Artificial SEI (solid electrolyte interface) membrane as well as preparation method and application thereof
By using ternary hybrid SEI films prepared with materials such as Li2O, Li3N, LiF or Li2CO3, the conductivity and stability of existing SEI films are solved, the cycle stability and safety of lithium-ion batteries are improved, and the battery life is extended.
Patent Information
- Application Number
- CN202411151891.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
AI Technical Summary
The ionic conductivity, electrochemical stability and mechanical properties of the existing SEI films affect the cycle stability and safety of lithium-ion batteries.
Artificial SEI films are prepared using Li2O, Li3N, LiF or Li2CO3 and other materials. A ternary hybrid film is formed through two-stage pre-melting process and co-evaporation method to improve conductivity, electrochemical stability and mechanical properties, and enhance the toughness and high temperature and high pressure of the film. stability.
It achieves high capacity retention and rate performance, improves the transmission efficiency of Li ions and the stability of the membrane, extends the battery life and improves safety.
Smart Images

Figure CN119050358A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to an artificial SEI film and a preparation method and application thereof. Background Art
[0002] SEI (Solid Electrolyte Interphase) is a solid electrolyte film formed on the surface of the negative electrode during the battery cycle. The formed SEI film has a certain barrier to the ions and electrons in the electrolyte, which can limit the further decomposition of the electrolyte, while allowing the reversible insertion / deinsertion of lithium ions. This barrier protects the metallic lithium and electrolyte inside the battery from further reaction and corrosion. The formation of SEI largely determines the cycle stability and safety of the battery. A stable and tight SEI can reduce the release of electrolyte decomposition products, thereby slowing down the capacity decay of the battery and increasing the cycle life of the battery. However, the naturally formed SEI film usually has a thick and uneven structure, which is unstable, fragile, and has low ionic conductivity.
[0003] At present, the following methods are usually used to solve the problems existing in SEI film:
[0004] 1. Optimizing the electrolyte formula and selecting appropriate electrolytes and additives can reduce the instability and electrochemical activity of the SEI film. For example, adding salts or compounds with higher stability, such as phosphates and thioether compounds, can improve the formation and stability of the SEI film.
[0005] 2. Surface modification: Modifying the surface of the motor, for example, forming a stable coating on the electrode surface or using nanostructure design can improve the mechanical stability and electrochemical stability of the SEI film.
[0006] However, there are still some problems with the above methods. Optimizing the electrolyte formula may usually cause complex chemical reactions, resulting in dynamic changes in the composition and structure of the SEI film. These changes may affect the stability of the SEI film, thereby affecting the cycle stability and safety of the battery. At the same time, the formation of the SEI film will lead to lithium loss, reducing the initial coulombic efficiency. The cycle stability of the motor can be improved by constructing a modified layer on the surface of the motor (for example: Al2O3, SiO2, LiF, Li2CO3, Li3N, Li2S, etc.), but traditional single-layer modified materials cannot take into account electrochemical stability, rate performance, etc. at the same time. A good SEI film needs to have high electrochemical stability, high temperature stability, high ion transport, good toughness and density, so that the SEI film does not decompose at high voltage and high temperature. At the same time, high ion transport enables the battery to have high rate characteristics, and good toughness and density can inhibit the piercing of lithium dendrites and improve the life and safety of the battery. Summary of the invention
[0007] Based on the fact that the currently prepared SEI membranes have the problems of poor ionic conductivity, electrochemical stability and mechanical properties, the purpose of the present invention is to provide an artificial SEI membrane and a preparation method and application thereof. The artificial SEI membrane takes into account electrical conductivity, electrochemical stability and mechanical properties, and solves the problems of low ionic conductivity, electrochemical stability and mechanical properties of the SEI membrane. By establishing a structure-activity relationship, the prepared SEI membrane has multiple functions, and the battery prepared using the SEI membrane has a longer service life and higher safety.
