the oligomer having a functional group include curable urethane (meth)acrylates. The curable urethane (meth)acrylates may be hexafunctional or higher, or octafunctional or higher. The curable urethane (meth)acrylates may be decafunctional or lower.
[0070] Examples of the monomer having a functional group include polyfunctional (meth)acrylates. The polyfunctional (meth)acrylate may be difunctional or higher, or trifunctional or higher.
[0071] The resin composition may contain a photopolymerization initiator. When the resin composition contains a photopolymerization initiator, the polymerization reaction of the photocurable resin can be more easily initiated when the surface layer 2 is irradiated with active energy rays (eg, ultraviolet rays) to cure the surface layer 2 .
[0072] The photopolymerization initiator may be appropriately selected according to the type of the photocurable resin.
[0073] Examples of the photopolymerization initiator include 4,4′-bis(diethylamino)benzophenone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, ethyl 4-(dimethylamino)benzoate, [4-(methylphenylthio)phenyl]-phenylmethane, ethyl 4-dimethylaminobenzoate, methyl o-benzoylbenzoate, methyl benzoylformate, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)diphenylphosphine oxide, and 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propanone.
[0074] When the above-mentioned (meth) acrylic resin or the above-mentioned carbamate (meth) acrylate resin is used as the above-mentioned photocurable resin, as the photopolymerization initiator, it is preferred to use 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)diphenylphosphine oxide, or 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propanone, and it is particularly preferred to use 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propanone.
[0075] In addition, as a commercial product of 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propanone, the trade name "OMNIRAD907" manufactured by BASF Corporation is mentioned, for example.
[0076] When light is irradiated from the surface side of the surface layer 2 , the surface layer 2 can be sufficiently cured by a polymerization reaction of carbon-carbon bonds (C═C) of the photocurable resin.
[0077] On the other hand, as described above, in the bonding layer 3 , the photocurable resin and the cellulose triacetate are formed in a state of being strongly entangled with each other.
[0078] Therefore, when the surface layer 2 is irradiated with light, etc., the polymerization reaction of the carbon-carbon bond (C=C) of the photocurable resin may not be fully carried out in the bonding layer 3 due to the strong entanglement between the photocurable resin and the cellulose triacetate. That is, the curing in the bonding layer 3 will proceed more slowly than the curing in the surface layer 2.
[0079] As a result, even after the surface layer 2 is irradiated with light, carbon-carbon double bonds (C=C) derived from the photocurable resin remain in the bonding layer 3. Therefore, when imaging Raman measurement based on Raman spectroscopy is performed on the bonding layer 3 after irradiation with active energy rays, a peak derived from the carbon-carbon double bond (C=C) is observed. Specifically, in the bonding layer 3 after irradiation with active energy rays, a peak with a wave number of 1635 cm -1 That is, a peak intensity I B .
[0080] The resin composition may contain 1 part by mass or more, 2 parts by mass or more, or 4 parts by mass or more of the photopolymerization initiator relative to 100 parts by mass of the photocurable resin.
[0081] Furthermore, the resin composition may contain 10 parts by mass or less of the photopolymerization initiator relative to 100 parts by mass of the photocurable resin.
[0082] The resin composition may include an organic solvent for dissolving / suspending the photocurable resin. As the organic solvent, there may be mentioned monohydric alcohol solvents such as methanol, ethanol, isopropanol, butanol, 2-methoxyethanol, ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, or cyclopentanone, ester solvents such as methyl acetate, ethyl acetate, or butyl acetate, ether solvents such as diisopropyl ether or propylene glycol monomethyl ether, polyol solvents such as ethylene glycol or propylene glycol, non-cyclic aliphatic hydrocarbon solvents such as hexane, heptane, or octane, cyclic aliphatic hydrocarbons such as cyclohexane or cycloheptane, or aromatic hydrocarbon solvents such as benzene, toluene, or xylene. These may be used alone or in combination.
[0083] It should be noted that the surface layer 2 is Figure 2A to Figure 2D As shown, the above resin composition can be applied on the substrate layer 1 to form the coating layer 4 (see Figure 2A ) The base material layer 1 and the coating layer 4 are subjected to heat treatment (refer to Figure 2B to Figure 2D ) is formed.
[0084] In addition, when the coating layer 4 is formed, the surface layer of the substrate layer 1 is dissolved by the organic solvent contained in the resin composition, and by heating the substrate layer 1 and the coating layer 4, the molecular motion of a part of the cellulose triacetate C contained in the substrate layer 1 becomes active (see Figure 2B ), so that part of the cellulose triacetate C diffuses into the coating layer 4 (refer to Figure 2C ).
[0085] It should be noted that in order to activate the molecular motion of cellulose triacetate C, cellulose triacetate C must be transformed from a glass state to a rubber state.
[0086] Therefore, the above-mentioned heat treatment is performed at a temperature higher than the glass transition temperature Tg (130° C.) of cellulose triacetate.
[0087] Furthermore, in the portion where the cellulose triacetate C is diffused in the coating layer 4 as described above, the cellulose triacetate C and the photocurable resin are mixed with each other without being separated, thereby forming a compatible layer.
[0088] That is, as described above, the surface layer 2 composed of the photocurable resin and the compatible layer of the photocurable resin and cellulose triacetate C can be formed by the coating layer 4 .
[0089] In addition, as described above, during the heating treatment of the base layer 1 and the coating layer 4, the organic solvent contained in the coating layer 4 is volatilized. After the organic solvent is volatilized, the compatibilizing layer functions as a bonding layer 3 for bonding the base layer 1 and the surface layer 2 (see Figure 2D ).
