Ink-jet printing process capable of eliminating thin film contour and electroluminescent device thereof
Through means such as plasma treatment and simulated annealing algorithms, the problem of substrate surface characteristics affecting the spread of ink droplets is solved, eliminating film contours and improving the performance of electroluminescent devices, including improving luminous efficiency and chemical stability.
Patent Information
- Application Number
- CN202410982807.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the production process of electroluminescent devices, uneven surface roughness, hydrophilic or hydrophobic properties of the substrate, and poor ink compatibility lead to irregular contours and positioning deviations of ink droplets on the substrate, affecting the molding quality of the film.
Plasma treatment is used to improve the hydrophilicity and adhesion of the flexible substrate surface, and the simulated annealing algorithm and model predictive control (MPC algorithm) are used to ensure uniform inkjet thickness, and the reflective electrode layer and zinc oxide microcavity layer are combined to improve light extraction efficiency and chemical stability.
Effectively eliminate film contours, improve luminous efficiency and brightness, reduce power consumption, enhance the light extraction efficiency and chemical stability of the device, and ensure the stability of the production process and product consistency.
Smart Images

Figure BDA0004956563540000031 
Figure BDA0004956563540000071 
Figure FDA0004956563530000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electroluminescent device inkjet printing, in particular to an inkjet printing process capable of eliminating film profile and an electroluminescent device thereof. Background Art
[0002] Electroluminescent devices are display devices that use electroluminescent materials to emit light when stimulated. They can be divided into AC and DC types according to the excitation voltage. Both can be made of powder or thin film electroluminescent materials. DC electroluminescent powder contains a layer of zinc sulfide about 50 microns thick, doped with fine-grained manganese, and copper sulfide coated on the outside. This device requires a large current molding process to establish a stable working area at the anode. It can achieve a brightness of about 1000 candela / m2 and a half-life of 1000 hours. Other studies on AC thin film electroluminescence include directly combining it with the integrated matrix of thin film transistors, combining it with a black layer and a thin film transistor actuator to improve the contrast, and using AC thin film electroluminescence with storage properties as the screen of an electron beam tube, using an AC voltage to maintain its storage properties and using an electron beam for site selection and display.
[0003] Inkjet printing is a highly efficient special printing method. It can be used in packaging industry production lines to quickly print production date, batch number, barcode and other contents. A dot matrix image is an image depicted by colored dots called pixels. When editing a dot matrix image, the pixels are modified. Because the data that constitutes the dot matrix image is fixed in a grid of a specific size, when the dot matrix image is enlarged, the edges of the image will become blurred. The dot matrix image principle software can be used for editing and processing dot matrix images, including image adjustment, mask processing, and geometric changes of images. It can also be used for the production of special effects, including rotation, size change, clarity emphasis and softening functions, virtual shadow generation, gradient adjustment and color correction.
[0004] At present, inkjet printing technology is used in the production process of electroluminescent devices. Inkjet printing technology can be used to deposit organic light-emitting materials, charge transfer materials, etc. onto a substrate, making the manufacture of OLEDs more flexible and efficient, and capable of achieving high-precision patterning. However, during use, the surface roughness, hydrophilicity or hydrophobicity and other properties of the substrate will affect the spreading of ink droplets on the substrate. If the surface of the substrate is uneven or has poor compatibility with the ink, the ink droplets will form irregular contours on the substrate, and positioning deviations will easily lead to thin film contours. Therefore, those skilled in the art provide an inkjet printing process and an electroluminescent device that can eliminate thin film contours, in order to solve the problems raised in the above background technology. Summary of the invention
[0005] 1. Technical issues to be solved
[0006] In view of the shortcomings of the prior art, the present invention provides an inkjet printing process and an electroluminescent device that can eliminate the thin film profile, which solves the problem that the surface roughness, hydrophilicity or hydrophobicity of the substrate will affect the spreading of ink droplets on the substrate. If the surface of the substrate is uneven or has poor compatibility with the ink, the ink droplets will form irregular profiles on the substrate, and positioning deviations will easily lead to the problem of thin film profile.