[0008] The present invention is achieved through the following technical solutions:
[0009] In a first aspect, the present application provides an artificial SEI film, whose raw material components include Li2O and Li3N, and also include LiF or Li2CO3; wherein the mass ratio of Li2O, Li3N and LiF or Li2CO3 is (0.4-1.2):(0.4-1.2):1.
[0010] Among them, LiF has low formation energy and wide band gap, which can improve the stability of SEI film; Li2O has a very low Poisson's ratio, which can improve the toughness of SEI film; Li3N has a very low Li migration energy barrier, which can improve the conductivity of Li ions; Li2CO3 has low formation energy and wide band gap, as well as a lower Li migration energy barrier, which can improve the stability of SEI film.
[0011] The SEI film prepared using the raw material composition and dosage of the present application has a high capacity retention rate and rate performance, taking into account electrical conductivity, electrochemical stability and mechanical properties, and has higher Li ion conductivity. It can guide Li to deposit quickly, and improve the stability of the SEI film, so that it can withstand higher voltages and temperatures. In addition, the toughness of the SEI film is also improved, so that it can withstand the pressure of Li dendrites without being easily broken. In addition, when the ternary material constitutes a mixed artificial SEI film, due to the characteristics of its multi-component components, a large number of grain boundaries will naturally form at the junction of different materials. These grain boundaries provide a wider space than the interior of the crystal, thereby significantly promoting the transmission efficiency of Li ions. Specifically, the existence of grain boundaries opens up a smoother path for the migration of Li ions, making the transmission of Li in the ternary mixed artificial SEI film more efficient than that inside a single material.
[0012] In a second aspect, the present application provides a method for preparing an artificial SEI film, comprising the following steps:
[0013] Weigh Li2O, Li3N and LiF or Li2CO3 according to the mass ratio, mix them evenly to obtain a raw material mixture for later use;
[0014] Pre-melting the raw material mixture in a vacuum environment to obtain a melted material;
[0015] The molten material is deposited on a lithium substrate to form a SEI film, which is then cooled and solidified to firmly bond the SEI film to the lithium substrate.
[0016] When evaporating the SEI film, a co-evaporation method or a discrete mask coating method is used for preparation, and the evaporation is performed in an oxygen-free or extremely low-oxygen environment.
[0017] Before depositing the SEI film on the lithium substrate, the surface of the lithium substrate is cleaned, preheated, and other treatments are performed to ensure adhesion and uniformity of evaporation.
[0018] Furthermore, when the raw material is pre-melted, the pressure in the vacuum environment is controlled at 10 -4 Pa~10 -5 Pa.
[0019] Furthermore, when pre-melting the raw materials, a two-stage pre-melting process is adopted.
[0020] Among them, the two-stage pre-melting process is:
[0021] The first stage of pre-melting: the preset temperature is about 150-500℃, and the duration is about 10-120 minutes. This stage allows the impurities and gases in the solid to be discharged and the temperature gradient to be reduced. The second stage of pre-melting: the temperature is raised to above the melting point, the temperature range is 200-1000℃, and the duration is about 10-120 minutes.
[0022] Furthermore, the evaporation rate when the raw material is pre-melted is
[0023] Furthermore, when depositing the SEI film, the heating power was kept constant at 300W.
[0024] Furthermore, the preparation method of the lithium substrate comprises the following steps:
[0025] Producing a smooth lithium surface by vaporizing lithium;
[0026] The vaporized lithium is placed in a crucible and heated to pre-melt;
[0027] The pre-melted lithium is deposited to obtain a lithium substrate.
[0028] Furthermore, the diameter of the lithium foil to be heated and pre-melted is 12 mm to 16 mm, and the thickness is 350 μm to 450 μm.
[0029] In a third aspect, the present application provides a lithium electrode, on the surface of which the artificial SEI film described above or the artificial SEI film prepared by the above preparation method is provided.
[0030] In a fourth aspect, the present application provides a lithium battery, comprising a lithium electrode, wherein the surface of the lithium electrode is provided with the above-mentioned artificial SEI film or the artificial SEI film prepared by the above-mentioned preparation method.
