Preparation method of non-stoichiometric iron phosphate material and sodium ion battery positive electrode material

Through the preparation method of non-stoichiometric iron phosphate materials, using buffer solutions and oxidative co-precipitation technology to accurately control the iron-phosphorus ratio, the problem of difficult control of the iron-phosphorus ratio in the preparation of sodium-ion battery cathode materials has been solved, and efficient and low-cost sodium production has been achieved. Preparation of cathode materials for ion batteries improves electrochemical performance.

CN118771331AActive Publication Date: 2024-10-15SHENZHEN JANAENERGY TECH CO LTD

Patent Information

Application Number
CN202411000070.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-15
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

In the existing preparation process of sodium-ion battery cathode materials, the iron-phosphorus ratio is difficult to accurately control, resulting in high material costs and complex processes, which limits the low-cost popularization and application of sodium-ion batteries.

Method used

Using a non-stoichiometric preparation method of iron phosphate materials, the pH value is adjusted by adding a buffer solution to the phosphorus source solution, combined with oxidative co-precipitation and high-temperature roasting steps to control the iron-to-hydrogen ratio and the concentration of phosphate, accurately regulate the iron-phosphorus ratio, and reduce Material costs, improved product yield and electrochemical performance.

Benefits of technology

The preparation of iron phosphate materials with high yield, low cost and excellent electrochemical properties is achieved, which is suitable for sodium-ion battery cathode materials and improves the specific capacity and rate performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771331A_ABST
    Figure CN118771331A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a non-stoichiometric ferric phosphate material and a sodium ion battery positive electrode material, the preparation method comprises the following steps: S1, preparation of a precursor solution: adding a buffer solution into a phosphoric acid solution to adjust the pH range of a reaction system to 0.5-3, adding ferrite, and uniformly mixing to obtain the precursor solution; and S2, solid precipitation and separation: adding an oxidizing agent into the precursor solution under a temperature control condition, carrying out temperature control aging after an oxidation reaction is completed, and carrying out solid-liquid separation to obtain the non-stoichiometric ferric phosphate material FexHy (POm) (3x + y) / (2m-5). ZH2O solid. The method has the characteristics of high product yield, low cost, high compaction density and excellent electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a method for preparing a non-stoichiometric iron phosphate material and a positive electrode material for a sodium ion battery. Background Art

[0002] In sodium-ion batteries, especially sodium iron phosphate pyrophosphate system sodium-ion batteries, due to its abundant raw material reserves, low price, high safety and excellent electrochemical performance, it will gradually become an alternative to lithium iron phosphate batteries. For this type of sodium-ion battery, its key positive electrode material is sodium iron phosphate pyrophosphate (Na4Fe3(PO4)2P2O7, which has an iron-phosphorus ratio of 0.75.

[0003] However, in the preparation process of Na4Fe3(PO4)2P2O7, iron phosphate (FePO4) with an iron-phosphorus ratio of 1 is mainly used as the raw material. Therefore, in order to balance the element ratio, more phosphorus sources, such as dihydrogen phosphates, need to be introduced in the preparation process. Moreover, based on the need to accurately control the iron-phosphorus ratio, higher requirements are required for the purity of the phosphorus source material, which increases the material cost of the positive electrode material and is not conducive to reducing the overall cost of sodium-ion batteries. Analyzing from the preparation process of iron phosphate, the existing preparation method of iron phosphate is mainly a chemical method, which uses phosphoric acid and an iron source as raw materials, and prepares iron phosphate (FePO4) based on the co-precipitation reaction of phosphate and trivalent iron, and generates waste liquid that needs to be subsequently treated.

[0004] Therefore, the difference in the iron-phosphorus ratio seriously limits its widespread application in the synthesis of sodium iron pyrophosphate. In addition, there are additional waste liquid treatment costs and high process costs, which is not conducive to the low-cost popularization and application of sodium-ion batteries.

[0005] In response to this, Chinese invention patent application CN116409766A discloses a method for regulating the iron-phosphorus ratio within the range of 0.8-1.7. The iron-phosphorus ratio of the synthesized iron phosphate material is too high to directly meet the low iron-phosphorus ratio requirement for the production of sodium iron pyrophosphate (Na4Fe3(PO4)2P2O7, iron-phosphorus ratio of 0.75).

[0006] In addition, when iron phosphate is used as a raw material to produce electrode materials, such as lithium iron phosphate, sodium iron pyrophosphate, sodium iron phosphate, etc., the particle size and morphology of the iron phosphate precursor particles have a significant impact on the synthesis of the final electrode material product and its electrochemical properties. A smaller particle size usually means a shorter ion insertion and extraction path, which is beneficial to improving the specific capacity and rate performance of the electrode material; a specific morphology, such as a spherical shape, can increase the compaction density and optimize the processing performance of the material. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing a non-stoichiometric iron phosphate material and a positive electrode material for a sodium ion battery, which have the characteristics of high product yield, low cost, high compaction density and excellent electrochemical performance.

[0008] The present invention can be implemented by the following technical solutions: The present invention discloses a method for preparing a non-stoichiometric iron phosphate material, comprising the following steps: S1. Preparation of precursor solution: adding a buffer solution to the phosphorus source solution to adjust the pH range of the reaction system to 1-3, adding ferrous salt, and mixing to obtain a precursor solution; S2. Solid precipitation and separation: Under temperature control, an oxidant is added to the precursor solution of step S1, and after the oxidation reaction is completed, the temperature is controlled and aged, and the solid-liquid separation is performed to obtain non-stoichiometric acid iron phosphate Fe x H y (PO m ) (3x+y) / (2m-5) zH2O solid; S3, high temperature roasting: the non-stoichiometric acid iron phosphate Fe in step S2 is x H y (PO m ) (3x+y) / (2m-5) · The zH2O solid is calcined at high temperature to remove all or part of the bound water to obtain a non-stoichiometric iron phosphate material In non-stoichiometric acid ferric phosphate Fe x H y (PO m ) (3x+y) / (2m-5) In zH2O and non-stoichiometric iron phosphate materials with all or part of the bound water removed, the iron-hydrogen ratio x / y ranges from 1 / 3 to 17 / 3, x ranges from 0.5 to 0.95, y ranges from 0.15 to 1.5, z ranges from 1 to 4, and m ranges from 3.5 to 4.

