Method for preparing phosphate from phosphorus-containing wastewater
By carrying out precipitation reaction and metathesis treatment of trisodium phosphate and calcium ions in wastewater, combined with decolorization and oxidation treatment, phosphate is prepared, which solves the problems of high cost and low resource recovery efficiency of struvite crystallization method, and realizes efficient nitrogen and phosphorus resources. recycling and environmental protection.
Patent Information
- Application Number
- CN202411065340.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing struvite crystallization method has high costs in recovering nitrogen and phosphorus resources in wastewater and it is difficult to take into account the recovery of nitrogen resources and phosphorus resources in the form of other nitrogen sources, resulting in low resource recovery efficiency.
By adding trisodium phosphate to the wastewater to react with calcium ion precipitation, and performing a metathesis reaction under heating conditions to generate an ammonium dihydrogen phosphate solution, then adding a decolorizing agent and performing wet oxidation, nanofiltration, cooling crystallization, centrifugation and drying. Prepare phosphate to achieve efficient recovery of nitrogen and phosphorus resources.
It improves the recovery efficiency of nitrogen and phosphorus resources, reduces the cost of resource recovery, and reaches a COD removal rate of 20%-30% in wastewater, achieving waste reuse and environmental protection.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nitrogen and phosphorus wastewater treatment, and in particular to a method for preparing phosphate by utilizing phosphorus-containing wastewater. Background Art
[0002] The one-way flow of phosphorus from land to sea has led to a gradual decrease in the amount of land phosphorus resources, and the excessive discharge of nitrogen and phosphorus in wastewater will lead to eutrophication of water bodies and affect the ecological environment of water bodies. Therefore, how to achieve effective treatment of nitrogen and phosphorus-containing wastewater and sustainable utilization of nitrogen and phosphorus resources in wastewater has become the focus of current research. At present, the main methods used for phosphorus recovery are: chemical precipitation, biological method, adsorption method, and crystallization method.
[0003] Among them, the struvite crystallization precipitation method is a method currently used by wastewater treatment plants to simultaneously process and recover nitrogen and phosphorus resources. This method controls the mixing of magnesium ions, ammonium ions and phosphate ions in water in a ratio of 1:1:1 to form struvite precipitation, thereby achieving nitrogen and phosphorus removal and recovery. The obtained struvite crystals are a high-quality slow-release fertilizer.
[0004] However, due to the low grade of struvite crystals and the reliance on reagents such as ammonium salts and magnesium salts to directly recover nitrogen and phosphorus resources using the struvite crystallization precipitation method, the output and cost of the struvite crystallization method are difficult to match, which is not conducive to the use of the struvite crystallization method in the recovery of nitrogen and phosphorus resources in wastewater, and it is also difficult to take into account the recovery of nitrogen and phosphorus resources in other forms of nitrogen sources.
[0005] Therefore, how to balance the recovery of nitrogen and phosphorus resources in wastewater, improve the recovery efficiency of nitrogen and phosphorus resources and reduce the cost of nitrogen and phosphorus resource recovery is a hot topic for technical personnel in this field. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing phosphate using phosphorus-containing wastewater, so as to solve the problems existing in the prior art, recycle nitrogen and phosphorus resources in the wastewater, and reduce the cost in the process of nitrogen and phosphorus resource recovery.
[0007] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0008] 1. A method for preparing phosphate using phosphorus-containing wastewater, comprising the following specific steps:
[0009] S1. Add trisodium phosphate to the wastewater, so that the trisodium phosphate reacts with calcium ions in the water for precipitation, and the S / N ratio of the wastewater is 1.5-2.1;
[0010] S2, heating the wastewater to 25±2°C, with a hydraulic retention time of 0.5-15h, gradually adding ammonium salt until the pH value reaches 6.5-7.5, and performing double decomposition reaction to generate diammonium phosphate solution, wherein the conversion rate of waste phosphoric acid reaches more than 98% in the reaction;
[0011] S3, adding a decolorizing agent accounting for 3%-5% of the total weight of the phosphorus-containing wastewater to the solution after the reaction for decolorization;
[0012] S4, after the decolorization is completed, the diammonium phosphate solution is subjected to a nanofiltration treatment after wet oxidation;
[0013] S5. Cooling, crystallizing, centrifuging and drying the filtered diammonium phosphate solution to obtain a finished product.