[0031] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0032] (1) The SEI film prepared by the raw material composition and dosage specified in the present invention has a high capacity retention rate and rate performance, takes into account the electrical conductivity, electrochemical stability and mechanical properties, has higher Li ion conductivity, can guide Li to deposit rapidly, and improves the stability of the SEI film, so that it can withstand higher voltages and temperatures. In addition, the toughness of the SEI film is also improved, so that it can withstand the pressure of Li dendrites without being easily broken.
[0033] (2) When the ternary material of the present invention forms a mixed artificial SEI film, due to the characteristics of its multi-component components, a large number of grain boundaries will naturally form at the junction of different materials. These grain boundaries provide a wider space than the interior of the crystal, thereby significantly promoting the transmission efficiency of Li ions. Specifically, the existence of grain boundaries opens up a smoother path for the migration of Li ions, making the transmission of Li in the ternary mixed artificial SEI film more efficient than that in a single material. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings:
[0035] Figure 1 The ohmic internal resistance of the embodiment of the present invention and the comparative example.
[0036] Figure 2 1 and 2 are the interface impedances of the embodiment of the present invention and the comparative example. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.
[0038] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Example 1
[0040] This embodiment provides a method for preparing an electrode with a ternary hybrid multifunctional artificial SEI film, which is carried out according to the following steps:
[0041] S1. Preparation of lithium matrix: Producing a smooth lithium surface by vaporizing lithium.
[0042] S2. Fix the lithium foil (15.6 mm in diameter and 450 μm in thickness) 30 cm above the crucible and place it in a mold of a circular custom groove.
[0043] S3, in vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0044] S4. Depositing the pre-melted lithium metal to obtain a lithium substrate, wherein the heating power is 300 W (constant power).
[0045] S6. Weigh LiF, Li2O, and Li3N in a mass ratio of 1:1:1, and mix them evenly to obtain a raw material mixture;
[0046] S7, the raw material mixture is placed in a vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0047] S8. Depositing the pre-melted ternary mixture on a lithium substrate to form a SEI film.
[0048] S9. After the SEI film is formed, it is cooled and solidified so that the evaporated SEI material is firmly bonded to the substrate.
[0049] The properties of the raw materials used in this example are shown in Table 1 below.
[0050] Table 1
[0051] nature LiF <![CDATA[Li2O]]> <![CDATA[Li3N]]> Bandgap(eV) 8.72 4.90 0.98 Formation energy (eV / atom) -3.19 -2.06 -0.483 Li migration barrier (eV) 0.17 0.32 0.13 Poisson's ratio 0.20 0.16 0.23
[0052] The electrode prepared by the method of this embodiment was assembled into a button battery, and its capacity retention rate and impedance were tested. The test results of the capacity retention rate are shown in Table 7 below, which is 85.89%. The test results of the ohmic internal resistance and the interface impedance are shown in Table 7 below. Figure 1 , Figure 2 As shown in Table 8. From the test results, the SEI film prepared by the method of this embodiment has high capacity retention and rate performance, takes into account conductivity, electrochemical stability and mechanical properties, has higher Li ion conductivity, can guide Li to deposit quickly, and improves the stability of the SEI film, so that it can withstand higher voltage and temperature, in addition, it also improves the toughness of the SEI film, so that it can withstand the pressure of Li dendrites without being easily broken.
[0053] Example 2
[0054] This embodiment provides a method for preparing an electrode with a ternary mixed multifunctional artificial SEI film. The difference from Embodiment 1 is that the raw material components in this embodiment are LiF, Li2O, and Li2CO3. The specific preparation method is as follows:
[0055] S1. Preparation of lithium matrix: Producing a smooth lithium surface by vaporizing lithium.
[0056] S2. Fix the lithium foil (15.6 mm in diameter and 450 μm in thickness) 30 cm above the crucible and place it in a mold of a circular custom groove.