[0007] (II) Technical solution
[0008] To achieve the above objectives, the present invention is implemented by the following technical solutions: an inkjet printing process capable of eliminating the film profile comprises the following steps:
[0009] S1. Design: Use computer-aided design software and image processing software to design the required patterns and texts, and convert the designed files into a format that can be recognized by the printer, such as PDF or a dedicated printing format;
[0010] S2. Material preparation, transparent electrode, reflective electrode, flexible substrate and phosphorescent material, preparation of ink containing luminescent material anode ink, charge transport material ink, microcavity layer ink, hole layer ink, phosphorescent ink, reflective electrode layer ink and luminescent electrode cathode ink;
[0011] S3. Surface treatment of flexible substrates: using plasma to treat the surface roughness of flexible substrates. Plasma treatment can significantly improve the hydrophilicity, adhesion, biocompatibility and other properties of the substrate surface, thereby providing better surface conditions for subsequent printing, coating, bonding and other processes;
[0012] S3.1. Pretreatment of the flexible substrate: cleaning the surface of the flexible substrate to remove grease and dust from the surface;
[0013] S3.2. Place the cleaned flexible substrate into the vacuum chamber of the plasma treatment equipment, start the vacuum pump, and reduce the pressure in the vacuum chamber to the level required for plasma treatment; inject argon gas, excite the gas by radio frequency, generate plasma, and set the plasma treatment time to 40s;
[0014] S3.3. After the plasma treatment is completed, turn off the RF or microwave generator, stop the plasma generation, and slowly restore the atmospheric pressure in the vacuum chamber to avoid damage to the substrate due to pressure difference;
[0015] S3.4. After the treatment is completed, the substrate is removed and a subsequent drying or cooling treatment is performed;
[0016] S3.5. Use contact angle meter, X-ray photoelectron spectroscopy (XPS) and other equipment to check the hydrophilicity and chemical composition of the substrate surface;
[0017] S3.6. Adhesion test An adhesion test was performed using a tape test to evaluate the effect of the plasma treatment;
[0018] S4. Positioning calibration, printing calibration patterns on ordinary paper to evaluate the printing quality, using simulated annealing algorithm to find the global optimal solution, simulating the physical annealing process, that is, heating and slowly cooling the metal to reduce its internal defects to reach the lowest energy state;
[0019] S4.1. Randomly select an initial solution S, set the initial temperature T and cooling rate α, and at the current temperature, randomly select a neighborhood solution, calculate the difference ΔE between the new solution and the current solution, and if ΔE<0, accept the new solution as the current solution. If ΔE>0, accept the new solution with a certain probability, which is usually given by the Metropolis criterion.
[0020]
[0021] Repeat the above process until the preset number of iterations is reached and the system reaches a balanced state;
[0022] S4.2. Gradually reduce the temperature T = α*T, and repeat the iterative process until the temperature drops sufficiently low or the system reaches a stable state. When the temperature is sufficiently low or the system reaches a stable state, the algorithm terminates;
[0023] S5. Calculate the printing thickness and establish a mathematical model to describe the dynamic behavior of the system, including the state equation and output equation of the system;
[0024] S5.1. Based on the system model, the MPC algorithm predicts the system output in the future in each control cycle. The MPC algorithm determines the control input by solving an optimization problem. The optimization problem includes the objective function, constraints and prediction model.
[0025] S5.2. In each control cycle, the MPC algorithm solves an optimization problem to find the optimal control input sequence. From the optimal control input sequence obtained, the MPC algorithm only implements the control input at the current moment. Then, the system state is updated according to the actual system dynamics.
[0026] S5.3. In the next control cycle, the system state will be updated, and the MPC algorithm will repeat the above process to predict future behavior and optimize the control input. The system model is:
[0027]
[0028] in is the system at time step The state of uk is the control input, A and B are the system matrices. By precisely controlling the thickness, the MPC algorithm can ensure the consistency and quality of the product. The MPC algorithm can enhance the stability of the system and reduce fluctuations in the production process by predicting future behavior and adjusting the control input in advance, making the inkjet thickness more uniform. Uniform thickness helps ensure that the charge is evenly distributed in the light-emitting layer, thereby improving the luminous efficiency and brightness, and improving the color purity and color gamut.
