High-strength zirconium silicate composite ceramic grinding medium and preparation method thereof
By adopting the preparation method of high-strength zirconium silicate composite ceramic grinding media and using ceramic waste to replace zircon stone, the problems of insufficient strength and high production cost of zirconium silicate beads are solved, and high strength, wear resistance and corrosion resistance are achieved. , extending the service life and providing secondary use of ceramic waste.
Patent Information
- Application Number
- CN202411259835.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The strength of existing zirconium silicate beads is low, making it difficult to meet the needs of high-speed sand mills, and the production cost is high. Moreover, the existing process is difficult to prepare microbeads smaller than 1 mm, and cannot meet the needs of ultra-fine grinding.
The preparation method of high-strength zirconium silicate composite ceramic grinding media is adopted, including the mixing and sintering of zircon stone, ceramic waste, silicon carbide powder, bauxite and other ingredients, and forming a sphere through pressing and ball rolling machine to improve the strength of the grinding media. and wear resistance.
It reduces production costs, improves the strength and wear resistance of zirconium silicate composite ceramic grinding media, extends its service life, and provides a secondary use method for ceramic waste. The cost is significantly lower than that of conventional zirconium silicate beads.
Smart Images

Figure CN118771884A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramics, and in particular to a high-strength zirconium silicate composite ceramic grinding medium and a preparation method thereof. Background Art
[0002] Ultrafine grinding sand mills are widely used in new energy battery materials, paints, coatings and other fields. Through various complex movements such as mutual collision and extrusion of grinding media, materials are crushed; grinding media, also known as grinding media, are the key to crushing materials. At present, the types of grinding media are roughly steel balls, glass beads, ordinary ceramic beads, alumina beads, zirconium silicate beads, zirconium oxide beads, etc., with different performances and prices. Steel balls are less used due to their poor corrosion resistance and wear resistance; glass beads have low strength, high wear and easy to pollute materials; ordinary ceramic grinding media (the main crystal phase is aluminum silicate and glass phase), the product has coarse grains and poor performance, and can only be used in low-end fields; alumina ceramic grinding media (the main crystal phase is α-alumina) is mainly used for grinding hard mineral materials, but alumina materials have low fracture toughness and poor wear resistance, and are not suitable for high-speed sand mills; zirconium oxide has a high specific gravity and good performance, and is a high-end grinding material, but the price is very high, which is 3 to 4 times that of zirconium silicate beads, and due to phase change aging, it is limited to use in some medium and high temperature conditions.
[0003] Zirconium silicate beads are composed of uniform and dense zirconium silicate grains. The grain boundaries usually have a low melting point SiO2 glass phase. The zirconium oxide content is usually 45-65wt%, and the mechanical properties are good. It is an excellent grinding medium material. It is suitable for the dispersion and grinding of materials with high viscosity, medium temperature and medium hardness, such as titanium dioxide, calcium carbonate, kaolin, paint, etc. The current production process of zirconium silicate beads is basically high temperature melting method and sintering method.
[0004] In the prior art, the invention patent "Silicon Zirconium Ball Manufacturing Technology" with application number CN99118965.5 discloses a method for preparing microspheres by mixing molten zircon and a solvent. The disadvantage of this method is that the size of the zirconium silicate balls is small and the particle size uniformity is poor. The invention patent "A Method for Preparing Zirconium Silicate Beads" with application number CN201010122895.8 discloses a method for producing zirconium silicate balls by isostatic pressing and high-temperature sintering. The disadvantage of this method is that the isostatic pressing capacity is low, the cost is high, and it is almost impossible to produce beads below 3mm. As the demand for ultra-fine grinding becomes more and more widespread, the domestic market demand for microspheres below 1mm will be the dominant direction in the future.
[0005] Moreover, the overall strength of zirconium silicate ceramic materials is lower than that of zirconia ceramic materials and zirconium-aluminum composite ceramic materials. Since the rotation speed of the sand mill is quite high and the linear speed reaches more than 20 meters / second, the impact force is very large, and the strength requirements of the grinding beads are very high. Therefore, the present application provides a high-strength zirconium silicate composite ceramic grinding medium and a preparation method thereof to meet the needs. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a high-strength zirconium silicate composite ceramic grinding medium and a preparation method thereof to solve the existing problems.
[0007] In order to solve the above technical problems, the present invention provides the following technical solutions: A high-strength zirconium silicate composite ceramic grinding medium, comprising, in percentage, 60%-75% zircon, 10%-15% ceramic waste, 5%-10% silicon carbide powder, 0%-8% bauxite, 2%-5% dolomite, 1%-3% barium carbonate, 1%-2% yttrium oxide, 2%-3% montmorillonite, 0%-3% aluminum oxide, 0%-3% magnesium oxide, 2%-4% dispersant, and 2%-4% binder.
[0008] In some examples, the binder is a mixture of one or more of zirconium oxide, aluminum oxide, or aluminum silicate.
[0009] In some examples, the dispersant is one of sodium dodecyl sulfate, alkyl polyoxyethylene ether, alkyl benzene sulfonate or a mixture thereof, the ceramic waste is ceramic waste containing zirconium oxide, aluminum oxide and silicon dioxide, and the zircon should be zircon raw material containing zirconium oxide of not less than 60wt%.