[0057] S3, in vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0058] S4. Depositing the pre-melted lithium metal to obtain a lithium substrate, wherein the heating power is 300 W (constant power).
[0059] S6. Weigh LiF, Li2O, and Li2CO3 in a mass ratio of 1:1:1, and mix them evenly to obtain a raw material mixture;
[0060] S7, the raw material mixture is placed in a vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0061] S8. Depositing the pre-melted ternary mixture on a lithium substrate to form a SEI film.
[0062] S9. After the SEI film is formed, it is cooled and solidified so that the evaporated SEI material is firmly bonded to the substrate.
[0063] The properties of the raw materials used in this example are shown in Table 2 below.
[0064] Table 2
[0065] nature LiF <![CDATA[Li2O]]> <![CDATA[Li2CO3]]> Bandgap(eV) 8.72 4.90 5.06 Formation energy (eV / atom) -3.19 -2.06 -2.24 Li migration barrier (eV) 0.17 0.32 0.23 Poisson's ratio 0.20 0.16 0.28
[0066] The electrode prepared by the method of this embodiment was assembled into a button battery, and its capacity retention rate and impedance were tested. The test results of the capacity retention rate are shown in Table 7 below, which is 85.81%. The test results of the ohmic internal resistance and the interface impedance are shown in Table 7 below. Figure 1 , Figure 2 As shown in Table 8. From the test results, the SEI film prepared by the method of this embodiment has high capacity retention and rate performance, takes into account conductivity, electrochemical stability and mechanical properties, has higher Li ion conductivity, can guide Li to deposit quickly, and improves the stability of the SEI film, so that it can withstand higher voltage and temperature, in addition, it also improves the toughness of the SEI film, so that it can withstand the pressure of Li dendrites without being easily broken.
[0067] Example 3
[0068] This embodiment provides a method for preparing an electrode with a ternary mixed multifunctional artificial SEI film, which is different from Embodiment 1 in that the mass ratio of the raw material components LiF, Li2O, and Li3N in this embodiment is 0.8:0.8:1. Other technical features are the same as those in Embodiment 1.
[0069] The specific preparation method is as follows:
[0070] S1. Preparation of lithium matrix: Producing a smooth lithium surface by vaporizing lithium.
[0071] S2. Fix the lithium foil (15.6 mm in diameter and 450 μm in thickness) 30 cm above the crucible and place it in a mold of a circular custom groove.
[0072] S3, in vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0073] S4. Depositing the pre-melted lithium metal to obtain a lithium substrate, wherein the heating power is 300 W (constant power).
[0074] S6. Weigh LiF, Li2O, and Li3N in a mass ratio of 0.8:0.8:1, and mix them evenly to obtain a raw material mixture;
[0075] S7, the raw material mixture is placed in a vacuum environment (10-5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0076] S8. Depositing the pre-melted ternary mixture on a lithium substrate to form a SEI film.
[0077] S9. After the SEI film is formed, it is cooled and solidified so that the evaporated SEI material is firmly bonded to the substrate.
[0078] The properties of the raw materials used in this example are shown in Table 3 below.
[0079] Table 3
[0080] nature LiF <![CDATA[Li2O]]> <![CDATA[Li3N]]> Bandgap(eV) 8.72 4.90 0.98 Formation energy (eV / atom) -3.19 -2.06 -0.483 Li migration barrier (eV) 0.17 0.32 0.13 Poisson's ratio 0.20 0.16 0.23
[0081] The electrode prepared by the method of this embodiment was assembled into a button battery, and its capacity retention rate and impedance were tested. The test results of the capacity retention rate are shown in Table 7 below, which is 86.23%. The test results of the ohmic internal resistance and the interface impedance are shown in Table 7 below. Figure 1 , Figure 2 As shown in Table 8. From the test results, the SEI film prepared by the method of this embodiment has high capacity retention and rate performance, takes into account conductivity, electrochemical stability and mechanical properties, has higher Li ion conductivity, can guide Li to deposit quickly, and improves the stability of the SEI film, so that it can withstand higher voltage and temperature, in addition, it also improves the toughness of the SEI film, so that it can withstand the pressure of Li dendrites without being easily broken.