[0014] As an improvement, the concentration of sulfide in the wastewater is 82.74-564.67 mg S / L; the concentration of nitrite is 18.36-145.10 mg N / L; and the concentration of phosphate is 20.0-227.9 mg P / L.
[0015] As an improvement, the S / N ratio in the wastewater is 1.5-2.1.
[0016] As an improvement, the magnesium source in step S4 is at least one of magnesium chloride, magnesium sulfate and magnesium oxide.
[0017] As an improvement, the decolorizing agent in step S2 is activated carbon, and the decolorizing agent is a mixture of bentonite: hydrogen peroxide: potassium permanganate in a mass ratio of 3:2:1.
[0018] As an improvement, the cooling crystallization process in step S4 is as follows: the filtered diammonium phosphate solution is placed in a reaction pot, and the reaction pot is heated by a coil, stirred, sucked, and bubbled, and cooled and crystallized after the temperature reaches 100-110°C and the pomel degree is 35.
[0019] As an improvement, the centrifugation and drying process in step S4 is as follows: the fluid semi-finished product after crystallization is sent to a centrifuge for centrifugation to squeeze out the water, and when the water content is about 3% to 5%, the material is discharged; the centrifuged material is sent to a dryer for drying or a drying room for drying until the water content of the product is 0.2% to 0.3%, which is the finished product.
[0020] The advantages of the present invention compared with the prior art are:
[0021] 1. Add trisodium phosphate during wastewater treatment. Trisodium phosphate reacts with calcium ions in the water to precipitate. While forming the precipitate, COD in the water will be removed, with a removal rate of 20% to 30%;
[0022] 2. Effectively converting phosphorus-containing wastewater into useful diammonium phosphate fertilizer not only completes the task of waste recycling, but also is beneficial to environmental protection. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0024] The present application fully explains the problems of the prior art in the technical background, and there are no superordinate or general problems. The problems to be solved by the present application are described in detail in the following invention content and specific implementation methods, the technical problems to be solved by the technical scheme are clarified, and it is determined that the technical scheme of the present application has beneficial effects relative to the objective prior art.
[0025] An embodiment provided by the present invention:
[0026] A method for preparing phosphate using phosphorus-containing wastewater, the specific steps are as follows:
[0027] S1. Add trisodium phosphate to the wastewater, so that the trisodium phosphate reacts with calcium ions in the water for precipitation, and the S / N ratio of the wastewater is 1.5;
[0028] The concentration of sulfide in the wastewater is 82.74-564.67 mg S / L; the concentration of nitrite is 18.36-145.10 mg N / L; and the concentration of phosphate is 20.0-227.9 mg P / L.
[0029] S2, heating the wastewater to 27°C, with a hydraulic retention time of 1.5h, gradually adding ammonium salt until the pH value reaches 6.5-7.5, and performing double decomposition reaction to generate diammonium phosphate solution, in which the conversion rate of waste phosphoric acid reaches more than 98%;
[0030] The decolorizing agent in step S2 is activated carbon, and the decolorizing agent is a mixture of bentonite: hydrogen peroxide: potassium permanganate in a mass ratio of 3:2:1.
[0031] S3, adding a decolorizing agent accounting for 8% of the total weight of the phosphorus-containing wastewater to the solution after the reaction for decolorization;
[0032] S4, after the decolorization is completed, the diammonium phosphate solution is subjected to a nanofiltration treatment after wet oxidation;
[0033] The magnesium source in step S4 is at least one of magnesium chloride, magnesium sulfate and magnesium oxide;
[0034] The cooling crystallization process in step S4 is as follows: the filtered diammonium phosphate solution is placed in a reaction pot, and the reaction pot is heated by a coil, stirred, sucked, and bubbled, and cooled and crystallized after the temperature reaches 100°C and the pomel degree is 35.
[0035] S5. Cooling, crystallizing, centrifuging and drying the filtered diammonium phosphate solution to obtain a finished product.
