Gypsum-based polymer waterproof mortar
Through heat treatment and modification of gypsum-based polymer waterproof mortar, the problem of decreased waterproof performance of polymer cement waterproof mortar under low temperature conditions was solved, and a new cementitious material with excellent waterproof effect and high impermeability pressure was prepared.
Patent Information
- Application Number
- CN202410715931.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polymer cement waterproof mortar ages under long-term low temperature conditions, resulting in a decrease in waterproofing performance.
Gypsum-based polymer waterproof mortar is used, and soluble phosphorus and organic matter are removed through heat treatment and dehydration (calcination at 820°C for 0 to 2 hours), and modified phosphogypsum, slag and other materials are used to prepare a new waterproof mortar with hydraulic cementitious materials.
It improves the performance stability and waterproofing effect of waterproof mortar, and the anti-seepage pressure reaches 2.8MPa, exceeding the industry standard and broadening the application fields of phosphogypsum.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterproof mortar, and more particularly to a gypsum-based polymer waterproof mortar. Background Art
[0002] Waterproof mortar has good weather resistance, durability, impermeability, compactness, high adhesion and strong waterproof and anti-corrosion effect. It can resist corrosion from soda ash production medium, urea, ammonium nitrate, seawater hydrochloric acid and acidic and alkaline salts. It is mixed with sand, ordinary cement and special cement to form cement mortar. By casting or spraying the mixed cement mortar or applying it manually, a solid waterproof and anti-corrosion mortar layer is formed on the concrete and surface. It is a rigid and tough waterproof and anti-corrosion material. Mixing with cement and sand can modify the mortar and can be used for the treatment of building walls and floors and the waterproof layer of underground projects. There are three types of waterproof mortars used as waterproof layers in waterproof projects: (1) waterproof mortar mixed with waterproofing agent, (2) rigid multi-layer cement mortar, and (3) polymer cement waterproof mortar.
[0003] Among them, polymer cement waterproof mortar is a mortar prepared with cement, polymer dispersion as cementing material and sand. After the polymer cement mortar hardens, the polymer in the mortar can effectively close the connected pores, increase the density and crack resistance of the mortar, and thus improve the impermeability and impact resistance of the mortar. Polymer dispersion is a liquid material in which a certain amount of polymer latex (such as synthetic rubber, synthetic resin, natural rubber, etc.) and auxiliary additives (such as emulsifiers, stabilizers, defoamers, curing agents, etc.) are added to water and the polymer particles are evenly dispersed in water after stirring. Commonly used polymer varieties include: silicone, cationic chloroprene latex, ethylene-polyvinyl acetate copolymer emulsion, styrene-butadiene rubber latex, vinyl chloride-vinyl chloride copolymer emulsion, etc.
[0004] However, since polymers are mixed into this mortar, it will age, change, and have poor waterproof performance after being used under low temperature conditions for a long time.
[0005] Therefore, a solution needs to be proposed to solve this problem. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a gypsum-based polymer waterproof mortar, which can remove soluble phosphorus, organic matter and other impurities through heat treatment dehydration, i.e., calcination at a constant temperature of 820°C for 0 to 2 hours, so as to stabilize its performance.
[0007] The above technical purpose of the present invention is achieved through the following technical scheme: a gypsum-based polymer waterproof mortar, comprising the following components in parts by weight: 41.6-60 parts of phosphogypsum, 4.4-6 parts of building gypsum, 30-50 parts of slag, 4 parts of cement, 0.15-0.30 parts of K2SO4, 33-39 parts of water, 150-225 parts of fine sand, 0-5 parts of latex powder, 0-4.5 parts of tung oil or 0-1.5 parts of calcium stearate, 5-10 parts of nano magnesium oxide, 5-10 parts of fly ash, 0.07-0.13 parts of water reducer and 0-0.15 parts of defoamer, wherein the water-cement ratio is 0.33-0.39.
