A fluorine-doped silicon dioxide material, its preparation method and application

By preparing fluorine-doped silicon dioxide materials and forming SiO2 nanoparticles through acid-base treatment and hydrothermal reaction, the problem of excessively high dielectric constant of high-frequency, low-dielectric-constant resins was solved, and high-frequency, high-speed transmission and signal stability of low-dielectric-modified resin materials were achieved.

CN118771398BActive Publication Date: 2026-11-17GUANGDONG YOUJU ADVANCED NEW MATERIALS CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411078483.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2026-11-17
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The dielectric constant of existing high-frequency, low-dielectric-constant resins is still relatively high, which fails to fully meet the requirements of 5G communication technology for high-frequency, high-speed transmission and signal stability.

Method used

Fluorine-doped silica material was obtained by using magnesium-containing zeolite as raw material, undergoing acid-base treatment, negative pressure wetting, and hydrothermal reaction to form SiO2 nanoparticles, and then calcining and cleaning to obtain fluorine-doped silica material with dielectric constant Dk=2.3~2.7 and dielectric loss Tanδ0.001~0.0025.

Benefits of technology

It significantly reduces the dielectric constant and dielectric loss of the material, improves the electrical properties of the material, and is suitable for low dielectric modified resin materials in 5G communication technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771398B_ABST
    Figure CN118771398B_ABST
Patent Text Reader

Abstract

This invention discloses a fluorine-doped silica material, comprising the following chemical components by weight percentage: 89-93% silicon oxide, 1-3% aluminum oxide, 0.05-0.2% magnesium oxide, 0.5-2% calcium oxide, 1.7-4% ferric oxide, and 3-5% fluorine; wherein the fluorine is linked by Si-F bonds; and the fluorine-doped silica material is composed of agglomerated near-spherical particles of 200-500 nanometers. This invention obtains the modified silica material by treating it with a magnesium-containing zeolite alkali / acid, reacting it with ammonium fluoride, and finally calcining it. The modified silica material of this invention has the advantage of low dielectric constant.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of silicon materials technology. Background Technology

[0002] High-frequency low-dielectric-constant resins are materials with low loss, high-frequency response, and good electrical properties, and are widely used in microwave communication, wireless networks, and radio frequency modules. With the development of 5G communication technology, the requirements for high-frequency, high-speed transmission and signal stability are increasing. High-frequency low-dielectric-constant resins have attracted much attention due to their excellent performance; however, their dielectric constant is still relatively high (Dk>3), which does not fully meet the requirements.

[0003] Adding low-dielectric inorganic fillers can effectively reduce the dielectric constant of engineering composite resins. Currently, low-dielectric inorganic fillers are mainly composed of silicon oxide (Dk=4). One type involves introducing air (Dk=1) through hollow glass microspheres or aerogels to reduce the average dielectric constant; another type involves doping to obtain fluorinated SiO2, because fluorine can effectively reduce the dipole polarization of the dielectric, thereby achieving the purpose of reducing the dielectric constant. Summary of the Invention

[0004] The purpose of this invention is to provide a low-dielectric fluorine-doped silicon dioxide material, as well as a testing method and application.

[0005] This invention is achieved through the following technical solution: A fluorine-doped silicon dioxide material, by weight percentage, comprises the following chemical components: 89-93% silicon oxide, 1-3% aluminum oxide, 0.5-2% calcium oxide, 1.7-4% ferric oxide, 0.05-0.2% magnesium oxide, and 3-5% fluorine; wherein the fluorine is linked to the silicon oxide through Si-F bonds. Furthermore, fluorine-doped silicon dioxide materials are composed of agglomerated spherical particles of 200-500 nanometers (see appendix). Figure 1 ).

[0006] The dielectric constant D of the fluorine-doped silicon dioxide material of the present invention k =2.3~2.7, dielectric loss Tanδ is 0.001~0.0025.

[0007] The method for preparing fluorine-doped silicon dioxide material of the present invention includes the following steps: Step A: The zeolite is first treated with an alkaline solution, and then treated with an acidic solution. After solid-liquid separation, modified zeolite A is obtained. Step B: Mix the fluorinating agent aqueous solution with modified zeolite A and stir under negative pressure to obtain modified zeolite B; Step C: The modified zeolite B is subjected to a hydrothermal reaction to obtain modified zeolite C; Step D: Calcine the modified zeolite C at 500~700℃, and then clean and crush it to obtain fluorine-doped silicon dioxide material.

[0008] The zeolite used in this invention is a magnesium-containing zeolite, wherein the magnesium content is 0.5-2%. The fluorine-doped silica material obtained after treatment by the method of this invention also contains 0.05-0.2% magnesium oxide.