[0009] Further, since phosphoric acid is a medium-strong acid, it has a greater impact on the pH of the solution system. The buffering capacity of the buffer solution is directly related to its total concentration. In the same buffer system, when the buffer ratio remains unchanged, the greater the total concentration of the buffer solution, the more the number of its anti-acid components and anti-alkali components. This means that after adding the same amount of acid or alkali, the smaller the change in the buffer ratio, the greater the buffer capacity, thereby showing a stronger buffering capacity. On the contrary, if the total concentration is small, the buffer capacity is also small, and the buffering capacity is weakened therewith. Combined with the height of the concentration of the phosphoric acid and the solubility of the effective component of the buffer solution, the higher the concentration of phosphoric acid in the solution, the more stable the pH, the greater the concentration of the required buffer solution, but the buffer solution concentration is too high, the viscosity of the solution increases, which is unfavorable for the reaction process and subsequent cleaning process, and the concentration of ferrous ions is adjusted according to the concentration of the phosphate radicals put in, to ensure the iron-phosphorus ratio of the product, if the concentration of ferrous ions is too high, the product iron-phosphorus ratio is higher. Therefore, the final concentration range of phosphoric acid solution is 0.1-12wt%, the concentration range of buffer solution is 0.01-1 mol / L, and the concentration of ferrous ions in ferrous salt is 0.1-8wt%. Through the above control, the pH of the reaction solution is kept at a low level, and the control of pH and iron-phosphorus ratio of feed (0.2-0.85) can effectively regulate the non-stoichiometric acid ferric phosphate Fe x H y (PO m ) (3x+y) / (2m-5) ·The hydrogen content in zH2O, the iron-hydrogen ratio x / y is regulated to be 1 / 3-17 / 3, based on the charge conservation, and finally effectively ensures the preparation of non-stoichiometric iron phosphate materials. At the same time, the lower pH is not conducive to the precipitation of other phosphates (such as titanium phosphate, magnesium phosphate, aluminum phosphate), so the more cost-effective recycled phosphoric acid can be used to obtain high-purity non-stoichiometric acid iron phosphate.

[0010] Further, in step S2, an oxidant is added to the precursor solution, and the reaction of rapidly nucleating and forming an iron phosphate complex through an oxidation coprecipitation reaction is an exothermic reaction. The higher the reaction temperature, the faster the reaction rate, which is conducive to the rapid generation of a solid with a concentrated particle size distribution and uniform particle distribution. However, if the reaction temperature is too high, the reaction rate will be too fast, the heat release will be serious, and there will be safety hazards, so the oxidation reaction temperature is 30-80°C. There are two main reactions involved during aging, one is the conversion and dissolution of the precipitate, and the other is the aggregation and growth of the precipitated particles. The higher the temperature, the higher the degree of dissociation of polyphosphate, which is easy to cause the pH of the solution to decrease, and then lead to a decrease in the iron-phosphorus ratio of the product, and when the aging temperature is high, the particles aggregate quickly and are easy to form large particles. When the aging temperature is low, the particles slowly aggregate and grow closely, and finally a spherical material with a high compacted density can be obtained. The reaction temperature is 30-80°C; the aging conditions are: the aging temperature ranges from 10-80°C and the aging time is 2-10h.

[0011] Furthermore, in step S3, the high temperature calcination conditions are: the calcination temperature is 100-700°C, and the calcination time ranges from 1 to 10 hours. The operation of this step is to remove the bound water of the prepared iron phosphate complex. The low temperature and short calcination time cannot completely remove the bound water, but can achieve the purpose of partially removing the crystal water. However, the high temperature and long calcination time will cause the iron phosphate complex to agglomerate and pyrophosphorylate. Specifically, the Fe x H y (PO m ) (3x+y) / (2m-5) ·zH2O solid is calcined at a high temperature of 100-800℃, and the bound water is gradually removed as the calcination temperature increases. By controlling the calcination temperature, non-stoichiometric acid iron phosphate materials with different water contents can be obtained. The range of x / y in the non-stoichiometric acid iron phosphate material is 1 / 3-17 / 3. The phosphate complex prepared by the current co-precipitation method often carries 1-4 bound waters. In order to facilitate the expression of the general formula, 3x+y=3 is specified, that is, the coefficient of the phosphate group is 1. Based on the test of the iron-hydrogen ratio of the product, the range of x is 0.5-0.95, the range of y is 0.15-1.5, and the range of z is 1-4. Pyrophosphorylation of phosphate may occur during the reaction heating process, the aging heating process, and the calcination process. If there is pyrophosphate in the raw material, it will be in the Fe x H y (PO m ) (3x+y) / (2m-5) When pyrophosphate is introduced into zH2O, the range of m is 3.5-4. The iron-phosphorus ratio of the non-stoichiometric acid ferric phosphate and the non-stoichiometric ferric phosphate material is 0.5-0.95.

[0012] Furthermore, the buffer solution is one or more of disodium hydrogen phosphate-citric acid buffer, phthalic acid-hydrochloric acid buffer, glycine-sulfuric acid buffer, phthalic acid-sulfuric acid buffer, phosphoric acid-sodium dihydrogen phosphate, and oxalic acid-sodium hydrogen oxalate.

[0013] Furthermore, the buffer solution is one or more of disodium hydrogen phosphate-citric acid buffer, phthalic acid-hydrochloric acid buffer, glycine-sulfuric acid buffer, phthalic acid-sulfuric acid buffer, phosphoric acid-sodium dihydrogen phosphate, and oxalic acid-sodium hydrogen oxalate.

[0014] Furthermore, the ferrous salt is one or more of ferrous sulfate, ferrous sulfate heptahydrate, ferrous chloride, ferrous nitrate, and sodium ferrous sulfate.

[0015] Furthermore, the phosphorus source is one or more of phosphates and pyrophosphates such as crude phosphoric acid, refined phosphoric acid, diammonium phosphate, sodium dihydrogen phosphate, and sodium pyrophosphate.

