Preparation method and application of high-nickel cobalt-free positive electrode precursor material

By using organic amines as precipitants to prepare high-nickel and cobalt-free cathode materials in co-precipitation reactions, the problem of structural stability and performance degradation of high-nickel and cobalt-containing materials during cycling is solved, and high capacity, excellent rate and cycle performance are achieved. cathode material suitable for mass production.

CN118771471APending Publication Date: 2024-10-15JINGMEN GEM NEW MATERIAL CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410758883.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing high-nickel and cobalt-containing cathode materials suffer from lattice collapse and particle fragmentation due to microcracks during long cycles, resulting in a decrease in rate performance and cycle life, making it difficult to achieve excellent electrochemical performance and structural stability.

Method used

Organic amines are used as precipitants to prepare high-nickel and cobalt-free cathode precursor materials through co-precipitation reactions, which avoids the difficulty of pH control and uneven sedimentation. The resulting material has a more complete structure, a lower degree of cation mixing, and excellent Cycling performance and rate performance.

Benefits of technology

A high-nickel and cobalt-free cathode material that achieves high capacity, high rate performance and excellent cycle performance, and the preparation method is simple to operate, has few control process parameters, is suitable for large-scale production, and has low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771471A_ABST
    Figure CN118771471A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of a high-nickel cobalt-free positive electrode precursor material. The preparation method comprises the following steps: mixing reaction raw materials including a high-nickel cobalt-free mixed salt solution and a precipitant solution in a protective atmosphere, and carrying out a co-precipitation reaction to obtain the high-nickel cobalt-free positive electrode precursor material, wherein the precipitant solution comprises an organic amine solution. According to the preparation method provided by the invention, the organic amine is used as a precipitator, OH <-> can be stably provided without the action of a complexing agent, and the conditions that the pH is not easy to control and the sedimentation is not uniform are avoided, so that the positive electrode material prepared from the obtained high-nickel cobalt-free precursor material is more complete in structure, lower in cation mixing degree and higher in specific surface area. And the lithium ion battery has excellent cycle performance and rate capability, and is relatively high in capacity. In addition, the preparation method provided by the invention also has the advantages of simplicity in operation, few control process parameters, low requirements on reaction equipment and low preparation cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium-ion batteries and relates to a preparation method and application of a high-nickel cobalt-free positive electrode precursor material. Background Art

[0002] The growing global electric vehicle (EV) market has put forward higher requirements on the cost and energy density of lithium-ion battery electrode materials. Among the existing positive electrode materials, high-nickel layered LiNi x Co y Mn 1-x-y O2(NCM, x ≥ 0.8) and LiNi x Co y Al 1-x-y O2 (NCA, x ≥ 0.8) is considered to be one of the most promising cathode materials for electric vehicles due to its high theoretical specific capacity and operating voltage. However, due to the scarcity and high price of cobalt (Co) resources on the earth, it poses a major challenge to the low-cost and sustainable goals pursued by the battery industry. Therefore, low-cobalt or cobalt-free has become a research hotspot for high-nickel layered cathode materials.

[0003] In high-nickel and cobalt-containing ternary cathode materials, the cobalt element not only plays a role in stabilizing the structure, but also improves the conductivity, playing a very important role. After cobalt-free, the high-nickel layered cathode materials will suffer from lattice collapse and particle breakage caused by microcracks during long cycles, which will lead to a decrease in rate performance and cycle life, resulting in huge challenges in structural stability, rate performance, cycle life, etc. Therefore, in nickel-rich cathode materials, it is a considerable challenge to significantly reduce or even remove the cobalt content while achieving excellent electrochemical performance.

[0004] Therefore, how to obtain high-nickel cobalt-free positive electrode materials with high capacity, excellent rate performance and cycle performance is an urgent problem to be solved. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention aims to provide a method for preparing a high-nickel cobalt-free positive electrode precursor material and its application. The preparation method provided by the present invention uses an organic amine as a precipitant and can stably provide OH without the need for a complexing agent. - , avoiding the situation that pH is difficult to control and uneven sedimentation, the cathode material prepared from the high-nickel cobalt-free precursor material thus obtained has a more complete structure, a lower degree of cation mixing, excellent cycle performance and rate performance, and a higher capacity. In addition, the preparation method provided by the present invention also has the advantages of simple operation, few control process parameters, low requirements for reaction equipment, and low preparation cost.