[0009] In step A, the aqueous solution of the alkali is either NaOH / water or KOH / water, with a concentration range of 0.05~1M; the aqueous solution of the acid is either sulfuric acid / water, hydrochloric acid / water, or nitric acid / water, with a concentration range of 0.2~2M; the alkali treatment time ranges from 20 to 50 minutes, and the temperature ranges from 40 to 80 degrees Celsius. o C; The acid treatment time range is 2~5 hours, and the temperature range is 60~90 degrees Celsius. o C.

[0010] In step B, the fluorinating agent is selected from at least one of ammonium fluoride and ammonium bifluoride, and its aqueous solution concentration is 0.1~2M; the negative pressure condition is -5~-20MPa; and the temperature range is 15~30℃. o C.

[0011] In step C, the hydrothermal reaction is carried out at 150-200 °C for 4-12 h.

[0012] In step C, the calcination time is 2~10 hours.

[0013] The application of fluorine-doped silica materials is for the preparation of low-dielectric modified resin materials. The resins can be commonly used 5G engineering resins such as LCP, PPS, PEI, and PBT. When the fluorine-doped silica material of this invention is ground to a particle size of 500 nm to 5 μm, it can be applied to low-dielectric modified resin materials.

[0014] The present invention has the following beneficial effects: This invention uses magnesium-containing zeolite as raw material. First, it undergoes acid and alkali treatment to facilitate the dissolution of magnesium-containing substances through acid / alkali reactions, thereby expanding the structural pores and removing metallic impurities. Negative pressure wetting ensures sufficient contact between the zeolite interior and the fluorinating agent. Then, taking advantage of the much higher dissolution rate of aluminum compared to silicon during the hydrothermal reaction, the zeolite structure collapses to form SiO2 nanoparticles, which are then fluorinated. Magnesium, rich in hydroxyl groups, effectively reduces the polarity of the zeolite through dissolution. Surface residues are removed by calcination and cleaning, followed by re-pulverization to obtain the final fluorinated SiO2 nanomaterial. This material exhibits a low dielectric constant Dk = 2.3~2.7 and a dielectric loss of 0.001~0.0025 (Tanδ). Attached Figure Description

[0015] Figure 1 Microscopic morphology images of the fluorine-doped silicon dioxide material at different scales in this invention. Detailed Implementation

[0016] The present invention will now be described in detail with reference to specific embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the invention in any way. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.

[0017] The raw materials used in this invention are sourced from the following sources: Magnesium-containing zeolite: contains approximately 2% magnesium, has a dielectric constant of approximately 3.8, and a dielectric loss of approximately 0.1.

[0018] Magnesium-free zeolite: magnesium content <0.02%, dielectric constant approximately 3.5, dielectric loss approximately 0.1.

[0019] Hydrochloric acid, sulfuric acid, alkali, fluorinating agents, etc. are analytical grade raw materials, and water is distilled water.

[0020] The following are the preparation methods of the materials used in the examples and comparative examples:

[0021] Example 1: Step A: Magnesium-containing zeolite was first treated with alkali in 0.5M NaOH / water solution at 60°C for 30 min, and then treated with acid in 0.7M sulfuric acid / water solution at 80°C for 3 h. After solid-liquid separation, modified zeolite A was obtained. Step B: Mix 0.7M ammonium fluoride / water solution and 0.7M ammonium bifluoride / water solution at a ratio of 3:1, then mix with the above modified zeolite A, and stir at -10MPa and room temperature for 20 min to obtain modified zeolite B; Step C: The modified zeolite B is subjected to a hydrothermal reaction at 150℃ for 6 hours to obtain modified zeolite C; Step D: Calcine the modified zeolite C at 600℃ for 6 hours, wash it with distilled water, and pulverize it to obtain fluorine-doped silicon dioxide material.

[0022] Example 2: Step A: Magnesium-containing zeolite was first treated with alkali in 0.5M NaOH / water solution at 60°C for 40 min, and then treated with acid in 0.7M sulfuric acid / water solution at 90°C for 2 h. After solid-liquid separation, modified zeolite A was obtained. Step B: Mix 0.5M ammonium fluoride / water solution with the above modified zeolite A, stir at -10MPa and room temperature for 20 min to obtain modified zeolite B; Step C: The modified zeolite B is subjected to a hydrothermal reaction at 180℃ for 8 hours to obtain modified zeolite C; Step D: Calcine the modified zeolite C at 550℃ for 5 hours, wash it with distilled water, and pulverize it to obtain fluorine-doped silicon dioxide material.