[0029] S6. Printing inkjet printing, place the back of the flexible substrate inside the inkjet printing device, add the ink with the reflective electrode into the ink box, start the inkjet printing device, print the reflective electrode on the back surface of the flexible substrate, the thickness of the reflective electrode layer is 10nm, clean up the remaining ink inside the printing nozzle, turn the flexible substrate over, add the ink with the transparent electrode anode into the oil box, start the inkjet printing device, print the anode pattern on the flexible substrate, and then replace the hole ink, phosphorescent ink, microcavity layer ink, charge transfer layer ink and light-emitting electrode cathode ink for inkjet printing in sequence, the thickness of the hole layer is 5nm, the thickness of the phosphorescent layer is 5nm, the thickness of the microcavity layer is 10nm, the thickness of the charge transfer layer is 5nm, and the thickness of the light-emitting electrode cathode layer and the light-emitting electrode anode layer are both 5nm;
[0030] S7. Processing and packaging: heat-treat the printed film to improve the crystallinity and electrical properties of the material, check the accuracy and uniformity of the printed pattern, test the electrical properties of the OLED device, assemble the OLED device with other components, and complete the final packaging of the OLED device to ensure its stability and reliability during use.
[0031] Preferably, the simulated annealing algorithm receives a criterion to define an energy function for evaluating the quality of the solution. When the algorithm ends, the current solution S is output as the global optimal solution. The simulated annealing algorithm can jump out of the local optimal solution by simulating the physical annealing process, thereby increasing the probability of finding the global optimal solution. The simulated annealing algorithm helps to find the global optimal position configuration, rather than just staying at the local optimal solution, to optimize performance indicators.
[0032] An electroluminescent device includes a reflective electrode layer responsible for reflecting light emitted from a light-emitting layer to improve the light extraction efficiency of the device;
[0033] Flexible substrates break away from the limitations of traditional rigid materials and achieve lighter, more portable and more durable designs;
[0034] The light-emitting electrode anode layer is made of transparent conductive material and is used to inject positive charges;
[0035] A hole layer, used to improve the electron transfer efficiency between the anode and the light-emitting layer and the phosphor layer;
[0036] The phosphor layer, as the light-emitting layer of the organic light-emitting diode, emits light through the recombination of electrons and holes, which determines the light-emitting color and efficiency of the OLED;
[0037] A microcavity layer, which helps electrons move through the device and regulates light-emitting efficiency;
[0038] A charge transport layer, which helps electrons and holes to be transported from the external electrodes to the phosphor layer to enhance the charge injection efficiency;
[0039] The cathode layer is usually made of metal materials such as aluminum or calcium, which is used to inject electrons.
[0040] Preferably, the microcavity layer is a distributed Bragg reflector made of zinc oxide. Zinc oxide has a relatively high refractive index and can achieve high reflectivity when alternately stacked with a low refractive index material.
[0041] (III) Beneficial effects
[0042] The invention provides an inkjet printing process capable of eliminating the thin film profile and an electroluminescent device thereof.
[0043] It has the following beneficial effects:
[0044] 1. In the present invention, by using plasma-treated two end surfaces of the flexible substrate, the polar groups on the surface of the flexible substrate are increased, thereby increasing the surface energy, enhancing the adhesion with ink, adhesive, etc., and reducing the generation of film profiles. The reflective electrode layer can reflect the light emitted from the light-emitting layer back to the outside, and the added reflective electrode layer can improve the light extraction efficiency of the device and enhance the luminous brightness. Improving the light extraction efficiency means that at the same brightness, the current required by the device is smaller, thereby reducing power consumption.
[0045] 2. In the present invention, zinc oxide has a relatively high refractive index. When alternately stacked with low-refractive index materials, high reflectivity can be achieved, which is helpful for improving light extraction efficiency and enhancing device performance. Zinc oxide has good chemical stability and can resist chemical corrosion in the environment, ensuring stable performance of the device during long-term use, and has good thermal stability.
[0046] 3. In the present invention, the simulated annealing algorithm can jump out of the local optimal solution and increase the probability of finding the global optimal solution by simulating the physical annealing process. The simulated annealing algorithm helps to find the global optimal position configuration instead of just staying at the local optimal solution, so as to optimize performance indicators and reduce the generation of film contours.