[0008] The present invention is further configured as follows: the modified phosphogypsum is prepared according to the following method: (1) phosphogypsum is mixed with quicklime and aged to obtain an initial material; (2) the initial material is mixed evenly with water, and then the pH value is adjusted to 6-8, filtered and dried to obtain treated phosphogypsum; (3) the treated phosphogypsum is mixed evenly with reaction solution A to form a mixed solution B, wherein the reaction solution A is an ethanol solution of a modifier; (4) the pH value of the mixed solution B is adjusted to 6-8, heated, dried, and ground to obtain modified phosphogypsum.
[0009] The present invention is further configured as follows: the particle size of the fine sand is 0.3-1.18 mm.
[0010] The present invention is further configured as follows: the water reducer is a polycarboxylate water reducer.
[0011] The present invention is further configured as follows: the latex powder is a dispersible latex powder.
[0012] The present invention is further configured as follows: the tung oil is raw tung oil.
[0013] The present invention is further configured as follows: in terms of mass fractions, the quicklime is 5-20 parts relative to 100 parts of the phosphogypsum.
[0014] The present invention is further configured as follows: the mass ratio of the initial material to water is 1:0.3-0.8, and the pH value is adjusted with ammonia water.
[0015] In summary, the present invention has the following beneficial effects:
[0016] The phosphogypsum used in the present invention is dehydrated by heat treatment, i.e., calcined at a constant temperature of 820°C for 0 to 2h, so as to remove impurities such as soluble phosphorus and organic matter, thereby making its performance stable. The present invention aims to develop a new type of cementitious material, which uses calcined phosphogypsum as a base material and adds materials such as metakaolin and slag to produce waterproof mortar with excellent waterproof effect. The phosphogypsum-based waterproof mortar prepared by the present invention uses phosphogypsum and slag as main raw materials and uses alkaline excitation. The cementitious material produced by the present invention has water-hardening property, which breaks the limitation that gypsum can only be used as an air-hardening cementitious material, and provides a wider range of possibilities for future application fields. DETAILED DESCRIPTION
[0017] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with specific embodiments. It should be noted that the embodiments of the present application and the features therein may be combined with each other without conflict.
[0018] In the description of the present invention, it should be noted that the terms "upper", "lower", "inside", "outside", "top / bottom" and the like indicating directions or positional relationships are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.
[0019] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "provided with", "set / connected", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0020] The present invention is described in detail below.
[0021] A gypsum-based polymer waterproof mortar comprises the following components in parts by weight: 41.6-60 parts of phosphogypsum, 4.4-6 parts of building gypsum, 30-50 parts of slag, 4 parts of cement, 0.15-0.30 parts of K2SO4, 33-39 parts of water, 150-225 parts of fine sand, 0-5 parts of latex powder, 0-4.5 parts of tung oil or 0-1.5 parts of calcium stearate, 5-10 parts of nano magnesium oxide, 5-10 parts of fly ash, 0.07-0.13 parts of water reducing agent and 0-0.15 parts of defoaming agent, wherein the water-cement ratio is 0.33-0.39.
[0022] Modified phosphogypsum is prepared according to the following method: (1) phosphogypsum and quicklime are mixed and aged to obtain an initial material; (2) the initial material is mixed evenly with water, and then the pH value is adjusted to 6-8, filtered and dried to obtain treated phosphogypsum; (3) the treated phosphogypsum is mixed evenly with reaction solution A to form a mixed solution B, wherein the reaction solution A is an ethanol solution of a modifier; (4) the pH value of the mixed solution B is adjusted to 6-8, heated, dried, and ground to obtain modified phosphogypsum.
[0023] In terms of mass, the amount of quicklime is 5-20 parts relative to 100 parts of phosphogypsum, the mass ratio of the initial material to water is 1:0.3-0.8, and the pH value is adjusted with ammonia water.
[0024] The particle size of the fine sand is 0.3-1.18 mm, the water reducer is a polycarboxylic acid water reducer, the latex powder is a dispersible latex powder, and the tung oil is raw tung oil.
[0025] The present invention can make full use of phosphogypsum waste, solve the problem of phosphogypsum treatment, and lay a foundation for expanding the application of phosphogypsum.