[0016] Further, the oxidant is one or more of oxidants such as sodium persulfate, hydrogen peroxide, oxygen, ozone, air, sodium hypochlorite, and peracetic acid, and the concentration of hydrogen peroxide is 1-30wt%. Hydrogen peroxide is an oxidant that is easy to make explosives. When used as an oxidant in the present invention, if the concentration is too low, it will lead to excessive dilution of the solution, and the reaction speed is slow, which is not conducive to the rapid generation of solids with concentrated particle size distribution and uniform particle distribution. If the concentration is too high, it will cause the reaction to be too violent, which has potential safety hazards.

[0017] Another aspect of the present invention is to protect a sodium ion battery positive electrode material, which is prepared by mixing the non-stoichiometric acid ferric phosphate material prepared above as a precursor with a sodium source and sintering at high temperature.

[0018] Furthermore, the high temperature sintering conditions are: high temperature calcination at 600-700°C for 8-10h, and the protective atmosphere is argon and / or nitrogen. At high temperature, the phosphorus source, iron source and sodium source tend to form carbon-coated sodium iron phosphate pyrophosphate crystals. Too low a calcination temperature and too short a calcination time will lead to insufficient crystal conversion and impure crystal phases, while too high a calcination temperature and too long a calcination time will lead to crystal agglomeration and reduce its electrochemical performance.

[0019] Furthermore, the sodium salt is one or more of sodium carbonate, sodium dihydrogen phosphate, and sodium nitrate.

[0020] The present invention provides a method for preparing a non-stoichiometric iron phosphate material and a positive electrode material for a sodium ion battery, which have the following beneficial effects: First, the product yield is high. The present invention introduces a buffer solution into the reaction system to regulate the pH value of the reaction system to be stable in the range of 1-3, which can effectively regulate the iron-hydrogen ratio x / y of the non-stoichiometric acid ferric phosphate material to be in the range of 1 / 3-17 / 3. The method is used to regulate the iron-hydrogen ratio with the characteristics of accuracy, stability and reproducibility, and also obtains a high yield. Fe x H y (PO m ) (3x+y) / (2m-5) After further roasting and dehydration of zH2O, a partially or completely dehydrated non-stoichiometric iron phosphate material can be obtained; Second, the cost is low. In the present invention, based on the adjustment of the entire system, there is no excessively high requirement for the purity of the phosphorus source. The phosphorus source can use low-cost recycled phosphoric acid. Even if the recycled phosphoric acid contains more other impurities, the present invention can effectively avoid introducing other impurities in the recycled acid into the precipitated product by regulating the pH value, thereby improving the purity of the product and expanding the selectable range of low-cost phosphorus sources. Third, the compaction density is high. The oxidation coprecipitation reaction of the present invention selects a higher temperature range, which is conducive to the high temperature in the initial stage of the reaction, and quickly generates Fe with concentrated particle size distribution and uniform particle distribution. x Hy (PO m ) (3x+y) / (2m-5) ·zH2O; The aging temperature is selected in a relatively low temperature range to promote the slow aggregation and close growth of particles, and finally a spherical material with high compaction density can be obtained; Fourth, the electrochemical performance is excellent. The non-stoichiometric iron phosphate material prepared by the method of the present invention has small size and good dispersibility. According to the genetic characteristics between the precursor and the product, that is, the morphology structure of the product can inherit the morphology structure of the precursor. When the non-stoichiometric iron phosphate material precursor is used as the synthetic raw material of sodium iron pyrophosphate, a morphology structure similar to that of the precursor can be obtained. The sodium iron pyrophosphate positive electrode material prepared from the precursor has uniform phase distribution, high rate, high specific capacity, high compaction density and good processability. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Attached Figure 1 This is the charge and discharge curve of the positive electrode material of Example 1. DETAILED DESCRIPTION

[0022] In order to enable those skilled in the art to better understand the technical solution of the present invention, the product of the present invention is further described in detail below in conjunction with embodiments.

[0023] The present invention discloses a method for preparing a non-stoichiometric iron phosphate material, comprising the following steps: S1. Preparation of precursor solution: adding a buffer solution to a phosphoric acid solution to adjust the pH of the reaction system to 1-3, adding ferrous salt, and mixing to obtain a precursor solution; S2. Solid precipitation and separation: Under temperature control, an oxidant is added to the precursor solution in step S1, and after the oxidation reaction is completed, the temperature is controlled and aged, and the solid-liquid separation is performed to obtain Fe x H y (PO m ) (3x+y) / (2m-5) zH2O solid; S3, high temperature calcination: the Fe x H y (PO m ) (3x+y) / (2m-5) · Non-stoichiometric iron phosphate material obtained by calcining zH2O solid at high temperature to remove all or part of the bound water; In Fe x H y (PO m ) (3x+y) / (2m-5) · A non-stoichiometric iron phosphate material obtained by removing all or part of the crystal water from zH2O, wherein the iron-hydrogen ratio x / y is in the range of 1 / 3-17 / 3, x is in the range of 0.5-0.95, y is in the range of 0.15-1.5, z is in the range of 1-4, and m is in the range of 3.5-4.

[0024] Furthermore, in step S1, the concentration range of the phosphorus source solution is 0.1-12wt%, the concentration range of the buffer solution is 0.01-1 mol / L, the ferrous ion concentration of the ferrous salt is 0.1-8wt%, and the iron-phosphorus ratio of the feed is 0.2-0.85.

[0025] Furthermore, in step S2, the reaction temperature is 30-80°C; the aging conditions are: the aging temperature ranges from 10-80°C, and the aging time is 2-10h.

[0026] Furthermore, in step S3, the high temperature calcination conditions are: the calcination temperature is 100-700° C., and the calcination time ranges from 1 to 10 hours.

[0027] Furthermore, the buffer solution is one or more of disodium hydrogen phosphate-citric acid buffer, phthalic acid-hydrochloric acid buffer, glycine-sulfuric acid buffer, phthalic acid-sulfuric acid buffer, phosphoric acid-sodium dihydrogen phosphate, and oxalic acid-sodium hydrogen oxalate.

[0028] Furthermore, the ferrous salt is one or more of ferrous sulfate, ferrous sulfate heptahydrate, ferrous chloride, ferrous nitrate, and sodium ferrous sulfate.

[0029] Furthermore, the phosphorus source is one or more of phosphates and pyrophosphates such as crude phosphoric acid, refined phosphoric acid, diammonium phosphate, sodium dihydrogen phosphate, and sodium pyrophosphate.