[0082] Example 4
[0083] This embodiment is a method for preparing an electrode with a ternary mixed multifunctional artificial SEI film. The difference from Embodiment 2 is that the mass ratio of the raw material components LiF, Li2O, and Li2CO3 in this embodiment is 0.8:0.8:1. Other technical features are the same as those in Embodiment 2.
[0084] The specific preparation method is as follows:
[0085] S1. Preparation of lithium matrix: Producing a smooth lithium surface by vaporizing lithium.
[0086] S2. Fix the lithium foil (15.6 mm in diameter and 450 μm in thickness) 30 cm above the crucible and place it in a mold of a circular custom groove.
[0087] S3, in vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0088] S4. Depositing the pre-melted lithium metal to obtain a lithium substrate, wherein the heating power is 300 W (constant power).
[0089] S6. Weigh LiF, Li2O, and Li2CO3 in a mass ratio of 0.8:0.8:1, and mix them evenly to obtain a raw material mixture;
[0090] S7, the raw material mixture is placed in a vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0091] S8. Depositing the pre-melted ternary mixture on a lithium substrate to form a SEI film.
[0092] S9. After the SEI film is formed, it is cooled and solidified so that the evaporated SEI material is firmly bonded to the substrate.
[0093] The properties of the raw materials used in this example are shown in Table 4 below.
[0094] Table 4
[0095] nature LiF <![CDATA[Li2O]]> <![CDATA[Li2CO3]]> Bandgap(eV) 8.72 4.90 5.06 Formation energy (eV / atom) -3.19 -2.06 -2.24 Li migration barrier (eV) 0.17 0.32 0.23 Poisson's ratio 0.20 0.16 0.28
[0096] The electrode prepared by the method of this embodiment was assembled into a button battery, and its capacity retention rate and impedance were tested. The test results of the capacity retention rate are shown in Table 7 below, which is 84.97%. The test results of the ohmic internal resistance and the interface impedance are shown in Table 7 below. Figure 1 , Figure 2 As shown in Table 8. From the test results, the SEI film prepared by the method of this embodiment has high capacity retention and rate performance, takes into account conductivity, electrochemical stability and mechanical properties, has higher Li ion conductivity, can guide Li to deposit quickly, and improves the stability of the SEI film, so that it can withstand higher voltage and temperature, in addition, it also improves the toughness of the SEI film, so that it can withstand the pressure of Li dendrites without being easily broken.
[0097] Example 5
[0098] This embodiment provides a method for preparing an electrode with a ternary mixed multifunctional artificial SEI film, which is different from Embodiment 1 in that the mass ratio of the raw material components LiF, Li2O, and Li3N in this embodiment is 0.6:0.6:1. Other technical features are the same as those in Embodiment 1.
[0099] The specific preparation method is as follows:
[0100] S1. Preparation of lithium matrix: Producing a smooth lithium surface by vaporizing lithium.
[0101] S2. Fix the lithium foil (15.6 mm in diameter and 450 μm in thickness) 30 cm above the crucible and place it in a mold of a circular custom groove.
[0102] S3, in vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0103] S4. Depositing the pre-melted lithium metal to obtain a lithium substrate, wherein the heating power is 300 W (constant power).
[0104] S6. Weigh LiF, Li2O, and Li3N in a mass ratio of 0.6:0.6:1, and mix them evenly to obtain a raw material mixture;
[0105] S7, the raw material mixture is placed in a vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0106] S8. Depositing the pre-melted ternary mixture on a lithium substrate to form a SEI film.
[0107] S9. After the SEI film is formed, it is cooled and solidified so that the evaporated SEI material is firmly bonded to the substrate.
[0108] The properties of the raw materials used in this example are shown in Table 5 below.