[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a method for preparing a high-nickel cobalt-free positive electrode precursor material, the preparation method comprising the following steps:

[0008] The reaction raw materials include a high-nickel cobalt-free mixed salt solution and a precipitant solution. Under a protective atmosphere, the reaction raw materials are mixed to perform a coprecipitation reaction to obtain the high-nickel cobalt-free positive electrode precursor material;

[0009] Wherein, the precipitant solution includes an organic amine solution.

[0010] It should be noted that the definition of high nickel in the present invention is that the stoichiometric ratio of nickel in the positive electrode material is ≥ 0.8 or the molar proportion of nickel in the non-lithium metal element is ≥ 80%.

[0011] It should be noted that the protective atmosphere in the present invention is a conventional technical choice, including but not limited to nitrogen atmosphere or inert gas atmosphere (such as argon, helium) and the like.

[0012] The preparation method provided by the present invention uses organic amine as a precipitant and can stably provide OH without the action of a complexing agent. - , avoiding the situation that the pH is difficult to control and the sedimentation is uneven. The positive electrode material prepared from the high-nickel cobalt-free precursor material thus obtained has a more complete structure, a lower degree of cation mixing (lithium-nickel mixing), excellent cycle performance and rate performance, and a higher capacity. In addition, the preparation method provided by the present invention also has the advantages of simple operation, few control process parameters, low requirements for reaction equipment, and low preparation cost, and is suitable for large-scale production.

[0013] In the present invention, if the precipitant is not an organic amine but a conventional precipitant, such as liquid caustic soda, then a complexing agent needs to be added. Since the solubility product constants of metal elements such as nickel, magnesium, and aluminum are quite different, such as Al 3+ It is difficult to react with ammonia water, and it is very easy to form flocculent products. In addition, Al(OH)3 is an amphoteric hydroxide, which will generate aluminate ions at high pH values, which is prone to uneven sedimentation. Moreover, when the solutions are mixed, NH 4+ It will react with the surrounding solution first to form a concentration gradient, making the pH of the solution difficult to control. At the same time, when a sulfate mixed solution is used in the reaction process, it will react with ammonia water to produce wastewater that is difficult to treat. In addition, the prepared high-nickel cobalt-free precursor material has problems such as uneven particle distribution, partial agglomeration, and high degree of cation mixing.

[0014] Preferably, the high-nickel cobalt-free mixed salt solution includes, in addition to nickel, non-cobalt transition metal elements.

[0015] Preferably, the non-cobalt transition metal element includes any one of manganese, magnesium or aluminum, or a combination of at least two of them. Typical but non-limiting combinations include a combination of manganese and magnesium, a combination of manganese and aluminum, and a combination of magnesium and aluminum.

[0016] Preferably, the concentration of the high-nickel cobalt-free mixed salt solution is 80-120 g / L, for example 80 g / L, 90 g / L, 100 g / L, 110 g / L or 120 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] Preferably, the mass concentration of the organic amine solution is 30-60%, for example 30%, 33%, 35%, 38%, 40%, 43%, 45%, 48%, 50%, 53%, 55%, 58% or 60%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] In the present invention, if the mass concentration of the organic amine is too low, it will be unfavorable for the organic amine to dissolve in the salt solution, resulting in incomplete precipitation of salt ions and reduced yield. If the mass concentration of the organic amine is too high, the salt ion concentration will be too low, resulting in less precipitation and a corresponding reduction in yield.

[0019] Preferably, the organic amine includes any one or a combination of at least two of di-n-butylamine (DNBA), 2-amino-2-methyl-1-propanol (isobutanolamine, AMP), trisaminopropanol (3-hydroxypropylamine, MPA), dimethylethanolamine (DMEA) or diethylaminoethanol (N,N-diethylethanolamine, DMAP).