[0030] Furthermore, the oxidant is one or more of oxidants selected from the group consisting of sodium persulfate, hydrogen peroxide, oxygen, ozone, air, sodium hypochlorite, and peracetic acid, and the concentration of hydrogen peroxide is 1-30 wt %.

[0031] Another aspect of the present invention is to protect a sodium ion battery positive electrode material, using the non-stoichiometric acid iron phosphate Fe prepared above x H y (PO m ) (3x+y) / (2m-5) The zH2O material or non-stoichiometric iron phosphate material is prepared by mixing a precursor with a sodium source and sintering at high temperature.

[0032] Furthermore, the high temperature sintering conditions are: high temperature sintering at 600-700° C. for 8-10 hours, and the protective atmosphere is argon and / or nitrogen.

[0033] Furthermore, the sodium salt is one or more of sodium carbonate, sodium dihydrogen phosphate, and sodium nitrate.

[0034] Example 1 This embodiment relates to a non-stoichiometric acid ferric phosphate material and a sodium ion battery positive electrode material prepared using the same as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: dilute crude phosphoric acid to obtain dilute phosphoric acid (1.6 wt%), add 0.5 mol / L phthalic acid-hydrochloric acid buffer to the dilute phosphoric acid solution as a buffer solution system, adjust the pH value of the reaction system to be stable at about 2, add ferrous salt (2.2 wt%) according to an iron-phosphorus ratio of 0.75:1 and mix well to obtain a uniform solution; S2. Precipitation and separation of solids: at 70°C, an oxidant is added to the homogeneous solution of step S1 above to rapidly nucleate the solution through an oxidation coprecipitation reaction; after the oxidation reaction is completed, the reaction solution is aged at 40°C for 4h, and the solid obtained by solid-liquid separation is dried in an oven at 100 degrees overnight.

[0035] S3, high temperature calcination: calcine the solid obtained in step S2 at 300° C. for 10 h to remove bound water and obtain a non-stoichiometric acid ferric phosphate material; S4, high temperature sintering: the solid of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron pyrophosphate positive electrode material, whose charge and discharge curve is as follows: Figure 1 As shown, the charge capacity is as high as 108.2 mAh g -1 It can be seen that the use of non-stoichiometric acid ferric phosphate materials as iron-phosphorus sources can achieve the preparation of high-performance sodium iron pyrophosphate positive electrode materials.

[0036] Example 2 This embodiment relates to a non-stoichiometric acid ferric phosphate material and a sodium ion battery positive electrode material prepared using the same as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: dilute crude phosphoric acid to obtain dilute phosphoric acid (1.6 wt%), add 0.5 mol / L phthalic acid-hydrochloric acid buffer to the dilute phosphoric acid solution as a buffer solution system, adjust the pH value of the reaction system to be stable at about 2, add ferrous salt (2.2 wt%) according to an iron-phosphorus ratio of 0.75:1 and mix well to obtain a uniform solution; S2, precipitation and separation of solids: at 50°C, an oxidant is added to the homogeneous solution of step S1 above, and nucleation is rapidly formed through oxidation coprecipitation reaction; after the oxidation reaction is completed, the reaction solution is aged at 40°C for 4h, and the solid obtained by solid-liquid separation is dried in an oven at 100 degrees overnight; S3, high temperature calcination: calcine the solid obtained in step S2 at 300° C. for 8 h to remove bound water and obtain a non-stoichiometric acid ferric phosphate material; S4, high temperature sintering: the solid of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode material, the electrochemical properties of which are shown in Table 1. It can be seen that the use of non-stoichiometric acid iron phosphate material as an iron-phosphorus source can achieve the preparation of a high-performance sodium iron phosphate pyrophosphate positive electrode material.

[0037] Example 3 This embodiment relates to a non-stoichiometric acid ferric phosphate material and a sodium ion battery positive electrode material prepared using the same as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: dilute crude phosphoric acid to obtain dilute phosphoric acid (1.6 wt%), add 0.5 mol / L phthalic acid-hydrochloric acid buffer to the dilute phosphoric acid solution as a buffer solution system, adjust the pH value of the reaction system to be stable at about 2, add ferrous salt (2.2 wt%) according to an iron-phosphorus ratio of 0.75:1 and mix well to obtain a uniform solution; S2, precipitation and separation of solids: at 30°C, an oxidant is added to the homogeneous solution of step S1 above, and nucleation is rapidly formed through oxidation coprecipitation reaction; after the oxidation reaction is completed, aging is carried out at 40°C for 4 hours, and the solid obtained by solid-liquid separation is dried in an oven at 100 degrees overnight; S3, high temperature calcination: calcine the solid obtained in step S2 at 300° C. for 6 h to remove bound water and obtain a non-stoichiometric acid ferric phosphate material; S4, high temperature sintering: the solid of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode material, the electrochemical properties of which are shown in Table 1. It can be seen that the use of non-stoichiometric acid iron phosphate material as an iron-phosphorus source can achieve the preparation of a high-performance sodium iron phosphate pyrophosphate positive electrode material.

[0038] Example 4 This embodiment relates to a non-stoichiometric acid ferric phosphate material and a sodium ion battery positive electrode material prepared using the same as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: dilute crude phosphoric acid to obtain dilute phosphoric acid (0.8 wt%), add 0.5 mol / L phthalic acid-hydrochloric acid buffer to the dilute phosphoric acid solution as a buffer solution system, adjust the pH value of the reaction system to be stable at about 2, add ferrous salt (1.1 wt%) according to an iron-phosphorus ratio of 0.75:1 and mix well to obtain a uniform solution; S2, precipitation and separation of solids: at 70°C, an oxidant is added to the homogeneous solution of step S1 above, and nucleation is rapidly formed through oxidation coprecipitation reaction; after the oxidation reaction is completed, the reaction solution is aged at 40°C for 4h, and the solid obtained by solid-liquid separation is dried in an oven at 100 degrees overnight; S3, high temperature calcination: calcine the solid obtained in step S2 at 300° C. for 4 h to remove bound water and obtain a non-stoichiometric acid ferric phosphate material; S4, high temperature sintering: the solid of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode material, the electrochemical properties of which are shown in Table 1. It can be seen that the use of non-stoichiometric acid iron phosphate material as an iron-phosphorus source can achieve the preparation of a high-performance sodium iron phosphate pyrophosphate positive electrode material.