[0047] 4. In the present invention, by precisely controlling the thickness, the MPC algorithm can ensure the consistency and quality of the product. By predicting future behavior and adjusting the control input in advance, the MPC algorithm can enhance the stability of the system, reduce fluctuations in the production process, and make the inkjet thickness more uniform. Uniform thickness helps to ensure that the charge is evenly distributed in the light-emitting layer, thereby improving the luminous efficiency and brightness, and improving the color purity and color gamut. DETAILED DESCRIPTION
[0048] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] Embodiment 1:
[0050] An embodiment of the present invention provides an inkjet printing process capable of eliminating a thin film profile, comprising the following steps:
[0051] S1. Design: Use computer-aided design software and image processing software to design the required patterns and texts, and convert the designed files into a format that can be recognized by the printer, such as PDF or a dedicated printing format;
[0052] S2. Material preparation, transparent electrode, reflective electrode, flexible substrate and phosphorescent material, preparation of ink containing luminescent material anode ink, charge transport material ink, microcavity layer ink, hole layer ink, phosphorescent ink, reflective electrode layer ink and luminescent electrode cathode ink;
[0053] S3. Surface treatment of flexible substrates: using plasma to treat the surface roughness of flexible substrates. Plasma treatment can significantly improve the hydrophilicity, adhesion, biocompatibility and other properties of the substrate surface, thereby providing better surface conditions for subsequent printing, coating, bonding and other processes;
[0054] S3.1. Pretreatment of the flexible substrate: cleaning the surface of the flexible substrate to remove grease and dust from the surface;
[0055] S3.2. Place the cleaned flexible substrate into the vacuum chamber of the plasma treatment equipment, start the vacuum pump, and reduce the pressure in the vacuum chamber to the level required for plasma treatment; inject argon gas, excite the gas by radio frequency, generate plasma, and set the plasma treatment time to 40s;
[0056] S3.3. After the plasma treatment is completed, turn off the RF or microwave generator, stop the plasma generation, and slowly restore the atmospheric pressure in the vacuum chamber to avoid damage to the substrate due to pressure difference;
[0057] S3.4. After the treatment is completed, the substrate is removed and a subsequent drying or cooling treatment is performed;
[0058] S3.5. Use contact angle meter, X-ray photoelectron spectroscopy (XPS) and other equipment to check the hydrophilicity and chemical composition of the substrate surface;
[0059] S3.6. Adhesion test An adhesion test was performed using a tape test to evaluate the effect of the plasma treatment;
[0060] S4. Positioning calibration, printing calibration patterns on ordinary paper to evaluate the printing quality, using simulated annealing algorithm to find the global optimal solution, simulating the physical annealing process, that is, heating and slowly cooling the metal to reduce its internal defects to reach the lowest energy state;
[0061] S4.1. Randomly select an initial solution S, set the initial temperature T and cooling rate α, and at the current temperature, randomly select a neighborhood solution, calculate the difference ΔE between the new solution and the current solution, and if ΔE<0, accept the new solution as the current solution. If ΔE>0, accept the new solution with a certain probability, which is usually given by the Metropolis criterion.
[0062]
[0063] Repeat the above process until the preset number of iterations is reached and the system reaches a balanced state;
[0064] S4.2. Gradually reduce the temperature T = α*T, and repeat the iterative process until the temperature drops sufficiently low or the system reaches a stable state. When the temperature is sufficiently low or the system reaches a stable state, the algorithm terminates;
[0065] S5. Calculate the printing thickness and establish a mathematical model to describe the dynamic behavior of the system, including the state equation and output equation of the system;
[0066] S5.1. Based on the system model, the MPC algorithm predicts the system output in the future in each control cycle. The MPC algorithm determines the control input by solving an optimization problem. The optimization problem includes the objective function, constraints and prediction model.
[0067] S5.2. In each control cycle, the MPC algorithm solves an optimization problem to find the optimal control input sequence. From the optimal control input sequence obtained, the MPC algorithm only implements the control input at the current moment. Then, the system state is updated according to the actual system dynamics.
[0068] S5.3. In the next control cycle, the system state will be updated, and the MPC algorithm will repeat the above process to predict future behavior and optimize the control input. The system model is:
[0069]
[0070] in is the system at time step The state of uk is the control input, A and B are the system matrices. By precisely controlling the thickness, the MPC algorithm can ensure the consistency and quality of the product. The MPC algorithm can enhance the stability of the system and reduce fluctuations in the production process by predicting future behavior and adjusting the control input in advance, making the inkjet thickness more uniform. Uniform thickness helps ensure that the charge is evenly distributed in the light-emitting layer, thereby improving the luminous efficiency and brightness, and improving the color purity and color gamut.