[0020] Preferably, the feed rate of the high-nickel cobalt-free mixed salt solution is 8 to 10 L / h, for example 8 L / h, 8.5 L / h, 9 L / h, 9.5 L / h or 10 L / h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] Preferably, the feed rate of the precipitant solution is 0.5 to 1.5 L / h, for example, 0.5 L / h, 0.6 L / h, 0.7 L / h, 0.8 L / h, 0.9 L / h, 1 L / h, 1.1 L / h, 1.2 L / h, 1.3 L / h, 1.4 L / h or 1.5 L / h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] Preferably, the reaction raw materials also include a doping salt solution.

[0023] Preferably, the doping salt solution comprises a zirconium salt solution.

[0024] In the present invention, zirconium is further doped during the preparation process, which can improve the atomic stability in the material lattice, and can improve the cycle performance and thermal stability of the material, opening up a new path for the sustainable development of electric vehicle batteries.

[0025] Preferably, the concentration of the doped salt solution is 1 to 10 g / L, for example, 1 g / L, 2 g / L, 3 g / L, 4 g / L, 5 g / L, 6 g / L, 7 g / L, 8 g / L, 9 g / L or 10 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, the feed rate of the doping salt solution is 0.3-0.5 L / h, such as 0.3 L / h, 0.4 L / h or 0.5 L / h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the reaction speed of the coprecipitation reaction is 100-500 r / min, for example, 100 r / min, 150 r / min, 200 r / min, 250 r / min, 300 r / min, 350 r / min, 400 r / min, 450 r / min or 500 r / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] Preferably, the temperature of the coprecipitation reaction is 75-85°C, for example 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C or 85°C, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] In the present invention, if the temperature of the coprecipitation reaction is too low, below 75°C, the ion activity in the solution is low, which will cause incomplete reaction and affect the yield; if the temperature is too high, exceeding 85°C, the volatilization amount of organic amine in the solution increases, resulting in incomplete precipitation of salt ions and reduced yield.

[0030] Preferably, the pH of the coprecipitation reaction is 10-12, for example, 10, 10.3, 10.5, 10.8, 11, 11.3, 11.5, 11.8 or 12, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] It should be noted that, in the present invention, after the coprecipitation reaction is completed, conventional washing and drying processes are sequentially performed.

[0032] As a preferred technical solution, the preparation method comprises the following steps:

[0033] A high-nickel cobalt-free mixed salt solution with a concentration of 80 to 120 g / L is mixed at a feeding rate of 8 to 10 L / h, an organic amine solution with a mass concentration of 30 to 60% is mixed at a feeding rate of 0.5 to 1.5 L / h, and a zirconium salt solution with a concentration of 1 to 10 g / L is mixed at a feeding rate of 0.3 to 0.5 L / h. In an environment with a pH of 10 to 12, a coprecipitation reaction is carried out at a reaction speed of 100 to 500 r / min at 75 to 85° C. to obtain the high-nickel cobalt-free positive electrode precursor material.

[0034] In a second aspect, the present invention provides a high-nickel, cobalt-free positive electrode precursor material, wherein the high-nickel, cobalt-free positive electrode precursor material is prepared by the preparation method described in the first aspect.

[0035] In a third aspect, the present invention provides a high-nickel cobalt-free positive electrode material, wherein the high-nickel cobalt-free positive electrode material is obtained by mixing and sintering the high-nickel cobalt-free positive electrode precursor material as described in the second aspect with a lithium source.

[0036] In the present invention, the method for preparing the positive electrode material from the high-nickel cobalt-free positive electrode precursor material is a conventional technical means. Exemplarily, the present invention provides a preparation process of a high-nickel cobalt-free positive electrode material:

[0037] The high-nickel-cobalt-free positive electrode precursor material of the second aspect is mixed evenly with a lithium source at a molar ratio of Me:Li of 1:(1.03-1.06), and heated from room temperature to 700-800°C at a heating rate of 4-6°C / min in an oxygen-containing atmosphere, calcined and kept at this temperature for 12-20 hours, and then naturally cooled to room temperature to obtain a high-nickel-cobalt-free positive electrode material;

[0038] Optionally, the mixing time is 30 to 40 minutes, the lithium source includes but is not limited to at least one of lithium hydroxide, lithium carbonate or lithium acetate; the oxygen-containing atmosphere includes air atmosphere or oxygen atmosphere, etc.