[0090] The bonding layer 3 can more strongly bond the base layer 1 and the surface layer 2 together by irradiating active energy rays (ultraviolet rays or the like).
[0091] This is because the irradiation with light allows a partial polymerization reaction of the photocurable resin to proceed, thereby sufficiently maintaining the cellulose triacetate entangled with the photocurable resin.
[0092] From the viewpoint of allowing the compatible layer to exhibit sufficient adhesion, the boiling point of the organic solvent is preferably ±10° C. of the highest temperature during the heat treatment of the coating layer.
[0093] For example, when the maximum temperature during the heat treatment of the coating layer is 130° C., cyclopentanone having a boiling point of 140° C. is preferably used as the organic solvent.
[0094] By making the difference between the maximum temperature and the boiling point of the organic solvent small, the organic solvent can be gradually volatilized from the coating layer formed of the resin composition. Thus, a compatibility layer in which triacetylcellulose and the photocurable resin are fully compatible can be formed between the substrate layer 1 and the surface layer 2. That is, a bonding layer 3 that can fully bond the substrate layer 1 and the surface layer 2 can be formed.
[0095] In addition, when the resin composition contains two or more organic solvents, when the two or more organic solvents form an azeotropic mixture, the azeotropic point is the above-mentioned boiling point.
[0096] Furthermore, from the viewpoint of sufficiently dissolving the surface layer portion of the substrate layer 1 and sufficiently diffusing a portion of the cellulose triacetate into the coating layer, the organic solvent is preferably ethyl acetate or cyclohexane.
[0097] It should be noted that, when the resin composition contains a tackifier as described later, since ethyl acetate cannot fully dissolve the tackifier, if only ethyl acetate is used as the organic solvent, coagulation of the tackifier may be generated in the bonding layer 3. If coagulation of the tackifier is generated in the bonding layer 3, it is undesirable from the perspective of poor appearance of the laminated film 10.
[0098] Here, since the above-mentioned thickener generally shows high solubility in toluene, it is preferable to use ethyl acetate and toluene in combination. By using ethyl acetate and toluene in combination, the surface layer of the substrate layer 1 can be fully dissolved, so that the cellulose triacetate contained in the surface layer can be fully diffused into the coating layer, and the thickener can be dissolved by toluene. That is, in the laminated film 10, the adhesion between the substrate layer 1 and the surface layer 2 by the bonding layer 3 can be fully ensured, and the occurrence of poor appearance due to the aggregation of the thickener can be suppressed.
[0099] The resin composition may contain a tackifier. Examples of the tackifier include organic clays such as smectite, talc, bentonite, montmorillonite, and kaolinite.
[0100] In addition, smectite which has been highly purified by hot water treatment is also called Sumecton.
[0101] The resin composition may contain 0.5 parts by mass or more, 1.0 parts by mass or more, or 2.5 parts by mass or more of the tackifier relative to 100 parts by mass of the photocurable resin. In addition, the resin composition may contain 5 parts by mass or less of the tackifier relative to 100 parts by mass of the photocurable resin.
[0102] The resin composition may contain a filler, which may be an inorganic filler or an organic filler.
[0103] Examples of the inorganic filler include silicon oxide particles, titanium oxide particles, aluminum oxide particles, zinc oxide particles, tin oxide particles, calcium carbonate particles, barium sulfate particles, talc particles, kaolin particles, and calcium sulfate particles.
[0104] Examples of the organic filler include polymethyl methacrylate resin particles (PMMA particles), silicone resin particles, polystyrene resin particles, polycarbonate resin particles, acrylic styrene resin particles, benzoguanamine resin particles, melamine resin particles, polyolefin resin particles, polyester resin particles, polyamide resin particles, polyimide resin particles, and polyvinyl fluoride resin particles.
[0105] The inorganic filler and the organic filler may be used alone or in combination of two or more.
[0106] It should be noted that, when the resin composition contains the filler, the filler is naturally also contained in the surface layer 2. The filler may have a property of absorbing light, so that the surface layer 2 can fully function as an antireflection layer.
[0107] The resin composition may contain 5 parts by mass or more, 7 parts by mass or more, or even 10 parts by mass or more of the filler relative to 100 parts by mass of the photocurable resin.
[0108] The resin composition may contain 30 parts by mass or less, or 20 parts by mass or less, of the filler relative to 100 parts by mass of the photocurable resin.
[0109] The resin composition may contain a leveling agent (surface modifier). Examples of the leveling agent include fluorine-based surfactants. Examples of commercially available fluorine-based surfactants include: Megafac F-556 manufactured by DIC Corporation,
[0110] The resin composition may contain 0.1 parts by mass or more, 0.2 parts by mass or more, or even 0.4 parts by mass or more of the leveling agent relative to 100 parts by mass of the photocurable resin.
[0111] The resin composition may contain 2 parts by mass or less, or 1 part by mass or less, of the leveling agent relative to 100 parts by mass of the photocurable resin.
[0112] In the laminated film 10 of the present embodiment, the surface layer 2 may function as a hard coat layer, may function as an antiglare layer, or may function as an antireflection layer.
[0113] The hard coat layer imparts scratch resistance or chemical resistance to the surface of the laminate film 10. Therefore, the laminate film 10 having the surface layer 2 functioning as a hard coat layer can be bonded to an image display unit in an image display device such as a tablet computer and used.
[0114] The antiglare layer is a layer for preventing external light from entering by scattering and reflecting light. Therefore, the laminated film 10 including the surface layer 2 as the antiglare layer can be bonded to an image display unit of an image display device of a car navigation system and used, for example.