[0071] S6. Printing inkjet printing, place the back of the flexible substrate inside the inkjet printing device, add the ink with the reflective electrode into the ink box, start the inkjet printing device, print the reflective electrode on the back surface of the flexible substrate, the thickness of the reflective electrode layer is 10nm, clean up the remaining ink inside the printing nozzle, turn the flexible substrate over, add the ink with the transparent electrode anode into the oil box, start the inkjet printing device, print the anode pattern on the flexible substrate, and then replace the hole ink, phosphorescent ink, microcavity layer ink, charge transfer layer ink and light-emitting electrode cathode ink for inkjet printing in sequence, the thickness of the hole layer is 5nm, the thickness of the phosphorescent layer is 5nm, the thickness of the microcavity layer is 10nm, the thickness of the charge transfer layer is 5nm, and the thickness of the light-emitting electrode cathode layer and the light-emitting electrode anode layer are both 5nm;
[0072] S7. Processing and packaging: heat-treat the printed film to improve the crystallinity and electrical properties of the material, check the accuracy and uniformity of the printed pattern, test the electrical properties of the OLED device, assemble the OLED device with other components, and complete the final packaging of the OLED device to ensure its stability and reliability during use.
[0073] The simulated annealing algorithm accepts a criterion to define an energy function to evaluate the quality of the solution. At the end of the algorithm, the current solution S is output as the global optimal solution. The simulated annealing algorithm can jump out of the local optimal solution by simulating the physical annealing process, increasing the probability of finding the global optimal solution. The simulated annealing algorithm helps to find the global optimal position configuration instead of just staying at the local optimal solution to optimize performance indicators.
[0074] An electroluminescent device includes a reflective electrode layer responsible for reflecting light emitted from a light-emitting layer to improve the light extraction efficiency of the device;
[0075] Flexible substrates break away from the limitations of traditional rigid materials and achieve lighter, more portable and more durable designs;
[0076] The light-emitting electrode anode layer is made of transparent conductive material and is used to inject positive charges;
[0077] A hole layer, used to improve the electron transfer efficiency between the anode and the light-emitting layer and the phosphor layer;
[0078] The phosphor layer, as the light-emitting layer of the organic light-emitting diode, emits light through the recombination of electrons and holes, which determines the light-emitting color and efficiency of the OLED;
[0079] A microcavity layer, which helps electrons move through the device and regulates light-emitting efficiency;
[0080] A charge transport layer, which helps electrons and holes to be transported from the external electrodes to the phosphor layer to enhance the charge injection efficiency;
[0081] The cathode layer is usually made of metal materials such as aluminum or calcium, which is used to inject electrons.
[0082] The microcavity layer is a distributed Bragg reflector made of zinc oxide. Zinc oxide has a high refractive index and can achieve high reflectivity when alternately stacked with low-refractive-index materials.
[0083] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An inkjet printing process that eliminates film contours, Features: The following steps are involved: S1. Design: Use computer-aided design software and image processing software to design the required patterns and texts, and convert the designed files into a format that can be recognized by the printer, such as PDF or a dedicated printing format; S2. Material preparation, transparent electrode, reflective electrode, flexible substrate and phosphorescent material, preparation of ink containing luminescent material anode ink, charge transport material ink, microcavity layer ink, hole layer ink, phosphorescent ink, reflective electrode layer ink and luminescent electrode cathode ink; S3. Surface treatment of flexible substrates: using plasma to treat the surface roughness of flexible substrates. Plasma treatment can significantly improve the hydrophilicity, adhesion, biocompatibility and other properties of the substrate surface, thereby providing better surface conditions for subsequent printing, coating, bonding and other processes; S3.
1. Pretreatment of the flexible substrate: cleaning the surface of the flexible substrate to remove grease and dust from the surface; S3.
2. Place the cleaned flexible substrate into the vacuum chamber of the plasma treatment equipment, start the vacuum pump, and reduce the pressure in the vacuum chamber to the level required for plasma treatment; inject argon gas, excite the gas by radio frequency, generate plasma, and set the plasma treatment time to 40s; S3.
3. After the plasma treatment is completed, turn off the RF or microwave generator, stop the plasma generation, and slowly restore the atmospheric pressure in the vacuum chamber to avoid damage to the substrate due to pressure difference; S3.
4. After the treatment is completed, the substrate is removed and a subsequent drying or cooling treatment is performed; S3.
5. Use contact angle meter, X-ray photoelectron spectroscopy (XPS) and other equipment to check the hydrophilicity and chemical composition of the substrate surface; S3.