[0039] Those skilled in the art can make adaptive selection and adjustment of the above preparation process and parameters according to actual needs.

[0040] In a fourth aspect, the present invention further provides a lithium-ion battery, wherein the lithium-ion battery comprises the high-nickel cobalt-free positive electrode material as described in the third aspect.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] The preparation method provided by the present invention uses organic amine as a precipitant and can stably provide OH without the action of a complexing agent. -, avoiding the situation that the pH is difficult to control and the sedimentation is uneven. The positive electrode material prepared from the high-nickel cobalt-free precursor material thus obtained has a more complete structure, a lower degree of cation mixing (lithium-nickel mixing), excellent cycle performance and rate performance, and a higher capacity. In addition, the preparation method provided by the present invention also has the advantages of simple operation, few control process parameters, low requirements for reaction equipment, and low preparation cost, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is an SEM image of the high-nickel, cobalt-free positive electrode precursor material prepared by the preparation method provided in Example 1.

[0044] Figure 2 This is an EDS graph of Zr in the high-nickel cobalt-free positive electrode precursor material prepared by the preparation method provided in Example 1. DETAILED DESCRIPTION

[0045] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions.

[0047] Example 1

[0048] This embodiment provides a high-nickel cobalt-free positive electrode precursor material, and the preparation method of the high-nickel cobalt-free positive electrode precursor material is as follows:

[0049] Nitrogen was introduced into the reactor, and then a metal salt mixed solution with a molar ratio of Ni:Al:Mg of 94:5:1 and a concentration of 100 g / L, a di-n-butylamine solution with a mass concentration of 45%, and a 5 g / L zirconium sulfate solution were added into the reactor at stable speeds of 9 L / h, 1 L / h, and 0.4 L / h, respectively, to start a coprecipitation reaction. During the reaction, the rotation speed was controlled at 300 r / min, the temperature of the reactor was stably controlled at 82°C, and the pH of the reaction system was controlled to be 11 during the reaction. As the coprecipitation reaction proceeded, when the particle size D50 of the sample in the reactor reached 4.5 μm, the feeding was stopped, and the reaction was continued until the material reaction was complete. The precursor was then post-treated by washing and drying to obtain a high-nickel and cobalt-free positive electrode precursor material.

[0050] Figure 1The SEM image of the high-nickel cobalt-free positive electrode precursor material prepared by the preparation method provided in Example 1 is shown. Figure 1 It can be seen that the crystals prepared by this method have uniform particle size, narrow particle size distribution range and no agglomeration phenomenon. The surface of the precursor material is regular, the sphericity is high, and the crystal structure is complete.

[0051] Figure 2 The EDS graph of Zr in the high-nickel cobalt-free positive electrode precursor material prepared by the preparation method provided in Example 1 is shown. Figure 2 It can be seen that the Zr element doped in the precursor material can be clearly observed and is evenly distributed, indicating that the distribution of doped elements in the material prepared by this method is good.

[0052] Example 2

[0053] This embodiment provides a high-nickel cobalt-free positive electrode precursor material, and the preparation method of the high-nickel cobalt-free positive electrode precursor material is as follows:

[0054] Nitrogen was introduced into the reactor, and then a metal salt mixed solution with a concentration of 120 g / L and a molar ratio of Ni:Al:Mg of 94:5:1, a di-n-butylamine solution with a mass concentration of 60%, and a 10 g / L zirconium sulfate solution were added into the reactor at stable speeds of 10 L / h, 1.5 L / h, and 0.5 L / h, respectively, to start a coprecipitation reaction. During the reaction, the rotation speed was controlled at 500 r / min, the temperature of the reactor was stably controlled at 85°C, and the pH of the reaction system was controlled to be 10.3 during the reaction. As the coprecipitation reaction proceeded, when the particle size D50 of the sample in the reactor reached 4.5 μm, the feeding was stopped, and the reaction was continued until the material reaction was complete, and then the precursor was post-treated such as washing and drying to obtain a high-nickel and cobalt-free positive electrode precursor material.