[0026] Traditional phosphogypsum has the problem of delaying cement hydration in cement-based applications, while the phosphogypsum rigid waterproof mortar provided by the present invention has a moderate setting time and can meet the needs of actual projects;
[0027] The preparation method of the modified phosphogypsum provided by the present invention improves the compatibility of the phosphogypsum with cement-based materials by modifying the phosphogypsum, so that the phosphogypsum has good compatibility with the cement-based materials;
[0028] 4) The maximum anti-seepage pressure of the phosphogypsum rigid waterproof mortar provided by the present invention can reach 2.8MPa, while the building materials industry standard of polymer mortar in my country (JC / T984-2011 standard) stipulates that the 28d anti-seepage pressure is ≥1.5MPa, which is qualified. It can be seen that the anti-seepage pressure of the phosphogypsum rigid waterproof mortar of the present invention far exceeds the industry standard
[0029] The phosphogypsum used in the present invention is dehydrated by heat treatment, i.e., calcined at a constant temperature of 820°C for 0 to 2h, so as to remove impurities such as soluble phosphorus and organic matter, thereby making its performance stable. The present invention aims to develop a new type of cementitious material, which uses calcined phosphogypsum as a base material and adds materials such as metakaolin and slag to produce waterproof mortar with excellent waterproof effect. The phosphogypsum-based waterproof mortar prepared by the present invention uses phosphogypsum and slag as main raw materials and uses alkaline excitation. The cementitious material produced by the present invention has water-hardening property, which breaks the limitation that gypsum can only be used as an air-hardening cementitious material, and provides a wider range of possibilities for future application fields.
[0030] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A gypsum-based polymer waterproof mortar, characterized in that: The invention comprises the following components in parts by weight: 41.6-60 parts of phosphogypsum, 4.4-6 parts of building gypsum, 30-50 parts of slag, 4 parts of cement, 0.15-0.30 parts of K2SO4, 33-39 parts of water, 150-225 parts of fine sand, 0-5 parts of latex powder, 0-4.5 parts of tung oil or 0-1.5 parts of calcium stearate, 5-10 parts of nano magnesium oxide, 5-10 parts of fly ash, 0.07-0.13 parts of water reducing agent and 0-0.15 parts of defoaming agent, wherein the water-cement ratio is 0.33-0.
39.
2. The gypsum-based polymer waterproof mortar according to claim 1, characterized in that: The modified phosphogypsum is prepared according to the following method: (1) mixing phosphogypsum with quicklime and aging to obtain an initial material; (2) mixing the initial material with water evenly, then adjusting the pH value to 6-8, filtering and drying to obtain treated phosphogypsum; (3) mixing the treated phosphogypsum with reaction solution A evenly to form a mixed solution B, wherein the reaction solution A is an ethanol solution of a modifier; (4) adjusting the pH value of the mixed solution B to 6-8, heating, drying and grinding to obtain modified phosphogypsum.
3. The gypsum-based polymer waterproof mortar according to claim 1, characterized in that: The particle size of the fine sand is 0.3-1.18 mm.
4. The gypsum-based polymer waterproof mortar according to claim 1, characterized in that: The water reducer is a polycarboxylate water reducer.
5. The gypsum-based polymer waterproof mortar according to claim 1, characterized in that: The latex powder is dispersible latex powder.
6. The gypsum-based polymer waterproof mortar according to claim 1, characterized in that: The tung oil is raw tung oil.
7. The gypsum-based polymer waterproof mortar according to claim 1, characterized in that: In terms of mass, the quicklime is 5-20 parts relative to 100 parts of the phosphogypsum.
8. The gypsum-based polymer waterproof mortar according to claim 1, characterized in that: The mass ratio of the initial material to water is 1:0.3-0.8, and the pH value is adjusted with ammonia water.
Citation Information
Patent Citations
Modified phosphogypsum and phosphogypsum rigid waterproof mortar and preparation method thereof
CN107686255A
Phosphogypsum-based waterproof mortar and preparation method thereof