[0115] The antireflection layer is a layer for preventing reflection of external light. Therefore, the laminated film 10 including the surface layer 2 as the antireflection layer can be bonded to an image display unit of an image display device of a car navigation system and used, for example.
[0116] In the laminated film 10 of the present embodiment, the thickness T of the base material layer 1 is B The thickness T of the substrate layer 1 may be 10 μm or more, 20 μm or more, or 30 μm or more. B The thickness may be 100 μm or less, 80 μm or less, or 50 μm or less.
[0117] The thickness T of the substrate layer 1 B The thickness T of the substrate layer 1 can be obtained by using a digital linear pointer meter (trade name "MODEL D-10HS", manufactured by Ozaki Manufacturing Co., Ltd.) as a measuring device. B The thickness T of the substrate layer 1 can be obtained by measuring the thickness of five random locations in the width direction of the substrate layer 1 using the digital linear pointer meter and taking the arithmetic average of the measured values. B The thickness T of the surface layer 2 described below can be S The measurement was performed in the same manner.
[0118] In the laminated film 10 of the present embodiment, the thickness T of the surface layer 2 is S The thickness T of the surface layer 2 may be 1.0 μm or more, 2.0 μm or more, or 3.0 μm or more. S The thickness may be 10.0 μm or less, 8.0 μm or less, or 5.0 μm or less.
[0119] Thickness T of surface layer 2 S The measurement can be performed using, for example, a transmission electron microscope (TEM) (product name "HT7820", manufactured by Hitachi High-Technologies Co., Ltd.) as a measuring device at a magnification of 10,000 times and an accelerating voltage of 100 kV. The thickness T of the surface layer 2 can be obtained by taking the arithmetic average of the thickness measurement values at at least 5 randomly selected locations. S .
[0120] In the laminated film 10 of the present embodiment, the thickness T of the bonding layer 3 is JThe thickness T of the bonding layer 3 may be 3.0 μm or more, 4.0 μm or more, or 5.0 μm or more. J It is particularly preferably 6.1 μm or more. J When the thickness is 6.1 μm or more, the bonding layer 3 exhibits particularly strong bonding properties.
[0121] In addition, the thickness T of the bonding layer 3 J The thickness may be 10.0 μm or less, 8.0 μm or less, or 7 μm or less.
[0122] Thickness T of the bonding layer 3 J The thickness T of the surface layer 2 can be S Calculate in the same way.
[0123] In the laminated film 10 of the present embodiment, the thickness T of the surface layer 2 is S The thickness T of the bonding layer 3 J The total value of T S +T J The thickness may be 6.0 μm or more, 8.0 μm or more, or 9.0 μm or more.
[0124] In addition, the above total value T S +T J The thickness may be 15.0 μm or less, 12.0 μm or less, or 10.0 μm or less.
[0125] In the laminated film 10 of the present embodiment, the thickness T of the bonding layer 3 is J Relative to the thickness T of the surface layer 2 S The thickness T of the bonding layer 3 J The total value of T S +T J The ratio [T J / (T S +T J )] can be greater than 0.30, can be greater than 0.40, and can also be greater than 0.50.
[0126] In addition, the above ratio [T J / (T S +T J )] can be 1.00 or less, 0.80 or less, 0.70 or less, or 0.65 or less.
[0127] As described above, in the laminated film 10 of the present embodiment, the thickness of the bonding layer 3 is set to T J μm, and when imaging Raman measurement based on Raman spectroscopy is performed on the bonding layer 3 after irradiation with active energy rays, the wavelength is 1730 cm-1 The intensity of the peak at which the peak top is observed is set as I A , will be at wave number 1635cm -1 The intensity of the peak at which the peak top is observed is set as I B When the above T and the above I A And the above I B The following relationship is satisfied.
[0128] Relational T J ×(I B / I A )≥15.0μm
[0129] In the laminated film 10 of the present embodiment, the above-mentioned [T J ×(I B / I A )] can be 16.0 μm or more. J ×(I B / I A )] can be 30.0 μm or less, can be 25.0 μm or less, can be 22.0 μm or less, and can also be 20.0 μm or less.
[0130] In the laminated film 10 of the present embodiment, I B / I A It may be 1.00 or more, 2.00 or more, or 3.00 or more. B / I A It may be 5.00 or less, or 4.00 or less.
[0131] In the laminated film 10 of the present embodiment, I A / I B It can be greater than 0.10, greater than 0.20, greater than 0.30, or greater than 0.30. A / I B It may be 0.60 or less, 0.50 or less, or 0.4 or less.
[0132] In the laminated film 10 of the present embodiment, [T J / (T S +T J )]×[I B / I A ] may be greater than 0.50, greater than 1.00, or greater than 1.50. J / (T S +T J )]×[I B / I A] can be 5.00 or less, 4.00 or less, 3.00 or less, 2.50 or less, or 2.00 or less.
[0133] The imaging Raman measurement based on the Raman spectroscopy method can be performed by measuring the Raman spectrum using a micro Raman spectrometer (trade name "alpha300RSA", manufactured by WITec).
[0134] In the measurement of the Raman spectrum, the Raman spectrum was obtained at 30,000 points of the cross section of the laminated film 10 in an area of 20 μm×15 μm under the conditions of a 100-times objective lens and an excitation wavelength of 532 nm.
[0135] In the obtained Raman spectrum, the wave number 75 cm -1 ~3780cm -1 The baseline was corrected by linear approximation and the wave number at 1730 cm was obtained. -1 The peak intensity I A , and at wave number 1635cm -1 The peak intensity I B .