[0055] Example 3

[0056] This embodiment provides a high-nickel cobalt-free positive electrode precursor material, and the preparation method of the high-nickel cobalt-free positive electrode precursor material is as follows:

[0057] Nitrogen was introduced into the reactor, and then a metal salt mixed solution with a concentration of 80 g / L and a molar ratio of Ni:Al:Mg of 94:5:1, a di-n-butylamine solution with a mass concentration of 30%, and a zirconium sulfate solution of 1 g / L were added into the reactor at stable speeds of 8 L / h, 0.5 L / h, and 0.3 L / h, respectively, to start a coprecipitation reaction. During the reaction, the rotation speed was controlled at 100 r / min, the temperature of the reactor was stably controlled at 75°C, and the pH of the reaction system was controlled to be 11.8 during the reaction. As the coprecipitation reaction proceeded, when the particle size D50 of the sample in the reactor reached 4.5 μm, the feeding was stopped, and the reaction was continued until the material reaction was complete, and then the precursor was post-treated such as washing and drying to obtain a high-nickel and cobalt-free positive electrode precursor material.

[0058] Example 4

[0059] The difference between this embodiment and embodiment 1 is that the high-nickel cobalt-free mixed salt solution in this embodiment is a nickel-manganese mixed salt solution (the molar ratio of nickel to manganese is 9:1).

[0060] The rest of the preparation methods and parameters were the same as those in Example 1.

[0061] Example 5

[0062] The difference between this embodiment and embodiment 1 is that in the preparation method provided in this embodiment, no zirconium sulfate solution is added, that is, no doping is performed.

[0063] The rest of the preparation methods and parameters were the same as those in Example 1.

[0064] Example 6

[0065] The difference between this embodiment and embodiment 1 is that in this embodiment, the di-n-butylamine solution is replaced by a 2-amino-2-methyl-1-propanol (AMP) solution, that is, the precipitant solution is a 2-amino-2-methyl-1-propanol (AMP) solution.

[0066] The rest of the preparation methods and parameters were the same as those in Example 1.

[0067] Example 7

[0068] The difference between this embodiment and embodiment 1 is that the mass concentration of the di-n-butylamine solution in this embodiment is 20%.

[0069] The rest of the preparation methods and parameters were the same as those in Example 1.

[0070] Example 8

[0071] The difference between this embodiment and embodiment 1 is that the mass concentration of the di-n-butylamine solution in this embodiment is 70%.

[0072] The rest of the preparation methods and parameters were the same as those in Example 1.

[0073] Example 9

[0074] The difference between this embodiment and embodiment 1 is that the temperature of the coprecipitation reaction in this embodiment is 70°C.

[0075] The rest of the preparation methods and parameters were the same as those in Example 1.

[0076] Example 10

[0077] The difference between this embodiment and embodiment 1 is that the temperature of the coprecipitation reaction in this embodiment is 100°C.

[0078] The rest of the preparation methods and parameters were the same as those in Example 1.

[0079] Comparative Example 1

[0080] This comparative example provides a high-nickel cobalt-free positive electrode precursor material, and the preparation method of the high-nickel cobalt-free positive electrode precursor material is as follows:

[0081] Nitrogen was introduced into the reactor, and then a metal salt mixed solution with a concentration of 100 g / L and a molar ratio of Ni:Al:Mg of 94:5:1, a sodium hydroxide solution with a mass concentration of 30%, an ammonia solution with a mass concentration of 20%, and a 5 g / L zirconium sulfate solution were added into the reactor at stable speeds of 9 L / h, 2.5 L / h, 1.5 L / h, and 0.4 L / h, respectively, to start a coprecipitation reaction. During the reaction, the rotation speed was controlled at 300 r / min, the temperature of the reactor was stably controlled at 50°C, and the pH of the reaction system was controlled to be 11 during the reaction. As the coprecipitation reaction proceeded, when the particle size D50 of the sample in the reactor reached 4.5 μm, the feeding was stopped, and the reaction was continued until the material reaction was complete. The precursor was then post-treated by washing and drying to obtain a high-nickel and cobalt-free positive electrode precursor material.