[0023] Example 3: Step A: Magnesium-containing zeolite was first treated with alkali in 0.4M NaOH / water solution at 60°C for 50 min, and then treated with acid in 0.6M sulfuric acid / water solution at 60°C for 4 h. After solid-liquid separation, modified zeolite A was obtained. Step B: Mix 0.7M ammonium bifluoride / water solution with the above modified zeolite A, stir at -5MPa and room temperature for 15 min to obtain modified zeolite B; Step C: The modified zeolite B is subjected to a hydrothermal reaction at 160℃ for 6 hours to obtain modified zeolite C; Step D: Calcine the modified zeolite C at 660℃ for 6 hours, wash with distilled water, and pulverize to obtain fluorine-doped silicon dioxide material.

[0024] Example 4: Step A: Magnesium-containing zeolite was first treated with alkali in 0.1M NaOH / water solution at 80°C for 50 min, and then treated with acid in 0.5M sulfuric acid / water solution at 70°C for 3 h. After solid-liquid separation, modified zeolite A was obtained. Step B: Mix 0.7M ammonium fluoride / water solution and 0.7M ammonium bifluoride / water solution at a ratio of 3:1, then mix with the above modified zeolite A, and stir at -10MPa and room temperature for 20 min to obtain modified zeolite B; Step C: The modified zeolite B is subjected to a hydrothermal reaction at 180℃ for 10 hours to obtain modified zeolite C; Step D: Calcine the modified zeolite C at 550℃ for 5 hours, wash it with distilled water, and pulverize it to obtain fluorine-doped silicon dioxide material.

[0025] Example 5: Step A: Magnesium-containing zeolite was first treated with alkali in 1M NaOH / water solution at 70°C for 30 min, and then treated with acid in 1.5M sulfuric acid / water solution at 60°C for 3 h. After solid-liquid separation, modified zeolite A was obtained. Step B: Mix 0.7M ammonium fluoride / water solution and 0.7M ammonium bifluoride / water solution at a ratio of 3:1, then mix with the above modified zeolite A, and stir at -15MPa and room temperature for 20 min to obtain modified zeolite B; Step C: The modified zeolite B is subjected to a hydrothermal reaction at 150℃ for 6 hours to obtain modified zeolite C; Step D: Calcine the modified zeolite C at 660℃ for 8 hours, wash with distilled water, and pulverize to obtain fluorine-doped silicon dioxide material.

[0026] Comparative Example 1: The difference from Example 1 is that the magnesium-containing zeolite is replaced with magnesium-free zeolite.

[0027] Comparative Example 2: The difference from Example 2 is that in step B, ammonium fluoride / water solution of the same concentration is used instead of HF / water solution.

[0028] Test methods for various parameters in the examples and comparative examples: (1) Elemental content of fluorine-doped silica: Samples were prepared using the borate melting method. 1.5 g of powdered sample was placed in a Pt / Au alloy (95% / 5%) crucible. Then, 10 g of lithium tetraborate and a lithium metaborate flux containing 0.5% lithium iodide (50:50 ratio) were added to the crucible. The crucible was then placed in a high-temperature environment and the sample was melted at 1050°C for 20 minutes. The molten glass sample was analyzed in detail using a Panalytical Axios WD-XRF instrument.

[0029] (2) Dielectric properties: The dielectric properties of the powder samples at frequencies of 1~8 GHz were tested using a 3656B vector network analyzer from China Electronics Technology Group Corporation (CETC) using the coaxial method. The sample and paraffin were mixed at a mass ratio of 5:5 and pressed into a ring with a thickness of about 3.2 mm.

[0030] Table 1: Component content and test results of fluorine-doped silica materials in the examples and comparative examples Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Comparative Example 2 Oxides of silicon, % 91.32 90.62 90.23 89.96 91.76 90.13 93.31 Alumina, % 1.31 1.58 1.53 2.03 1.11 2.47 2.12 Calcium oxide, % 1.08 1.27 1.33 1.62 1.14 1.51 1.30 Ferric oxide, % 1.72 2.02 1.93 3.12 2.05 1.83 0.90 Magnesium oxide, % 0.05 0.06 0.12 0.16 0.15 0 0.02 Fluorine element, % 4.42 4.03 3.96 3.04 3.56 3.33 2.02 Other elements, % 0.10 0.42 0.90 0.07 0.23 0.73 0.33 <![CDATA[dielectric constant (D k )]]> 2.35 2.50 2.63 2.70 2.65 3.05 2.96 Dielectric loss (Tanδ) 0.0012 0.0013 0.0013 0.0015 0.0018 0.0015 0.0257 As can be seen from Examples 1-5, the fluorine-doped silicon dioxide material obtained by the process of this application has excellent dielectric properties.

[0031] As can be seen from Comparative Example 1, even if the fluorine content is brought to the range of 3-5% using the process of this application, good dielectric properties cannot be obtained by using magnesium-free zeolite.

[0032] As can be seen from Comparative Example 2, when ammonium fluoride / water solution is replaced with HF / water solution, it is difficult to obtain materials with high F content. At the same time, the content of other elements is not within the scope of this invention, so the dielectric properties are poor.