[0136] In the laminated film 10 of the present embodiment, it is preferred that the bonding layer 3 has a bonding strength such that the bonding layer 3 does not peel off from the surface layer 2 even after the surface layer 2 is exposed to light for 144 hours or more.
[0137] Therefore, in the laminated film 10 of the present embodiment, the bonding layer 3 exhibits particularly strong bonding properties.
[0138] (Method for producing laminated film)
[0139] The method for producing a laminated film of the present embodiment comprises: applying a resin composition including a photocurable resin and an organic solvent capable of dissolving the cellulose triacetate on a base layer formed of a resin film including cellulose triacetate to form a coating layer; and heating the coating layer.
[0140] In the method for producing a laminated film according to the present embodiment, the heat treatment is performed so that the maximum temperature becomes 130° C. or higher.
[0141] The laminated film of this embodiment can be used, for example, Figure 3 The laminated film manufacturing apparatus 2000 shown in the figure is used for manufacturing.
[0142] In addition, as described below in the manufacturing method, at least a part of the base material original roll 1A becomes a base material layer.
[0143] like Figure 3As shown, the laminated film manufacturing apparatus 2000 comprises: a first continuous unwinding section 100, which continuously unwinds a substrate roll 1A containing triacetyl cellulose wound into a roll shape to the downstream; a pre-annealing section 200, which is arranged on the downstream side of the first continuous unwinding section 100 and pre-anneals the substrate roll 1A continuously unwound from the first continuous unwinding section 100; a first roller 300, which is arranged on the downstream side of the pre-annealing section 200 and is used to further convey the pre-annealed substrate roll 1A to the downstream side; and a die coater 400, which is arranged opposite to the conveying surface of the substrate roll 1A on the first roller 300 and is used to coat the exposed surface of the substrate roll 1A being conveyed by the first roller 300 with a photocurable resin and a solvent capable of dissolving the triacetyl cellulose. a resin composition containing an organic solvent; an oven 500, which is arranged on the downstream side of the first roller 300 and is used to heat the substrate roll 1A on which the coating layer of the above-mentioned resin composition is formed; an irradiation section 600, which is arranged on the downstream side of the oven 500 and is used to irradiate the above-mentioned coating layer formed on the substrate roll 1A with light such as ultraviolet rays (active energy rays); a second roller 700 and a third roller 800, which are arranged opposite to each other on the downstream side of the irradiation section 600, and sandwich the irradiated coating layer and the substrate roll 1A and further transport them to the downstream side; and a winding section 900, which is arranged on the downstream side of the second roller 700 and the third roller 800, and winds up the coating layer and the substrate roll 1A after being irradiated with light such as ultraviolet rays.
[0144] In addition, if Figure 3 As shown, the laminated film manufacturing apparatus 2000 comprises: a storage tank 1000, which stores the above-mentioned resin composition for coating by the die coater 400; and a second continuous discharge section 1100, which continuously discharges a protective film P wound into a roll for protecting the exposed surface of the coating layer after irradiation with ultraviolet rays, etc., to the second roller 700 and the third roller 800.
[0145] Below, using Figure 3 The method for producing a laminated film according to the present embodiment will be described using a laminated film production apparatus 2000 shown in FIG.
[0146] (Pre-annealing)
[0147] In the method for manufacturing a laminated film of the present embodiment, the substrate roll 1A continuously unrolled from the first continuous unrolling unit 100 is pre-annealed in the pre-annealing unit 200. By pre-annealing in the pre-annealing unit 200, stresses such as tensile residual stress and compressive residual stress remaining in the substrate roll 1A can be removed from the substrate roll 1A. Thus, it is possible to suppress damage such as rupture of the substrate roll 1A due to stress remaining in the substrate roll 1A during the manufacturing process of the laminated film.
[0148] In the present embodiment, the base material roll 1A is a base material roll containing cellulose triacetate. Therefore, the pre-annealing in the pre-annealing section 200 is preferably performed at a temperature in the range of 80° C. to 100° C.
[0149] (Formation of coating layer)
[0150] Next, the pre-annealed substrate roll 1A is conveyed to the first roller 300. The conveying speed (line speed) of the pre-annealed substrate roll 1A is preferably 20 m / h or more and 50 m / h or less. It should be noted that the conveying speed can be adjusted by appropriately adjusting the rotation speed of the first roller 300.
[0151] Then, using the die coater 400 disposed opposite to the first roll 300 , a resin composition containing a photocurable resin and an organic solvent capable of dissolving the cellulose triacetate is applied to the exposed surface of the pre-annealed substrate roll 1A to form a coating layer.
[0152] The resin composition contains an organic solvent capable of dissolving the cellulose triacetate. Therefore, the cellulose triacetate can be dissolved by the organic solvent in the surface layer portion of the substrate roll 1A on which the coating layer is formed as described above.
[0153] Coating using the die coater 400 can be implemented, for example, as follows: on the basis of using a 50μm thick PET spacer to make the thickness of the coating liquid ejection part of the die coater 400 reach 50μm, it is preferably implemented by setting the interval between the die lip of the die coater 400 and the substrate original roll 1A, that is, the die gap, to be greater than 300μm and less than 400μm.
[0154] Furthermore, the coating layer preferably has a thickness of 10 μm or more and 30 μm or less.
[0155] By setting the conveying speed of the pre-annealed base roll 1A in advance within the above-mentioned numerical range, the resin composition can be applied to the exposed surface of the pre-annealed base roll 1A with a nearly uniform thickness.
[0156] Examples of the organic solvent include the organic solvents described above, and among them, cyclopentanone is preferably used.
[0157] Examples of the photocurable resin include the photocurable resins described above, and among these, urethane (meth)acrylate resins are preferably used.