[0039] Example 5 This embodiment relates to a non-stoichiometric acid ferric phosphate material and a sodium ion battery positive electrode material prepared using the same as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: dilute crude phosphoric acid to obtain dilute phosphoric acid (1.2 wt%), add 0.5 mol / L phthalic acid-hydrochloric acid buffer to the dilute phosphoric acid solution as a buffer solution system, adjust the pH value of the reaction system to be stable at about 2, add ferrous salt (1.65 wt%) according to an iron-phosphorus ratio of 0.75:1 and mix well to obtain a uniform solution; S2, precipitation and separation of solids: at 70°C, an oxidant is added to the homogeneous solution of step S1 above, and nucleation is rapidly formed through oxidation coprecipitation reaction; after the oxidation reaction is completed, the reaction solution is aged at 40°C for 4h, and the solid obtained by solid-liquid separation is dried in an oven at 100 degrees overnight; S3, high temperature calcination: calcine the solid obtained in step S2 at 300° C. for 10 h to remove bound water and obtain a non-stoichiometric acid ferric phosphate material; S4, high temperature sintering: the solid of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode material, the electrochemical properties of which are shown in Table 1. It can be seen that the use of non-stoichiometric acid iron phosphate material as an iron-phosphorus source can achieve the preparation of a high-performance sodium iron phosphate pyrophosphate positive electrode material.

[0040] Example 6 This embodiment relates to a non-stoichiometric acid ferric phosphate material and a sodium ion battery positive electrode material prepared using the same as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: dilute crude phosphoric acid to obtain dilute phosphoric acid (3.2 wt%), add 0.5 mol / L phthalic acid-hydrochloric acid buffer to the dilute phosphoric acid solution as a buffer solution system, adjust the pH value of the reaction system to be stable in the range of 2, add ferrous salt (4.4 wt%) according to an iron-phosphorus ratio of 0.75:1, mix well and obtain a uniform solution; S2, precipitation and separation of solids: at 70°C, an oxidant is added to the homogeneous solution of step S1 above, and nucleation is rapidly formed through oxidation coprecipitation reaction; after the oxidation reaction is completed, the reaction solution is aged at 40°C for 4h, and the solid obtained by solid-liquid separation is dried in an oven at 100 degrees overnight; S3, high temperature calcination: calcine the solid obtained in step S2 at 100° C. for 10 h to remove bound water and obtain a non-stoichiometric acid ferric phosphate material; S4, high temperature sintering: the solid of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode material, the electrochemical properties of which are shown in Table 1. It can be seen that the use of non-stoichiometric acid iron phosphate material as an iron-phosphorus source can achieve the preparation of a high-performance sodium iron phosphate pyrophosphate positive electrode material.

[0041] Example 7 This embodiment relates to a non-stoichiometric acid ferric phosphate material and a sodium ion battery positive electrode material prepared using the same as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: dilute crude phosphoric acid to obtain dilute phosphoric acid (1.6 wt%), add 0.5 mol / L phthalic acid-hydrochloric acid buffer to the dilute phosphoric acid solution as a buffer solution system, adjust the pH value of the reaction system to be stable at about 2, add ferrous salt (2.2 wt%) according to an iron-phosphorus ratio of 0.75:1 and mix well to obtain a uniform solution; S2. Precipitation and separation of solids: at 70°C, an oxidant is added to the homogeneous solution of step S1 above to rapidly nucleate the solution through an oxidation coprecipitation reaction; after the oxidation reaction is completed, the reaction solution is aged at 40°C for 4h, and the solid obtained by solid-liquid separation is dried in an oven at 100 degrees overnight.

[0042] S3, high temperature calcination: calcine the solid obtained in step S2 at 400° C. for 10 h to remove bound water and obtain a non-stoichiometric acid ferric phosphate material; S4, high temperature sintering: the solid of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode material, the electrochemical properties of which are shown in Table 1. It can be seen that the use of non-stoichiometric acid iron phosphate material as an iron-phosphorus source can achieve the preparation of a high-performance sodium iron phosphate pyrophosphate positive electrode material.

[0043] Example 8 This embodiment relates to a non-stoichiometric acid ferric phosphate material and a sodium ion battery positive electrode material prepared using the same as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: dilute crude phosphoric acid to obtain dilute phosphoric acid (1.6 wt%), add 0.5 mol / L phthalic acid-hydrochloric acid buffer to the dilute phosphoric acid solution as a buffer solution system, adjust the pH value of the reaction system to be stable at about 2, add ferrous salt (2.2 wt%) according to an iron-phosphorus ratio of 0.75:1 and mix well to obtain a uniform solution; S2. Precipitation and separation of solids: at 70°C, an oxidant is added to the homogeneous solution of step S1 above to rapidly nucleate the solution through an oxidation coprecipitation reaction; after the oxidation reaction is completed, the reaction solution is aged at 40°C for 4h, and the solid obtained by solid-liquid separation is dried in an oven at 100 degrees overnight.

[0044] S3, high temperature calcination: calcine the solid obtained in step S2 at 450° C. for 10 h to remove bound water and obtain a non-stoichiometric acid ferric phosphate material; S4, high temperature sintering: the solid of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode material, the electrochemical properties of which are shown in Table 1. It can be seen that the use of non-stoichiometric acid iron phosphate material as an iron-phosphorus source can achieve the preparation of a high-performance sodium iron phosphate pyrophosphate positive electrode material.

[0045] Example 9 This embodiment relates to a non-stoichiometric acid ferric phosphate material and a sodium ion battery positive electrode material prepared using the same as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: dilute crude phosphoric acid to obtain dilute phosphoric acid (1.6 wt%), add 0.5 mol / L phthalic acid-hydrochloric acid buffer to the dilute phosphoric acid solution as a buffer solution system, adjust the pH value of the reaction system to be stable at about 2, add ferrous salt (2.2 wt%) according to an iron-phosphorus ratio of 0.75:1 and mix well to obtain a uniform solution; S2. Precipitation and separation of solids: at 70°C, an oxidant is added to the homogeneous solution of step S1 above to rapidly nucleate the solution through an oxidation coprecipitation reaction; after the oxidation reaction is completed, the reaction solution is aged at 40°C for 4h, and the solid obtained by solid-liquid separation is dried in an oven at 100 degrees overnight.