[0109] Table 5
[0110] nature LiF <![CDATA[Li2O]]> <![CDATA[Li3N]]> Bandgap(eV) 8.72 4.90 0.98 Formation energy (eV / atom) -3.19 -2.06 -0.483 Li migration barrier (eV) 0.17 0.32 0.13 Poisson's ratio 0.20 0.16 0.23
[0111] The electrode prepared by the method of this embodiment was assembled into a button battery, and its capacity retention rate and impedance were tested. The test results of the capacity retention rate are shown in Table 7 below, which is 85.91%. The test results of the ohmic internal resistance and the interface impedance are shown in Table 7 below. Figure 1 , Figure 2 As shown in Table 8. From the test results, the SEI film prepared by the method of this embodiment has high capacity retention and rate performance, takes into account conductivity, electrochemical stability and mechanical properties, has higher Li ion conductivity, can guide Li to deposit quickly, and improves the stability of the SEI film, so that it can withstand higher voltage and temperature, in addition, it also improves the toughness of the SEI film, so that it can withstand the pressure of Li dendrites without being easily broken.
[0112] Example 6
[0113] This embodiment provides a method for preparing an electrode with a ternary mixed multifunctional artificial SEI film, which is different from Embodiment 2 in that the mass ratio of the raw material components LiF, Li2O, and Li2CO3 in this embodiment is 0.6:0.6:1. Other technical features are the same as those in Embodiment 2.
[0114] The specific preparation method is as follows:
[0115] S1. Preparation of lithium matrix: Producing a smooth lithium surface by vaporizing lithium.
[0116] S2. Fix the lithium foil (15.6 mm in diameter and 450 μm in thickness) 30 cm above the crucible and place it in a mold of a circular custom groove.
[0117] S3, in vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0118] S4. Depositing the pre-melted lithium metal to obtain a lithium substrate, wherein the heating power is 300 W (constant power).
[0119] S6. Weigh LiF, Li2O, and Li2CO3 in a mass ratio of 0.6:0.6:1, and mix them evenly to obtain a raw material mixture;
[0120] S7, the raw material mixture is placed in a vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0121] S8. Depositing the pre-melted ternary mixture on a lithium substrate to form a SEI film.
[0122] S9. After the SEI film is formed, it is cooled and solidified so that the evaporated SEI material is firmly bonded to the substrate.
[0123] Among them, the properties of the raw materials used in this embodiment are shown in Table 6.
[0124] Table 6
[0125] nature LiF <![CDATA[Li2O]]> <![CDATA[Li2CO3]]> Bandgap(eV) 8.72 4.90 5.06 Formation energy (eV / atom) -3.19 -2.06 -2.24 Li migration barrier (eV) 0.17 0.32 0.23 Poisson's ratio 0.20 0.16 0.28
[0126] The electrode prepared by the method of this embodiment was assembled into a button battery, and its capacity retention rate and impedance were tested. The test results of the capacity retention rate are shown in Table 7 below, which is 85.84%. The test results of the ohmic internal resistance and the interface impedance are shown in Table 7 below. Figure 1 , Figure 2 As shown in Table 8. From the test results, the SEI film prepared by the method of this embodiment has high capacity retention and rate performance, takes into account conductivity, electrochemical stability and mechanical properties, has higher Li ion conductivity, can guide Li to deposit quickly, and improves the stability of the SEI film, so that it can withstand higher voltage and temperature, in addition, it also improves the toughness of the SEI film, so that it can withstand the pressure of Li dendrites without being easily broken.
[0127] Comparative Example 1
[0128] This comparative example provides a method for preparing a lithium electrode. The difference from Example 1 is that the SEI film is not evaporated in this comparative example, and the SEI film is naturally generated.
[0129] The specific preparation method is as follows:
[0130] S1. Preparation of lithium matrix: Producing a smooth lithium surface by vaporizing lithium.
[0131] S2. Fix the lithium foil (15.6 mm in diameter and 450 μm in thickness) 30 cm above the crucible and place it in a mold of a circular custom groove.