[0082] [Lithium-ion battery preparation and performance testing]

[0083] The lithium salt lithium hydroxide and the precursors obtained in Examples 1-10 and Comparative Example 1 were respectively mixed and ground in a mortar at a molar ratio of 1.04:1 for 30 minutes. In an oxygen atmosphere, the temperature was raised from room temperature to 750°C at a heating rate of 5°C / min. After calcination and heat preservation at this temperature for 15 hours, the temperature was naturally cooled to room temperature to obtain a high-nickel and cobalt-free positive electrode material.

[0084] The positive electrode materials, conductive carbon black SP (TIMCAL), and polyvinylidene fluoride PVDF (HSV900) provided in Examples 1-10 and Comparative Example 1 were mixed in a mass ratio of 90:5:5, and the solvent was N-methylpyrrolidone. The obtained slurry was evenly coated on the aluminum foil with a scraper with a coating gap of 100μm. After coating, it was first dried by blast at 120℃, then rolled, and finally the dried electrode was cut into Φ12 circular electrode sheets. After vacuum drying at 120℃, the electrode sheet was weighed to obtain a button half-battery positive electrode sheet; the negative electrode selected a Φ14 metal lithium sheet, the diaphragm was a Φ19 PP microporous membrane (Celgard2400), and the electrolyte selected a lithium battery basic electrolyte, that is, EC and DEC were used as a mixed solvent in a volume ratio of 1:1, and 1.1mol / L LiPF6 was added. The positive electrode sheet, metal lithium sheet, diaphragm and electrolyte were assembled to obtain a button battery.

[0085] The lithium ion batteries provided in Examples 1-10 and Comparative Example 1 were subjected to performance tests under constant current charge and discharge mode, a voltage range of 2.5 to 4.5 V, and a temperature of 25°C.

[0086] Discharge capacity test: at 0.1C (1C = 180mAg -1 ) to 4.3V;

[0087] Rate performance test: Charge and discharge cycle tests were conducted at 0.1C, 0.2C, 0.5C, 1C, 2C and 5C respectively. After 5 cycles at each rate, the battery returned to 0.1C and the capacity retention rate was calculated based on the capacity loss to compare the rate performance.

[0088] Cycle performance test: Charge and discharge tests were performed at 1C, and data statistics were collected on the material capacity after 100 cycles to obtain the cycle capacity retention rate.

[0089] The test results are shown in Table 1.

[0090] Table 1

[0091]

[0092]

[0093] From Table 1, we can get:

[0094] From the data results of Examples 1-6, it can be seen that the preparation method provided by the present invention is applicable to a variety of high-nickel cobalt-free material systems. The combination of high-nickel cobalt-free materials (nickel and transition metals) within a reasonable range can improve the capacity, rate performance and cycle performance of the materials by using the preparation method provided by the present invention.

[0095] From the data results of Example 1 and Examples 7 and 8, it can be seen that if the mass concentration of the organic amine is too low, the solubility of the organic amine in the salt solution will be reduced, resulting in incomplete precipitation of salt ions and reduced yield. If the mass concentration of the organic amine is too high, the salt ion concentration will be too low, resulting in less precipitation and a corresponding decrease in yield.

[0096] From the data results of Example 1 and Examples 9 and 10, it can be seen that during the coprecipitation reaction, if the reaction temperature is too low, the ion activity in the solution is low, which will cause incomplete precipitation reaction and affect the yield; if the temperature is too high, the volatility of organic amines in the solution increases, resulting in excessive salt ions that cannot be completely precipitated, which will also lead to a decrease in yield.