[0046] S3, high temperature calcination: calcine the solid obtained in step S2 at 600° C. for 10 h to remove bound water and obtain a non-stoichiometric acid ferric phosphate material; S4, high temperature sintering: the solid sodium source of step S3 is mixed, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode material, the electrochemical properties of which are shown in Table 1. It can be seen that the use of non-stoichiometric acid iron phosphate material as an iron-phosphorus source can achieve the preparation of a high-performance sodium iron phosphate pyrophosphate positive electrode material.

[0047] Example 10 This embodiment relates to a non-stoichiometric acid ferric phosphate material and a sodium ion battery positive electrode material prepared using the same as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: dilute crude phosphoric acid to obtain dilute phosphoric acid (1.6 wt%), add 0.5 mol / L phthalic acid-hydrochloric acid buffer to the dilute phosphoric acid solution as a buffer solution system, adjust the pH value of the reaction system to be stable at about 2, add ferrous salt (2.2 wt%) according to an iron-phosphorus ratio of 0.75:1 and mix well to obtain a uniform solution; S2. Precipitation and separation of solids: at 70°C, an oxidant is added to the homogeneous solution of step S1 above to rapidly nucleate the solution through an oxidation coprecipitation reaction; after the oxidation reaction is completed, the reaction solution is aged at 40°C for 4h, and the solid obtained by solid-liquid separation is dried in an oven at 100 degrees overnight.

[0048] S3, high temperature calcination: calcine the solid obtained in step S2 at 800° C. for 10 h to remove bound water and obtain a non-stoichiometric acid ferric phosphate material; S4, high temperature sintering: the solid of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode material, the electrochemical properties of which are shown in Table 1. It can be seen that the use of non-stoichiometric acid iron phosphate material as an iron-phosphorus source can achieve the preparation of a high-performance sodium iron phosphate pyrophosphate positive electrode material.

[0049] Embodiment 11 This embodiment relates to a non-stoichiometric acid ferric phosphate material and a sodium ion battery positive electrode material prepared using the same as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: dilute crude phosphoric acid to obtain dilute phosphoric acid (1.6 wt%), add 0.5 mol / L phthalic acid-hydrochloric acid buffer to the dilute phosphoric acid solution as a buffer solution system, adjust the pH value of the reaction system to be stable at about 2, add ferrous salt (2.5 wt%) according to an iron-phosphorus ratio of 0.85:1 and mix well to obtain a uniform solution; S2. Precipitation and separation of solids: at 0°C, add an oxidant to the homogeneous solution of step S1 to rapidly nucleate the solution through an oxidation coprecipitation reaction; after the oxidation reaction is completed, the reaction solution is aged at 30°C for 4h, and the solid obtained by solid-liquid separation is dried in an oven at 100 degrees overnight.

[0050] S3, high temperature calcination: calcine the solid obtained in step S2 at 300° C. for 10 h to remove bound water and obtain a non-stoichiometric acid ferric phosphate material; S4, high temperature sintering: the solid of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode material. It can be seen that the use of a non-stoichiometric acid ferric phosphate material as an iron-phosphorus source can achieve the preparation of a high-performance sodium iron phosphate pyrophosphate positive electrode material.

[0051] Example 12 This embodiment relates to a non-stoichiometric acid ferric phosphate material and a sodium ion battery positive electrode material prepared using the same as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: dilute crude phosphoric acid to obtain dilute phosphoric acid (1.6 wt%), add 0.5 mol / L phthalic acid-hydrochloric acid buffer solution to the dilute phosphoric acid solution as a buffer solution system, adjust the pH value of the reaction system to be stable at about 2, add ferrous salt (0.6 wt%) according to an iron-phosphorus ratio of 0.2:1, and mix well to obtain a uniform solution; S2. Precipitation and separation of solids: at 0°C, add an oxidant to the homogeneous solution of step S1 to rapidly nucleate the solution through an oxidation coprecipitation reaction; after the oxidation reaction is completed, the reaction solution is aged at 30°C for 4h, and the solid obtained by solid-liquid separation is dried in an oven at 100 degrees overnight.

[0052] S3, high temperature calcination: calcine the solid obtained in step S2 at 300° C. for 10 h to remove bound water and obtain a non-stoichiometric acid ferric phosphate material; S4, high temperature sintering: the solid of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode material, the electrochemical properties of which are shown in Table 1. It can be seen that the use of non-stoichiometric acid iron phosphate material as an iron-phosphorus source can achieve the preparation of a high-performance sodium iron phosphate pyrophosphate positive electrode material.

[0053] Example 13 This embodiment relates to a non-stoichiometric acid ferric phosphate material and a sodium ion battery positive electrode material prepared using the same as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: dilute crude phosphoric acid to obtain dilute phosphoric acid (1.6 wt%), add 0.5 mol / L phthalic acid-hydrochloric acid buffer to the dilute phosphoric acid solution as a buffer solution system, adjust the pH value of the reaction system to be stable at about 2, add ferrous salt (2.2 wt%) according to an iron-phosphorus ratio of 0.75:1 and mix well to obtain a uniform solution; S2. Precipitation and separation of solids: At 70°C, oxygen is introduced under high pressure into the homogeneous solution of step S1 above to rapidly nucleate through an oxidation coprecipitation reaction; after the oxidation reaction is completed, the reaction solution is aged at 30°C for 4h, and the solid obtained by solid-liquid separation is dried in an oven at 100 degrees overnight.

[0054] S3, high temperature calcination: calcine the solid obtained in step S2 at 300° C. for 10 h to remove bound water and obtain a non-stoichiometric acid ferric phosphate material; S4, high temperature sintering: the solid of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode material, the electrochemical properties of which are shown in Table 1. It can be seen that the use of non-stoichiometric acid iron phosphate material as an iron-phosphorus source can achieve the preparation of a high-performance sodium iron phosphate pyrophosphate positive electrode material.