[0158] It should be noted that in order to initiate the polymerization reaction of the above-mentioned photocurable resin by irradiation with ultraviolet rays or the like, the above-mentioned resin composition preferably contains a photopolymerization initiator. When the above-mentioned photocurable resin is a carbamate (meth)acrylate resin, the above-mentioned photopolymerization initiator is preferably 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propanone.
[0159] In addition, the resin composition preferably contains a tackifier so as to have a viscosity suitable for coating. As the tackifier, smectite is preferably contained.
[0160] It should be noted that the resin composition may be prepared, for example, by stirring and mixing the organic solvent, the photocurable resin, the photopolymerization initiator, the tackifier, and the like in the storage tank 1000 .
[0161] (Heat treatment)
[0162] Next, the base material roll 1A to which the formed coating layer is attached is conveyed to the oven 500 .
[0163] The conveying speed (line speed) of the base material roll 1A to which the coating layer is attached is preferably 20 m / h or more and 50 m / h or less as described above.
[0164] By setting the conveying speed in advance within the above-mentioned numerical range, the coating layer can be efficiently heated in the oven 500 .
[0165] In the present embodiment, the heating process in the oven 500 is performed so that the maximum temperature in the oven becomes 130° C. or higher.
[0166] As described above, the cellulose triacetate contained in the base roll 1A has a glass transition temperature Tg of 130° C. By setting the maximum temperature in the oven to 130° C. or higher, the cellulose triacetate dissolved in the organic solvent can be transformed from a glass state to a rubber state in the surface layer of the base roll 1A.
[0167] As a result, the molecular motion of the cellulose triacetate can be activated in the surface layer portion of the base material roll 1A.
[0168] Thereby, a part of the cellulose triacetate existing in the surface layer part of the base material original roll 1A can be diffused into the said coating layer.
[0169] Furthermore, in the portion of the coating layer where the cellulose triacetate is diffused, the cellulose triacetate and the photocurable resin are mixed with each other without being separated, thereby forming a compatible layer.
[0170] It should be noted that the portion of the coating layer where the cellulose triacetate is not diffused constitutes a surface layer.
[0171] The drying time until the maximum temperature reaches 130° C. or higher is preferably 10 seconds or longer, more preferably 20 seconds or longer, and even more preferably 30 seconds or longer.
[0172] The drying time at which the maximum temperature reaches 130° C. or higher may be 60 seconds or less, 50 seconds or less, or 40 seconds or less.
[0173] By setting the drying time at a maximum temperature of 130° C. or higher within the above numerical range, part of the cellulose triacetate contained in the surface layer of the base material roll 1A dissolved in the organic solvent can be efficiently diffused into the coating layer.
[0174] The maximum temperature in the heat treatment is preferably 200° C. or lower, more preferably 180° C. or lower, and further preferably 150° C. or lower.
[0175] By performing the heat treatment in this manner, a laminated film can be obtained in which an adhesive layer (compatible layer) and a surface layer are sequentially laminated on the base material roll 1A.
[0176] It should be noted that the above-mentioned heat treatment may also be carried out in multiple times at different temperatures. For example, after the first stage heat treatment is carried out at a temperature of 50°C or more and 90°C or less, the second stage heat treatment may be carried out at a temperature of 130°C or more, and then the third stage heat treatment may be carried out at a temperature of 50°C or more and 90°C or less.
[0177] By performing the heat treatment at different temperatures in a plurality of times, it is possible to suppress the sudden boiling of the organic solvent in the coating layer due to a rapid temperature rise, thereby suppressing the appearance defect of the coating layer due to the sudden boiling.
[0178] (illumination)
[0179] Next, the coating layer and the base material roll 1A after the heat treatment are conveyed to the light irradiation unit 600 .
[0180] The conveying speed (line speed) of the coating layer and the base material roll 1A after the heat treatment is preferably 20 m / h or more and 50 m / h or less as described above.
[0181] By setting the conveying speed in advance within the above-described numerical range, the light irradiation unit 600 can efficiently irradiate the coating layer after the heat treatment with light or the like.
[0182] The irradiation unit 600 preferably irradiates active energy rays, and among the active energy rays, preferably irradiates ultraviolet rays (for example, ultraviolet rays with a wavelength of 365 nm). Hereinafter, irradiation with active energy rays may be simply described as irradiation.
[0183] The above active energy rays are preferably emitted at a cumulative amount of 100 mJ / cm 2 The above method is preferably used to irradiate at 150 mJ / cm 2 The above method is preferably used to irradiate at 200 mJ / cm 2 Irradiation in the above manner.
[0184] The upper limit of the above-mentioned cumulative light intensity is usually 500 mJ / cm 2 .
[0185] As described above, by irradiating the coating layer and the base material roll 1A after the heat treatment, the curing reaction can be carried out in the portion of the coating layer where the cellulose triacetate is diffused (corresponding to the bonding layer) using the photocurable resin in a state of being entangled with the cellulose triacetate.
[0186] On the other hand, in the portion of the coating layer where the cellulose triacetate is not diffused (corresponding to the surface layer), the photocurable resin which is not entangled with the cellulose triacetate can be used to cause a curing reaction to proceed. Thus, in the laminated film of this embodiment, the surface layer can have sufficient strength.
[0187] In addition, since the polymerization reaction of the photocurable resin in a state of being entangled with the cellulose triacetate proceeds in the bonding layer, the bonding layer can be cured while the cellulose triacetate is appropriately maintained in the bonding layer.
[0188] Furthermore, since the cured bonding layer is formed in a state where the cellulose triacetate is appropriately maintained, the bonding layer can exhibit good bonding properties to the base material roll 1A.