6. Adhesion test An adhesion test was performed using a tape test to evaluate the effect of the plasma treatment; S4. Positioning calibration, printing calibration patterns on ordinary paper to evaluate the printing quality, using simulated annealing algorithm to find the global optimal solution, simulating the physical annealing process, that is, heating and slowly cooling the metal to reduce its internal defects to reach the lowest energy state; S4.
1. Randomly select an initial solution S, set the initial temperature T and cooling rate α, and at the current temperature, randomly select a neighborhood solution, calculate the difference ΔE between the new solution and the current solution, and if ΔE<0, accept the new solution as the current solution. If ΔE>0, accept the new solution with a certain probability, which is usually given by the Metropolis criterion. Repeat the above process until the preset number of iterations is reached and the system reaches a balanced state; S4.
2. Gradually reduce the temperature T = α*T, and repeat the iterative process until the temperature drops sufficiently low or the system reaches a stable state. When the temperature is sufficiently low or the system reaches a stable state, the algorithm terminates; S5. Calculate the printing thickness and establish a mathematical model to describe the dynamic behavior of the system, including the state equation and output equation of the system; S5.
1. Based on the system model, the MPC algorithm predicts the system output in the future in each control cycle. The MPC algorithm determines the control input by solving an optimization problem. The optimization problem includes the objective function, constraints and prediction model. S5.
2. In each control cycle, the MPC algorithm solves an optimization problem to find the optimal control input sequence. From the optimal control input sequence obtained, the MPC algorithm only implements the control input at the current moment. Then, the system state is updated according to the actual system dynamics. S5.
3. In the next control cycle, the system state will be updated, and the MPC algorithm will repeat the above process to predict future behavior and optimize the control input. The system model is: in is the system at time step The state of , uk is the control input, A and B are the system matrices; S6. Printing inkjet printing, place the back of the flexible substrate inside the inkjet printing device, add the ink with the reflective electrode into the ink box, start the inkjet printing device, print the reflective electrode on the back surface of the flexible substrate, the thickness of the reflective electrode layer is 10nm, clean up the remaining ink inside the printing nozzle, turn the flexible substrate over, add the ink with the transparent electrode anode into the oil box, start the inkjet printing device, print the anode pattern on the flexible substrate, and then replace the hole ink, phosphorescent ink, microcavity layer ink, charge transfer layer ink and light-emitting electrode cathode ink for inkjet printing in sequence, the thickness of the hole layer is 5nm, the thickness of the phosphorescent layer is 5nm, the thickness of the microcavity layer is 10nm, the thickness of the charge transfer layer is 5nm, and the thickness of the light-emitting electrode cathode layer and the light-emitting electrode anode layer are both 5nm; S7. Processing and packaging: heat-treat the printed film to improve the crystallinity and electrical properties of the material, check the accuracy and uniformity of the printed pattern, test the electrical properties of the OLED device, assemble the OLED device with other components, and complete the final packaging of the OLED device to ensure its stability and reliability during use.
2. An inkjet printing process capable of eliminating film profile according to claim 1, Features: The simulated annealing algorithm accepts a criterion to define an energy function for evaluating the quality of the solution. When the algorithm ends, the current solution S is output as the global optimal solution.
3. An electroluminescent device, using an inkjet printing process capable of eliminating film profiles as claimed in claims 1 to 3, Features: including a reflective electrode layer responsible for reflecting light emitted from the light-emitting layer to improve the light extraction efficiency of the device; Flexible substrates break away from the limitations of traditional rigid materials and achieve lighter, more portable and more durable designs; The light-emitting electrode anode layer is made of transparent conductive material and is used to inject positive charges; A hole layer, used to improve the electron transfer efficiency between the anode and the light-emitting layer and the phosphor layer; The phosphor layer, as the light-emitting layer of the organic light-emitting diode, emits light through the recombination of electrons and holes, which determines the light-emitting color and efficiency of the OLED; A microcavity layer, which helps electrons move through the device and regulates light-emitting efficiency; A charge transport layer, which helps electrons and holes to be transported from the external electrodes to the phosphor layer to enhance the charge injection efficiency; The light-emitting electrode cathode layer, usually made of metal materials such as aluminum or calcium, is used to inject electrons.
4. An electroluminescent device according to claim 3, Features: The microcavity layer is a distributed Bragg reflector made of zinc oxide.