[0033] The following are examples of applications of fluorine-doped silicon dioxide materials: Processing method: The resin and filler are premixed, and then melted and granulated using a twin-screw extruder at their respective suitable temperatures to obtain a composite resin. The filler is: the fluorine-doped silica material (F-SiO2) and hollow glass microspheres (HG) of this invention. The dielectric properties at 5 GHz when the filling amount is 5% are shown in the table below.

[0034] LCP LCP+HG <![CDATA[LCP+F-SiO2]]> PPS PPS+HG <![CDATA[PPS+F-SiO2]]> PBT PBT+HG <![CDATA[PBT+F-SiO2]]> <![CDATA[D k ]]> 3.1 2.75 2.73 3.0 2.71 2.74 3.15 2.86 2.88 Tanδ 0.0011 0.0012 0.0012 0.014 0.015 0.015 0.01 0.012 0.012 It is evident that the fluorine-doped silicon dioxide material of the present invention can significantly improve the dielectric properties of LCP, PPS, and PBT.

Claims

1. A fluorine-doped silicon dioxide material, characterized in that, By weight percentage, it includes the following chemical components: 89-93% silicon oxide, 1-3% aluminum oxide, 0.5-2% calcium oxide, 1.7-4% ferric oxide, 0.05-0.2% magnesium oxide, and 3-5% fluorine; wherein, fluorine is linked to silicon oxide through Si-F bonds. Furthermore, fluorine-doped silica materials are composed of agglomerated near-spherical particles of 200-500 nanometers. The method for preparing the fluorine-doped silicon dioxide material includes the following steps: Step A: The zeolite is first treated with an alkaline solution, and then treated with an acidic solution. After solid-liquid separation, modified zeolite A is obtained. Step B: Mix the fluorinating agent aqueous solution with modified zeolite A and stir under negative pressure to obtain modified zeolite B; Step C: The modified zeolite B is subjected to a hydrothermal reaction to obtain modified zeolite C; Step D: Calcine the modified zeolite C at 500~700℃, and then clean and crush it to obtain fluorine-doped silica material; The fluorinating agent is selected from at least one of ammonium fluoride and ammonium bifluoride, and its aqueous solution concentration is 0.1~2M; The zeolite is a magnesium-containing zeolite with a magnesium content of 0.5-2%.

2. The fluorine-doped silicon dioxide material of claim 1, wherein, Dielectric constant of fluorine-doped silicon dioxide material k = 2.3-2.7, dielectric loss Tan δ is 0.001-0.0025.

3. A method for producing the fluorine-doped silicon dioxide material as claimed in any one of claims 1-2, characterized in that, Includes the following steps: Step A: The zeolite is first treated with an alkaline solution, and then treated with an acidic solution. After solid-liquid separation, modified zeolite A is obtained. Step B: Mix the fluorinating agent aqueous solution with modified zeolite A and stir under negative pressure to obtain modified zeolite B; Step C: The modified zeolite B is subjected to a hydrothermal reaction to obtain modified zeolite C; Step D: Calcine the modified zeolite C at 500~700℃, and then clean and crush it to obtain fluorine-doped silica material; The fluorinating agent is selected from at least one of ammonium fluoride and ammonium bifluoride, and its aqueous solution concentration is 0.1~2M; The zeolite is a magnesium-containing zeolite with a magnesium content of 0.5-2%.

4. The method for preparing fluorine-doped silicon dioxide material according to claim 3, characterized in that, In step A, the aqueous solution of the alkali is NaOH / water solution or KOH / water solution, with a concentration range of 0.05~1M; the aqueous solution of the acid is sulfuric acid / water solution, hydrochloric acid / water solution or nitric acid / water solution, with a concentration range of 0.2~2M; the alkali treatment time range is 20~50min, and the temperature range is 40~80℃; the acid treatment time range is 2~5h, and the temperature range is 60~90℃.

5. The method for preparing fluorine-doped silicon dioxide material according to claim 3, characterized in that, In step B, the temperature range is 15~30℃.

6. The method for preparing fluorine-doped silicon dioxide material according to claim 3, characterized in that, In step C, the hydrothermal reaction is carried out at 150-200 °C for 4-12 h.

7. The method for preparing fluorine-doped silicon dioxide material according to claim 3, characterized in that, In step D, the calcination time is 2~10h.

8. The application of the fluorine-doped silicon dioxide material according to any one of claims 1-2, characterized in that, Used to prepare low dielectric modified resin materials.

Citation Information

Patent Citations

  • Low dielectric silica powder, resin composition containing the silica powder, and method for manufacturing low dielectric silica powder

    CN113754928A

  • Low-dielectric high-temperature-resistant silicon dioxide in-situ chemical composite powder as well as preparation method and application thereof

    CN118073005A