[0189] In addition, since the photocurable resin described above becomes a matrix resin and is continuous in the surface layer and the bonding layer, good bonding property is also exhibited between the surface layer and the bonding layer.
[0190] (Reeling up of laminated film)
[0191] Next, the laminated film after the light exposure is conveyed to the winding unit 900 by the second roller 700 and the third roller 800 , and the laminated film is wound up by the winding unit 900 .
[0192] The conveying speed (line speed) of the laminated film after light irradiation is preferably 20 m / h or more and 50 m / h or less as described above.
[0193] In addition, in the manufacturing method of the laminated film of this embodiment, the laminated film after light irradiation is wound up while the protective film P is continuously unrolled from the second continuous unrolling unit 1100 toward the second roll 700 and the third roll 800 .
[0194] In addition, the protective film P is continuously unrolled so as to cover the exposed surface of the coating layer (that is, the exposed surface of the surface layer) in the laminated film.
[0195] In order to appropriately cover the exposed surface of the surface layer with the protective film P, the continuous feeding speed of the protective film P is preferably set to the same speed as the conveying speed (line speed) of the laminated film after light irradiation.
[0196] By the above operation, the laminated film of the present embodiment can be obtained in a form in which the bonding layer and the surface layer are sequentially arranged on the base material roll 1A, and the protective film P is further arranged on the surface of the surface layer.
[0197] Matters disclosed in this specification include the following aspects.
[0198] (1) A laminated film comprising:
[0199] Base material layer,
[0200] a surface layer disposed on the substrate layer, and
[0201] a bonding layer disposed between the substrate layer and the surface layer to bond the substrate layer and the surface layer,
[0202] The substrate layer is formed of a resin film containing cellulose triacetate,
[0203] The surface layer is formed of a resin composition containing a photocurable resin.
[0204] The bonding layer is formed in the form of a compatibility layer in which a part of the cellulose triacetate contained in the base layer and a part of the photocurable resin contained in the surface layer are compatible with each other.
[0205] The thickness of the bonding layer is T J μm,
[0206] When the bonding layer was subjected to imaging Raman measurement based on Raman spectroscopy at a wave number of 1730 cm -1 The intensity of the peak at which the peak top is observed is set as I A , will be at wave number 1635cm -1 The intensity of the peak at which the peak top is observed is set as I Bhour,
[0207] The above T J , the above I A , and the above I B Satisfies the following relationship:
[0208] T J ×I B / I A ≥15.0μm.
[0209] (2) The laminated film according to (1) above, wherein
[0210] The bonding layer has a thickness of 6.1 μm or more.
[0211] (3) The laminated film according to (1) or (2) above, wherein
[0212] The bonding layer has a bonding strength such that the bonding layer is not peeled off from the surface layer after the surface layer is exposed to light for more than 144 hours.
[0213] (4) The laminated film according to any one of (1) to (3) above, wherein
[0214] The surface layer has a function as a hard coat layer.
[0215] (5) A method for producing a laminated film, the method comprising:
[0216] forming a coating layer by applying a resin composition including a photocurable resin and an organic solvent capable of dissolving the cellulose triacetate on a base layer formed of a resin film including cellulose triacetate; and
[0217] The coating layer is heated and dried.
[0218] In this method, the heat drying is performed so that the maximum temperature becomes 130° C. or higher.
[0219] (6) The method for producing a laminated film according to (5) above, wherein:
[0220] In the heat drying, heating at the maximum temperature is performed for 20 seconds or more.
[0221] It should be noted that the laminated film and the method for producing the laminated film of the present invention are not limited to the above-mentioned embodiment.
[0222] In addition, the laminated film and the method for producing the laminated film of the present invention are not limited by the above-mentioned effects.
[0223] The laminated film and the method for producing the laminated film of the present invention can be modified in various ways without departing from the gist of the present invention.
[0224] Example
[0225] Next, the present invention will be described in more detail with reference to the following examples. The following examples are intended to describe the present invention in more detail, but are not intended to limit the scope of the present invention.
[0226] <Example 1>
[0227] (Base material layer)
[0228] As the substrate layer, a triacetyl cellulose substrate (trade name "TJ40UL" manufactured by Fujifilm Corporation, thickness 40 μm) was used.
[0229] (Preparation of resin composition)
[0230] To a mixed solvent (PGM:CPN=60:40) of propylene glycol monomethyl ether (PGM) and cyclopentanone (CPN) as an organic solvent, 3 parts by mass of a photopolymerization initiator (trade name "OMNIRAD907" manufactured by BASF), 100 parts by mass of an ultraviolet curable urethane acrylate resin (trade name "LUXYDIR 17-806" manufactured by DIC, solid content concentration 80%) as a photocurable resin, and 0.01 parts by mass of a leveling agent (trade name "GRANDIC PC4100" manufactured by DIC) were added, and the mixture was stirred for 15 minutes using a disperser to prepare the resin composition of Example 1.
[0231] (Fabrication of bonding layer and surface layer)
[0232] The resin composition of Example 1 was applied onto a cellulose triacetate substrate as a substrate layer while the cellulose triacetate substrate was conveyed at a conveying speed (line speed) of 25 m / s to form a coating layer, and then a heat treatment was performed in an oven.
[0233] It should be noted that the coating layer is formed by using Figure 3 The invention is implemented by the device shown.
[0234] The heat treatment was performed by first heating at 90° C. for 25 seconds, then second heating at 130° C. for 25 seconds, and finally third heating at 90° C. for 25 seconds.
[0235] Thereby, the coating layer is dried.