[0097] From the data results of Example 1 and Comparative Example 1, it can be seen that the present invention uses specific organic amines as precipitants, and the problems of uneven metal ion precipitation and difficult pH control can be solved without the addition of complexing agents; while the high-nickel cobalt-free positive electrode precursor material prepared by the conventional co-precipitation method will have the problems of easy agglomeration and uneven particle size distribution, and when applied to the positive electrode, its initial discharge specific capacity, cycle performance and rate performance are all lower than those of the precursor material using organic amines as precipitants.

[0098] In summary, the preparation method provided by the present invention uses organic amine as a precipitant and can stably provide OH - , avoiding the situation that the pH is difficult to control and the sedimentation is uneven. The positive electrode material prepared from the high-nickel cobalt-free precursor material thus obtained has a more complete structure, a lower degree of cation mixing (lithium-nickel mixing), excellent cycle performance and rate performance, and a higher capacity. In addition, the preparation method provided by the present invention also has the advantages of simple operation, few control process parameters, low requirements for reaction equipment, and low preparation cost, and is suitable for large-scale production.

[0099] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a high-nickel cobalt-free positive electrode precursor material, characterized in that: The preparation method comprises the following steps: The reaction raw materials include a high-nickel cobalt-free mixed salt solution and a precipitant solution. Under a protective atmosphere, the reaction raw materials are mixed to perform a coprecipitation reaction to obtain the high-nickel cobalt-free positive electrode precursor material; Wherein, the precipitant solution includes an organic amine solution.

2. The preparation method according to claim 1, characterized in that: The high-nickel cobalt-free mixed salt solution includes, in addition to nickel, non-cobalt transition metal elements; Preferably, the non-cobalt transition metal element includes any one of manganese, magnesium or aluminum, or a combination of at least two of them.

3. The preparation method according to claim 1 or 2, characterized in that: The concentration of the high-nickel cobalt-free mixed salt solution is 80-120 g / L; Preferably, the mass concentration of the organic amine solution is 30-60%; Preferably, the organic amine includes any one of di-n-butylamine, isobutanolamine, 3-hydroxypropylamine, dimethylethanolamine or N,N-diethylethanolamine, or a combination of at least two thereof.

4. The preparation method according to any one of claims 1 to 3, characterized in that The feed rate of the high-nickel cobalt-free mixed salt solution is 8 to 10 L / h; Preferably, the feed rate of the precipitant solution is 0.5 to 1.5 L / h.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The reaction raw materials also include a doping salt solution; Preferably, the doping salt solution comprises a zirconium salt solution; Preferably, the concentration of the doped salt solution is 1 to 10 g / L; Preferably, the feed rate of the doping salt solution is 0.3-0.5 L / h.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The reaction speed of the coprecipitation reaction is 100-500 r / min; Preferably, the temperature of the coprecipitation reaction is 75-85°C; Preferably, the pH of the coprecipitation reaction is 10-12.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: A high-nickel cobalt-free mixed salt solution with a concentration of 80 to 120 g / L is mixed at a feeding rate of 8 to 10 L / h, an organic amine solution with a mass concentration of 30 to 60% is mixed at a feeding rate of 0.5 to 1.5 L / h, and a zirconium salt solution with a concentration of 1 to 10 g / L is mixed at a feeding rate of 0.3 to 0.5 L / h. In an environment with a pH of 10 to 12, a coprecipitation reaction is carried out at a reaction speed of 100 to 500 r / min at 75 to 85° C. to obtain the high-nickel cobalt-free positive electrode precursor material.

8. A high-nickel cobalt-free positive electrode precursor material, characterized in that: The high-nickel cobalt-free positive electrode precursor material is prepared by the preparation method according to any one of claims 1 to 7.

9. A high-nickel cobalt-free positive electrode material, characterized in that: The high-nickel cobalt-free positive electrode material is obtained by mixing and sintering the high-nickel cobalt-free positive electrode precursor material as claimed in claim 8 with a lithium source.

10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the high-nickel cobalt-free positive electrode material as claimed in claim 9.

Citation Information

Patent Citations

  • Lithium ion battery positive plate using cobalt-free high-nickel positive electrode material

    CN112382734A