[0055] Embodiment 14 This embodiment relates to a non-stoichiometric acid ferric phosphate material and a sodium ion battery positive electrode material prepared using the same as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: phosphoric acid and sodium iron pyrophosphate solution are used as phosphorus sources to prepare a reaction solution with a phosphorus concentration (1.6 wt%), 0.5 mol / L phthalic acid-hydrochloric acid buffer is added to the reaction solution as a buffer solution system, the pH value of the reaction system is adjusted to be stable at about 2, and ferrous salt (2.2 wt%) is added according to an iron-phosphorus ratio of 0.75:1 and mixed to obtain a uniform solution; S2. Precipitation and separation of solids: at 70°C, an oxidant is added to the homogeneous solution of step S1 above to rapidly nucleate the solution through an oxidation coprecipitation reaction; after the oxidation reaction is completed, the reaction solution is aged at 40°C for 4h, and the solid obtained by solid-liquid separation is dried in an oven at 100 degrees overnight.

[0056] S3, high temperature calcination: calcine the solid obtained in step S2 at 300° C. for 10 h to remove bound water and obtain a non-stoichiometric acid ferric phosphate material; S4, high temperature sintering: the solid of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode material, the electrochemical properties of which are shown in Table 1. It can be seen that the use of non-stoichiometric acid iron phosphate material as an iron-phosphorus source can achieve the preparation of a high-performance sodium iron phosphate pyrophosphate positive electrode material.

[0057] Embodiment 15 This embodiment relates to a non-stoichiometric acid ferric phosphate material and a sodium ion battery positive electrode material prepared using the same as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: For the reaction solution of ammonium dihydrogen phosphate solution with phosphorus concentration (1.6 wt%), 0.5 mol / L phthalic acid-hydrochloric acid buffer solution was added to the reaction solution as a buffer solution system, the pH value of the reaction system was adjusted to be stable at about 2, and ferrous salt (2.2 wt%) was added according to the iron-phosphorus ratio of 0.75:1 and mixed to obtain a uniform solution; S2. Precipitation and separation of solids: at 70°C, an oxidant is added to the homogeneous solution of step S1 above to rapidly nucleate the solution through an oxidation coprecipitation reaction; after the oxidation reaction is completed, the reaction solution is aged at 40°C for 4h, and the solid obtained by solid-liquid separation is dried in an oven at 100 degrees overnight.

[0058] S3, high temperature calcination: calcine the solid obtained in step S2 at 300° C. for 10 h to remove bound water and obtain a non-stoichiometric acid ferric phosphate material; S4, high temperature sintering: the solid of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode material, the electrochemical properties of which are shown in Table 1. It can be seen that the use of non-stoichiometric acid iron phosphate material as an iron-phosphorus source can achieve the preparation of a high-performance sodium iron phosphate pyrophosphate positive electrode material.

[0059] Comparative Example 1 This embodiment relates to an iron phosphate material and a sodium ion battery positive electrode material prepared using the iron phosphate material as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: dilute crude phosphoric acid to obtain dilute phosphoric acid (1.6 wt%), add 0.5 mol / L acetic acid-sodium acetate buffer to the dilute phosphoric acid solution as a buffer solution system, adjust the pH value of the reaction system to be stable in the range of 3.5, add ferrous salt according to an iron-phosphorus ratio of 0.75:1 and mix well to obtain a uniform solution; S2. Precipitation and separation of solids: at 70°C, an oxidant is added to the homogeneous solution of step S1 to rapidly nucleate the solution through an oxidation coprecipitation reaction; after the oxidation reaction is completed, the solution is aged at 40°C for 4 hours, and the iron phosphate composite material obtained by solid-liquid separation is dried in an oven at 100 degrees overnight.

[0060] S3, high temperature calcination: the solid obtained in step S2 is calcined at 300°C for 10 hours to remove bound water. However, due to the high pH of the reaction solution, part of the iron hydroxide is precipitated and the product is no longer a pure iron phosphate precursor.

[0061] S4, high temperature sintering: the solid of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron pyrophosphate positive electrode material, the electrochemical properties of which are shown in Table 1.

[0062] Comparative Example 2 This embodiment relates to a low iron-phosphorus ratio iron phosphate material and a sodium ion battery positive electrode material prepared using the iron phosphate material as a precursor, and the preparation method thereof comprises the following steps: S1. Preparation of precursor solution: dilute crude phosphoric acid to obtain dilute phosphoric acid (1.6 wt%), adjust the pH value of the reaction system to 0.4, add ferrous salt according to an iron-phosphorus ratio of 0.75:1 and mix well to obtain a uniform solution; S2. Precipitation and separation of solids: at 70°C, an oxidant is added to the homogeneous solution of step S1 above to rapidly nucleate the solution through an oxidation coprecipitation reaction; after the oxidation reaction is completed, the solution is aged at 40°C for 4 hours, and the iron phosphate composite material with bound water obtained by solid-liquid separation is dried in an oven at 100 degrees overnight.

[0063] S3, high temperature calcination: calcine the solid obtained in step S2 at 300° C. for 10 h to remove bound water, thereby obtaining an iron phosphate composite material; S4, high temperature sintering: the iron phosphate composite material of step S3 is mixed with a sodium source, and calcined under an inert atmosphere to obtain a sodium iron phosphate pyrophosphate positive electrode material, the electrochemical properties of which are shown in Table 1.

[0064] Table 1 Performance test results According to the test results in Table 1, it can be seen that: The Fe x H y (PO m ) (3x+y) / (2m-5) The zH2O preparation method can prepare an iron phosphate precursor with an iron-phosphorus ratio of 0.75, with a yield of up to 97%. x H y (PO m ) (3x+y) / (2m-5) · The compacted density of zH2O is higher.

[0065] As the pH regulated by the buffer solution decreases, the aging temperature increases, and the reactant concentration increases, the iron-to-hydrogen ratio (x / y) changes, which directly leads to a change in the iron-to-phosphorus ratio of the product corresponding to the prepared non-stoichiometric acid ferric phosphate, thereby achieving the purpose of controlling the iron-to-phosphorus ratio by controlling the iron-to-hydrogen ratio.

[0066] As can be seen from Examples 1 and 2, 3, and 13, the higher the initial temperature of the reaction, the faster the generation of particles with concentrated particle size distribution and uniform particle distribution; the lower temperature range selected for the aging temperature promotes the slow aggregation and close growth of the particles, and ultimately a spherical material with a high compaction density can be obtained.