[0236] The resin composition of Example 1 was applied onto the cellulose triacetate substrate so that the thickness after drying would be 9.8 μm.
[0237] Use a high pressure mercury lamp to achieve a cumulative light intensity of 245mJ / cm 2 The dried coating layer was irradiated with ultraviolet light having a wavelength of 365 nm.
[0238] In this way, a bonding layer and a surface layer were sequentially produced on the above-mentioned cellulose triacetate substrate.
[0239] That is, a laminated film of Example 1 in which the bonding layer and the surface layer were laminated in this order on the base layer was obtained.
[0240] <Example 2>
[0241] In the preparation of the bonding layer and the surface layer, the first drying was carried out at 60°C for 25 seconds, and the above-mentioned resin composition was coated on the above-mentioned base layer in a manner so that the thickness after drying reached 9.4 μm. In addition, a laminated film of Example 2 in which a bonding layer and a surface layer were sequentially laminated on a base layer was obtained in the same manner as Example 1.
[0242] <Example 3>
[0243] In the preparation of the bonding layer and the surface layer, the second drying was carried out at 140°C for 25 seconds, and the above-mentioned resin composition was coated on the above-mentioned base layer in a manner so that the thickness after drying reached 9.5 μm. In addition, a laminated film of Example 3 in which a bonding layer and a surface layer were sequentially laminated on a base layer was obtained in the same manner as Example 1.
[0244] <Example 4>
[0245] In the preparation of the bonding layer and the surface layer, the conveying speed (line speed) was set to 30 m / s, and the above-mentioned resin composition was coated on the above-mentioned base layer in a manner so that the thickness after drying reached 9.0 μm. In addition, a laminated film of Example 4 in which a bonding layer and a surface layer were sequentially laminated on a base layer was obtained in the same manner as Example 1.
[0246] <Comparative Example 1>
[0247] In the preparation of the bonding layer and the surface layer, the second drying was carried out at 120°C for 25 seconds, and the above-mentioned resin composition was coated on the above-mentioned base layer in a manner so that the thickness after drying reached 10.1 μm. In addition, a laminated film of Comparison Example 1 in which a bonding layer and a surface layer were sequentially laminated on a base layer was obtained in the same manner as in Example 1.
[0248] <Comparative Example 2>
[0249] In the preparation of the bonding layer and the surface layer, the second drying was carried out at 110°C for 25 seconds, and the above-mentioned resin composition was coated on the above-mentioned base layer in a manner so that the thickness after drying reached 9.7 μm. In addition, a laminated film of Comparison Example 2 in which a bonding layer and a surface layer were sequentially laminated on a base layer was obtained in the same manner as Example 1.
[0250] <Comparative Example 3>
[0251] In the preparation of the bonding layer and the surface layer, the resin composition was applied to the substrate layer in a manner such that the thickness after drying reached 9.6 μm, and a laminated film of Comparative Example 3 in which the bonding layer and the surface layer were sequentially laminated on the substrate layer was obtained in the same manner as in Example 1.
[0252] In addition, the manufacturing conditions of the laminated film of each example are shown in Table 1 below.
[0253] [Table 1]
[0254]
[0255] (Thickness measurement)
[0256] The thickness T of the surface layer of each laminated film was measured. S and the thickness of the bonding layer T J The thickness of the surface layer is T S and the thickness of the bonding layer T J The measurements were performed according to the method described in the first embodiment. The results are shown in Table 2 below.
[0257] It should be noted that the thickness T of the surface layer is also shown in Table 2 below. S and the thickness of the bonding layer T J The total value of and the thickness T of the surface layer S and the thickness of the bonding layer T J The total value of the bonding layer thickness T J .
[0258] (Imaging Raman Determination)
[0259] The bonding layer of the laminated film of each example was subjected to imaging Raman measurement based on Raman spectroscopy, and the wavelength of 1730 cm- 1 The peak intensity I of the peak at the top of the peak is observed A , and at wave number 1635cm- 1 The peak intensity I of the peak at the top of the peak is observed B The imaging Raman measurement was performed according to the method described in the first embodiment above.
[0260] Then, the peak intensity I was calculated for each laminated film. A Relative to the peak intensity I B The ratio (I A / I B ), and peak intensity I B Relative to the peak intensity I A The ratio (I B / I A ).
[0261] In addition, T J ×I B / I A , and [T J / (T S +T J )]×[I B / I A ].
[0262] The results are shown in Table 2 below.
[0263] (Durable Adhesion)
[0264] The laminated film of each example was evaluated for durable adhesion. The evaluation of durable adhesion was carried out by a fading adhesion test. The fading adhesion test is a test for evaluating durable adhesion (weather resistance) under ultraviolet irradiation.
[0265] In the tests in this specification, the laminated film of each example was put into an ultraviolet long-life discoloration meter (manufactured by SUGA Testing Instruments Co., Ltd., model "U48HB"), and the laminated film was irradiated with ultraviolet rays for a predetermined period of time.
[0266] In the fading test, a carbon arc lamp was used as the light source, the black panel temperature was set to 63°C, and the radiation intensity (integrated illuminance at 300 to 700 nm) was set to 500 W / m 2 , the ambient temperature is set to 40°C, and the ambient humidity is set to the range of 10%RH to 40%RH.
[0267] The laminated film was subjected to the following cross-cut peeling test 48 hours, 96 hours, 144 hours, 192 hours, 240 hours, and 500 hours after the start of ultraviolet irradiation, and the adhesion of the bonding layer to the surface layer was evaluated.
[0268] In addition, as a laminated film, the laminated film which has a plane size of 10 mm×10 mm was used.