[0132] S3, in vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0133] S4, depositing the pre-melted lithium metal to obtain a lithium substrate, wherein the heating power is 300 W (constant power). During assembly, a SEI film is formed naturally.
[0134] The electrode prepared by the method of this comparative example was assembled into a button battery, and its capacity retention rate and impedance were tested. The test results of the capacity retention rate are shown in Table 7 below, which is 75.29%. The test results of the ohmic internal resistance and the interface impedance are shown in Table 7 below. Figure 1 , Figure 2 and Table 8. From the data in Table 7 and Table 8 and Figure 1 , Figure 2 It can be seen from the curve that the capacity retention rate and rate performance, conductivity, electrochemical stability and mechanical properties of the comparative example are lower than those of the electrode prepared by the methods of Examples 1 to 6. The comparison proves that the electrode prepared by the composition, dosage and preparation method of the present application has better performance.
[0135] Comparative Example 2
[0136] This comparative example provides a method for preparing an electrode with a ternary mixed multifunctional artificial SEI film, which is different from Example 1 in that the mass ratio of the raw material components LiF, Li2O, and Li3N in this example is 0.1:0.1:1. Other technical features are the same as those in Example 1.
[0137] The specific preparation method is as follows:
[0138] S1. Preparation of lithium matrix: Producing a smooth lithium surface by vaporizing lithium.
[0139] S2. Fix the lithium foil (15.6 mm in diameter and 450 μm in thickness) 30 cm above the crucible and place it in a mold of a circular custom groove.
[0140] S3, in vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0141] S4. Depositing the pre-melted lithium metal to obtain a lithium substrate, wherein the heating power is 300 W (constant power).
[0142] S6. Weigh LiF, Li2O, and Li3N in a mass ratio of 0.1:0.1:1, and mix them evenly to obtain a raw material mixture;
[0143] S7, the raw material mixture is placed in a vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0144] S8. Depositing the pre-melted ternary mixture on a lithium substrate to form a SEI film.
[0145] S9. After the SEI film is formed, it is cooled and solidified so that the evaporated SEI material is firmly bonded to the substrate.
[0146] The raw materials used in this comparative example are shown in Table 1.
[0147] The electrode prepared by the method of this comparative example was assembled into a button battery, and its capacity retention rate and impedance were tested. The test results of the capacity retention rate are shown in Table 7 below, which is 76.97%. The test results of the ohmic internal resistance and the interface impedance are shown in Table 7 below. Figure 1 , Figure 2 and Table 8. From the data in Table 7 and Table 8 and Figure 1 , Figure 2It can be seen from the curve that the capacity retention rate and rate performance, conductivity, electrochemical stability and mechanical properties of the comparative example are lower than those of the electrode prepared by the methods of Examples 1 to 6. The comparison proves that the electrode prepared by the composition, dosage and preparation method of the present application has better performance.
[0148] Comparative Example 3
[0149] This comparative example provides a method for preparing an electrode with a ternary mixed multifunctional artificial SEI film, which is different from Example 2 in that the mass ratio of the raw material components LiF, Li2O, and Li2CO3 in this example is 0.1:0.1:1. Other technical features are the same as those in Example 2.
[0150] The specific preparation method is as follows:
[0151] S1. Preparation of lithium matrix: Producing a smooth lithium surface by vaporizing lithium.
[0152] S2. Fix the lithium foil (15.6 mm in diameter and 450 μm in thickness) 30 cm above the crucible and place it in a mold of a circular custom groove.
[0153] S3, in vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0154] S4. Depositing the pre-melted lithium metal to obtain a lithium substrate, wherein the heating power is 300 W (constant power).
[0155] S6. Weigh LiF, Li2O, and Li2CO3 in a mass ratio of 0.1:0.1:1, and mix them evenly to obtain a raw material mixture;
[0156] S7, the raw material mixture is placed in a vacuum environment (10 -5 Pa) for pre-melting, the heating power of the crucible is 200W, a two-stage pre-melting process is used, and the evaporation rate is
[0157] S8. Depositing the pre-melted ternary mixture on a lithium substrate to form a SEI film.