[0067] As can be seen from Examples 1 and 4, 5, and 6, as the reactant concentration increases, the iron-to-hydrogen ratio (x / y) of the prepared non-stoichiometric ferric phosphate decreases, while the corresponding iron-to-phosphorus ratio of the product also shows a downward trend.

[0068] As can be seen from Examples 1 and 7, 8, 9, and 10, between 300 and 800 degrees Celsius, as the calcination temperature increases, the water content of the prepared non-stoichiometric ferric phosphate gradually decreases, but it is still suitable for use as a raw material for the synthesis of sodium ferric acid phosphate pyrophosphate.

[0069] As can be seen from Examples 1 and 11 and 12, as the iron-phosphorus ratio of the feed is reduced, as the iron-hydrogen ratio (x / y) of the prepared non-stoichiometric ferric phosphate system decreases, the iron-phosphorus ratio of the corresponding product also shows a downward trend.

[0070] As can be seen from Examples 14 and 15, when other phosphorus sources or mixed phosphorus sources are used, non-stoichiometric iron phosphate with a low iron-hydrogen ratio and similar compaction density characteristics can still be prepared by regulating other parameters, and the electrochemical performance of sodium iron pyrophosphate synthesized using it as a precursor also maintains a high level.

[0071] As can be seen from Examples 1, 2, 3 and Comparative Examples 1 and 2, controlling the pH at about 2 by means of a buffer solution is beneficial to stabilizing the iron-phosphorus ratio of the obtained product, while lowering the pH of the reaction solution significantly reduces the iron-phosphorus ratio and yield of the prepared iron phosphate precursor, while increasing the pH of the reaction causes the precipitation of iron hydroxide and thus leads to an increase in the iron-phosphorus ratio of the product, making it no longer suitable for the synthesis of sodium ferric pyrophosphate.

[0072] The above embodiments are only specific embodiments of the present invention, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and these obvious replacement forms all belong to the protection scope of the present invention.

Claims

1. A method for preparing a non-stoichiometric iron phosphate material, characterized in that The following steps are involved: S1. Preparation of precursor solution: adding a buffer solution to the phosphorus source solution to adjust the pH of the reaction system to 1-3, adding ferrous salt, and mixing to obtain a precursor solution; S2. Solid precipitation and separation: Under temperature control, an oxidant is added to the precursor solution in step S1, and after the oxidation reaction is completed, the temperature is controlled and aged, and the solid-liquid separation is performed to obtain Fe x H y (PO m ) (3x+y) / (2m-5) zH2O solid; In Fe x H y (PO m ) (3x+y) / (2m-5) In zH2O, the iron-hydrogen ratio x / y ranges from 1 / 3 to 17 / 3, x ranges from 0.5 to 0.95, y ranges from 0.15 to 1.5, z ranges from 1 to 4, and m ranges from 3.5 to 4.

2. The method for preparing the non-stoichiometric ferric phosphate material according to claim 1, characterized in that: In step S1, the concentration range of the phosphorus source solution is 0.1-12wt%, the concentration range of the buffer solution is 0.01-1 mol / L, the ferrous ion concentration of the ferrous salt is 0.1-8wt%, and the iron-phosphorus ratio of the feed is 0.2-0.

85.

3. The method for preparing the non-stoichiometric ferric phosphate material according to claim 1, characterized in that: In step S2, the reaction temperature is 30-90°C; the aging conditions are: the aging temperature ranges from 10-90°C, and the aging time is 2-10h.

4. The method for preparing the non-stoichiometric ferric phosphate material according to claim 1, characterized in that: The buffer solution is one or more of disodium hydrogen phosphate-citric acid buffer, phthalic acid-hydrochloric acid buffer, glycine-sulfuric acid buffer, phthalic acid-sulfuric acid buffer, phosphoric acid-sodium dihydrogen phosphate, and oxalic acid-sodium hydrogen oxalate.

5. The method for preparing the non-stoichiometric ferric phosphate material according to claim 1, characterized in that: The ferrous salt is one or more of ferrous sulfate, ferrous sulfate heptahydrate, ferrous chloride, ferrous nitrate, and sodium ferrous sulfate; the phosphorus source is one or more of crude phosphoric acid, refined phosphoric acid, ammonium dihydrogen phosphate, sodium dihydrogen phosphate, and sodium pyrophosphate.

6. The method for preparing the non-stoichiometric ferric phosphate material according to claim 1, characterized in that: The oxidant is one or more of sodium persulfate, hydrogen peroxide, oxygen, ozone, air, sodium hypochlorite, peracetic acid and the like, and the concentration of the hydrogen peroxide is 1-30wt%.

7. The method for preparing the non-stoichiometric ferric phosphate material according to claim 1, characterized in that: The following steps are also included: S3, high temperature calcination: the Fe x H y (PO m ) (3x+y) / (2m-5) · The zH2O solid is calcined at a high temperature to obtain a non-stoichiometric iron phosphate material with all or part of the bound water removed.

8. The method for preparing the non-stoichiometric ferric phosphate material according to claim 7, characterized in that: In step S3, the high temperature calcination conditions are: the calcination temperature is 100-700° C., and the calcination time ranges from 1 to 10 hours.

9. A sodium ion battery positive electrode material, characterized in that: The non-stoichiometric iron phosphate material prepared according to any one of claims 1 to 8 is used as a precursor and mixed with a sodium source and sintered at high temperature to obtain the product.

10. The sodium ion battery positive electrode material according to claim 9, characterized in that: The high temperature sintering conditions are: high temperature roasting at 600-700°C for 8-10h, the protective atmosphere is argon and / or nitrogen; the sodium salt is one or more of sodium carbonate, sodium dihydrogen phosphate, and sodium nitrate.

Citation Information

Patent Citations

  • Method for flexibly regulating and controlling iron-phosphorus ratio of iron phosphate

    CN116409766A

  • Preparation method and application of battery-grade iron hydrogen phosphate

    CN116924369A

  • Method for preparing lithium iron phosphate from hydroxyl iron phosphate and lithium iron phosphate pole piece material and application

    CN117430102A

  • Method for preparing high performance lithium iron phosphate nanopowder

    US20240034626A1

Cited By

  • Iron phosphide precursor and preparation method therefor, sodium iron phosphate pyrophosphate, electrode sheet, battery, and electric device

    WO2026158194A1