[0269] (Checkerboard peel test)
[0270] Using a cutter, 100 (10×10) 1 mm square grids were formed in a checkerboard pattern on the exposed surface of the surface layer.
[0271] Next, an adhesive tape (manufactured by Sekisui Chemical Co., Ltd., trade name "Cellotape (registered trademark) No. 252") was attached to the exposed surface of the surface layer, and then peeled off.
[0272] This operation was repeated twice, and the ultraviolet irradiation time at which no peeling occurred in 100 grids of 1 mm square was examined.
[0273] For example, if the evaluation result is 48 hours (h), it means that when the ultraviolet irradiation is performed for 48 hours (h), none of the 100 1 mm square grids peel off, but when the ultraviolet irradiation is performed for 96 hours (h), at least one of the 100 1 mm square grids peels off.
[0274] In addition, the same contents are shown also when the evaluation results are 96 hours (h) and 144 hours (h).
[0275] When the evaluation time is 500 hours (h), it means that even when the ultraviolet irradiation is performed for 500 hours (h), no 1 mm square grid is peeled off.
[0276] The above-mentioned cross-grid peeling test is based on JIS K5600, but a point in which the number of 1 mm square grids is changed is 100 (in JIS K5600, the number of 1 mm square grids is 25).
[0277] The results are shown in Table 2 below.
[0278] (Steel wool (SW) resistance)
[0279] The laminated film of each example was evaluated for steel wool (SW) resistance. The SW resistance was evaluated under a load of 400 g or 800 g.
[0280] The SW resistance evaluation was carried out in the following procedure.
[0281] (1) The laminated film of each example was placed on a glass plate with the surface on which the surface layer was not formed facing downward.
[0282] (2) After steel wool #0000 was evenly placed on the side surface (smooth surface) of a cylinder with an outer diameter of 11 mm to obtain a cylinder with steel wool, the side surface of the cylinder with steel wool was reciprocated 10 times on the surface (exposed surface) of the surface layer of the laminated film of each example.
[0283] It should be noted that the conditions for reciprocating the side surface of the cylinder with steel wool were a load of 400 g or 800 g and a speed of about 100 mm / sec.
[0284] (3) The state of the scratches on the surface layer of the laminated film of each example was confirmed by visual observation and evaluated according to the following criteria. The results are shown in Table 2 below.
[0285] Good: No scratches were observed on the surface of the surface layer by visual observation.
[0286] Unacceptable: Through visual observation, at least a few scratches are observed on the surface of the surface layer.
[0287] (Appearance)
[0288] The appearance of the laminated film of each example was evaluated.
[0289] The appearance was evaluated by irradiating the laminated film of each example from the surface layer side with sodium lamp in a dark room and visually inspecting the reflection.
[0290] Specifically, the appearance was evaluated by visually checking whether or not there were defects such as bubbles or foreign matter of 100 μm or more in the surface layer.
[0291] It should be noted that the irradiation with sodium lamp light was performed from a position 50 cm above the surface layer.
[0292] In addition, the appearance was evaluated according to the following criteria. The results are shown in Table 2 below.
[0293] Good: No defects were found.
[0294] Unacceptable: At least a few defects were identified.
[0295] [Table 2]
[0296]
[0297] It can be confirmed from Table 2 that when the thickness of the bonding layer is set to T J μm, and when the above-mentioned bonding layer after ultraviolet irradiation was subjected to imaging Raman measurement based on Raman spectroscopy, the wavelength of the bonding layer was 1730 cm- 1 The intensity of the peak at which the peak top is observed is set as I A , will be at wave number 1635cm- 1 The intensity of the peak at which the peak top is observed is set as I B When the above T J , the above I A And the above I B Satisfy the relationship T J×I B / I A The laminated films of each example with a thickness of 15 μm or more were excellent in durable adhesion.
[0298] That is, it was confirmed that the laminated film of each example includes a bonding layer having sufficient bonding strength.
Claims
1. A laminated film comprising: Base material layer, a surface layer disposed on the substrate layer, and a bonding layer disposed between the base layer and the surface layer to bond the base layer and the surface layer, The substrate layer is formed of a resin film containing cellulose triacetate, The surface layer is formed of a resin composition containing a photocurable resin, The bonding layer is formed in the form of a compatibility layer in which a part of the cellulose triacetate contained in the base layer and a part of the photocurable resin contained in the surface layer are compatible with each other. The thickness of the bonding layer is set as T J μm, When the bonding layer is subjected to imaging Raman measurement based on Raman spectroscopy at a wave number of 1730 cm -1 The intensity of the peak at the top of the peak is set as I A , will be at wave number 1635cm -1 The intensity of the peak at the top of the peak is set as I B hour, The T J , said I A And the I B Satisfies the following relationship: T J ×I B / I A ≥15.0μm。 2. The laminated film according to claim 1, wherein The thickness T of the bonding layer J It is 6.1μm or more.
3. The laminated film according to claim 1 or 2, wherein After the surface layer is exposed to light for more than 144 hours, the bonding layer still has a bonding strength that does not peel off from the surface layer.
4. The laminated film according to claim 1 or 2, wherein The surface layer has the function of a hard coating layer.
5. A method for producing a laminated film, the method comprising: forming a coating layer by coating a resin composition including a photocurable resin and an organic solvent capable of dissolving the cellulose triacetate on a base layer formed of a resin film including cellulose triacetate; and The substrate layer and the coating layer are subjected to a heat treatment. in, The heat treatment is performed so that the maximum temperature becomes 130° C. or higher.
6. The method for producing a laminated film according to claim 5, wherein: In the heat treatment, heating is performed at the highest temperature for 20 seconds or more.