[0158] S9. After the SEI film is formed, it is cooled and solidified so that the evaporated SEI material is firmly bonded to the substrate.
[0159] The properties of the raw materials used in this comparative example are shown in Table 2.
[0160] The electrode prepared by the method of this comparative example was assembled into a button battery, and its capacity retention rate and impedance were tested. The test results of the capacity retention rate are shown in Table 7 below, which is 75.31%. The test results of the ohmic internal resistance and the interface impedance are shown in Table 7 below. Figure 1 , Figure 2 and Table 8. From the data in Table 7 and Table 8 and Figure 1 , Figure 2 It can be seen from the curve that the capacity retention rate and rate performance, conductivity, electrochemical stability and mechanical properties of the comparative example are lower than those of the electrode prepared by the methods of Examples 1 to 6. The comparison proves that the electrode prepared by the composition, dosage and preparation method of the present application has better performance.
[0161] Table 7
[0162]
[0163]
[0164] Table 8
[0165]
[0166] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. An artificial SEI film, It is characterized in that Its raw material components include Li 2 O and Li 3 N, also includes LiF or Li 2 CO 3 ; Among them, Li 2 O. Li 3 N and LiF or Li 2 CO 3 The mass ratio is (0.4~1.2):(0.4~1.2):
1.
2. A method for preparing the artificial SEI film according to claim 1, It is characterized in that The following steps are involved: Weigh Li according to mass ratio 2 O. Li 3 N and LiF or Li 2 CO 3 , mix evenly to obtain a raw material mixture for standby use; Pre-melting the raw material mixture in a vacuum environment to obtain a melted material; The molten material is deposited on a lithium substrate to form a SEI film, which is then cooled and solidified to firmly bond the SEI film to the lithium substrate.
3. The method for preparing an artificial SEI film according to claim 2, It is characterized in that When pre-melting the raw materials, the pressure in the vacuum environment is controlled at 10 -4 Pa~10 -5 Pa.
4. The method for preparing an artificial SEI film according to claim 2, It is characterized in that When pre-melting the raw materials, a two-stage pre-melting process is adopted.
5. The method for preparing an artificial SEI film according to claim 2, It is characterized in that The evaporation rate when pre-melting the raw material is 6. The method for preparing an artificial SEI film according to claim 2, It is characterized in that When depositing the SEI film, the heating power was kept constant at 300W.
7. The method for preparing an artificial SEI film according to claim 2, It is characterized in that The preparation method of the lithium substrate comprises the following steps: Producing a smooth lithium surface by vaporizing lithium; The vaporized lithium is placed in a crucible and heated to pre-melt; The pre-melted lithium is deposited to obtain a lithium substrate.
8. The method for preparing an artificial SEI film according to claim 7, It is characterized in that The lithium foil to be heated and pre-melted has a diameter of 12 mm to 16 mm and a thickness of 350 μm to 450 μm.
9. A lithium electrode, It is characterized in that The surface of the lithium electrode is provided with the artificial SEI film according to claim 1 or the artificial SEI film prepared by the preparation method according to any one of claims 2 to 8.
10. A lithium battery, It is characterized in that It comprises a lithium electrode, on the surface of which the artificial SEI film according to claim 1 or the artificial SEI film prepared by the preparation method according to any one of claims 2 to 8 is arranged.
Citation Information
Cited By
Lithium ion battery
CN119560637A
A lithium-ion battery
CN119560637B
Non-aqueous electrolyte and lithium ion battery
CN119581671A
Lithium negative electrode with multi-layer composite artificial SEI (solid electrolyte interface) film as well as preparation method and application of lithium negative electrode
CN119673947A
Lithium anode with multilayer composite artificial SEI film, its preparation method and application
CN119673947B