[0036] Example 2
[0037] A method for preparing phosphate using phosphorus-containing wastewater, the specific steps are as follows:
[0038] 1. Add trisodium phosphate to the wastewater, and the trisodium phosphate reacts with calcium ions in the water for precipitation, and the S / N ratio of the wastewater is 2.1;
[0039] 2. Heat the wastewater to 23°C, with a hydraulic retention time of 0.5h, and gradually add ammonium salt until the pH value reaches 6.5-7.5, and then perform double decomposition reaction to generate diammonium phosphate solution;
[0040] 3. Add a decolorizing agent accounting for 10% of the total weight of the phosphorus-containing wastewater to the solution after the reaction for decolorization;
[0041] 4. After decolorization is completed, the diammonium phosphate solution is subjected to wet oxidation and then nanofiltration treatment;
[0042] The cooling crystallization process is as follows: the filtered diammonium phosphate solution is placed in a reaction pot, which is heated by a coil, stirred, sucked, and bubbled. After the temperature reaches 130°C and the pH value is 35, it is cooled and crystallized. 5.
[0044] 6. Cool, crystallize, centrifuge and dry the filtered diammonium phosphate solution to obtain the finished product.
[0045] Preferably, the centrifugation and drying process is as follows: the semi-finished product after crystallization is transported to a centrifuge for centrifugation to squeeze out water, and when the water content is about 3% to 5%, the product is discharged; the centrifuged product is transported to a dryer for drying or a drying room for drying until the product has a water content of 0.1% to 0.2%, which is the finished product.
[0046] Those skilled in the art will readily appreciate other embodiments of the present application after considering the specification and practicing the application disclosed herein. The present application is intended to cover any variations, uses or adaptations of the present application, which follow the general principles of the present application and include common knowledge or customary techniques in the art that are not disclosed in the present application. The specification and examples are intended to be exemplary only, and the true scope of the present application is indicated by the claims.
[0047] It should be understood that the present application is not limited to the above description, and various modifications and changes can be made without departing from its scope. The above-described embodiments of the present application do not constitute a limitation on the scope of protection of the present application.
Claims
1. A method for preparing phosphate using phosphorus-containing wastewater, characterized in that: The specific steps are as follows: S1. Add trisodium phosphate to the wastewater, so that the trisodium phosphate reacts with calcium ions in the water for precipitation, and the S / N ratio of the wastewater is 1.5-2.1; S2, heating the wastewater to 25±2°C, with a hydraulic retention time of 0.5-15h, gradually adding ammonium salt until the pH value reaches 6.5-7.5, and performing double decomposition reaction to generate diammonium phosphate solution; S3, adding a decolorizing agent accounting for 8%-10% of the total weight of the phosphorus-containing wastewater to the solution after the reaction for decolorization; S4, after the decolorization is completed, the diammonium phosphate solution is subjected to a nanofiltration treatment after wet oxidation; S5. Cooling, crystallizing, centrifuging and drying the filtered diammonium phosphate solution to obtain a finished product.
2. The method for preparing phosphate using phosphorus-containing wastewater according to claim 1, characterized in that: The concentration of sulfide in the wastewater is 82.74-564.67 mg S / L; the concentration of nitrite is 18.36-145.10 mg N / L; and the concentration of phosphate is 20.0-227.9 mg P / L.
3. The method for preparing phosphate using phosphorus-containing wastewater according to claim 1, characterized in that: The conversion rate of waste phosphoric acid in the reaction in step S2 reaches more than 98%.
4. The method for preparing phosphate using phosphorus-containing wastewater according to claim 1, characterized in that: The magnesium source in step S4 is at least one of magnesium chloride, magnesium sulfate and magnesium oxide.
5. The method for preparing phosphate using phosphorus-containing wastewater according to claim 1, characterized in that: The decolorizing agent in step S2 is activated carbon, and the decolorizing agent is a mixture of bentonite: hydrogen peroxide: potassium permanganate in a mass ratio of 3:2:
1.
6. The method for preparing phosphate using phosphorus-containing wastewater according to claim 1, characterized in that: The cooling crystallization process in step S4 is as follows: the filtered diammonium phosphate solution is placed in a reaction pot, and the reaction pot is heated by a coil, stirred, sucked, and bubbled. After the temperature reaches 120-130°C and the pH value is 35, cooling and crystallization are performed.
7. A method for preparing phosphate using phosphorus-containing wastewater according to claim 6, characterized in that: The centrifugation and drying process in step S4 is as follows: the semi-finished product after crystallization is sent to a centrifuge for centrifugation to squeeze out the water, and when the water content is about 3% to 5%, the product is discharged; the centrifuged product is sent to a dryer for drying or a drying room for drying until the product has a water content of 0.1% to 0.2%, which is the finished product.