[0010] A method for preparing a high-strength zirconium silicate composite ceramic grinding medium comprises the following steps: S1. Preparation of zirconium silicate composite ceramic grinding medium raw materials; S2, preparation of zirconium silicate composite ceramic grinding medium spheres; S3. Sintering, grinding and quality inspection of spheres.
[0011] In some examples, the specific steps of S1 are: S101, the finished zircon and ceramic waste are mixed and crushed, and then water is added to pulp and filter to obtain a slurry with large particles of impurities filtered out; the slurry with large particles of impurities filtered out is de-ironized and then ground to D 50 ≤0.6μm, obtaining a first mixed slurry; S102, drying the ground first mixed slurry to obtain a first mixed powder; S103, mixing the first mixed powder with silicon carbide powder, bauxite, dolomite, barium carbonate, yttrium oxide, montmorillonite and aluminum oxide or magnesium oxide weighed in proportion, and then grinding the mixture in a sand mill until D 50 ≤0.4μm, and obtain the second mixed slurry; S104, drying the second mixed slurry to obtain a second mixed powder; S105, mixing the first mixed powder and the second mixed powder to obtain a third mixed powder for later use.
[0012] In some examples, the specific steps of S2 are: S201, mixing the prepared third mixed powder with a binder and a dispersant, adding adhesive glue to wet the powder, and putting the powder into a mud mixer to mix the powder into wet particles; S202, pressing the wet particles into blocks by pressing, and then drying the block ceramic grinding medium, crushing it by a crusher after drying, and sieving it through a 100-200 mesh sieve, and putting the sieved particles into a ball rolling machine; S203, evenly adding water and the third mixed powder into the ball rolling machine, so that the ceramic grinding medium in the ball rolling machine forms spheres of uniform size.
[0013] In some examples, the specific steps of S3 are: S301, placing the prepared sphere in a cool place for shade drying to reduce its moisture content to ≤3%, and then sintering the sphere; S302. After sintering, the sphere is cooled at room temperature. After being sufficiently cooled, the sphere is ground and polished. The ceramic grinding media of each sphere is quality inspected and stored after passing the inspection.
[0014] In some examples, the slurry in S101 is de-ironed using an electromagnetic de-ironing device, and the de-ironing step needs to be repeated three times before grinding can be performed. The drying temperature in S102 and S104 is 150° C.-200° C., and the drying time is 3 h-6 h.
[0015] In some examples, the bonding glue of S201 is a mixture of 10%-15% sodium fatty alcohol alkyl sulfonate, 10%-15% maltodextrin aqueous solution and 70%-80% deionized water, the drying temperature of the block ceramic grinding medium in S202 is 150°C-200°C, the drying time is 3h-6h, and the crushing of the block ceramic grinding medium in S202 is carried out by roller crushing or steel crushing.
[0016] In some examples, the shade drying time of S301 is 24h-48h, the sintering temperature in S301 is 1300°C-1600°C, and the sintering time is controlled between 6h-10h.
[0017] Compared with the prior art, the present invention has at least the following beneficial effects: In the above scheme, by using ceramic waste to replace part of the zircon, the consumption of zircon is reduced, the production cost of the enterprise is reduced, the raw material cost is low, the preparation method is simple, and the prepared high-strength zirconium silicate composite ceramic has high grinding medium strength, high toughness, wear resistance, erosion resistance, corrosion resistance, and abrasion resistance, and its wear resistance is better than that of conventional zirconium silicate beads; the service life is longer than that of conventional zirconium silicate beads, the cost is greatly reduced compared with conventional zirconium silicate beads, and a new utilization method is provided for ceramic waste, so that ceramic waste can be reused. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The accompanying drawings, which are incorporated herein and constitute a part of the specification, illustrate embodiments of the present disclosure and, together with the description, further serve to explain the principles of the present disclosure and to enable those skilled in the relevant art to make and use the present disclosure.
[0019] Figure 1 The present invention is a flow chart of a method for preparing a high-strength zirconium silicate composite ceramic grinding medium. DETAILED DESCRIPTION
[0020] The following is a detailed description of a high-strength zirconium silicate composite ceramic grinding medium and a preparation method thereof provided by the present invention in conjunction with the accompanying drawings and specific embodiments. At the same time, it is explained here that in order to make the embodiments more detailed, the following embodiments are listed as the best and preferred embodiments, and other alternatives can also be used by technicians in some known technical fields; and the accompanying drawings are only for more specific description of the embodiments, and are not intended to specifically limit the present invention.
[0021] It should be noted that the references to "one embodiment", "embodiment", "exemplary embodiment", "some embodiments" and the like in the specification indicate that the described embodiments may include specific features, structures or characteristics, but not every embodiment may include the specific features, structures or characteristics. In addition, when a specific feature, structure or characteristic is described in conjunction with an embodiment, it should be within the knowledge of a person skilled in the art to implement such feature, structure or characteristic in conjunction with other embodiments (whether or not explicitly described).
[0022] In general, a term can be understood, at least in part, from its use in context. For example, depending, at least in part, on the context, the term "one or more" as used herein can be used to describe any feature, structure, or characteristic in the singular sense, or can be used to describe a combination of features, structures, or characteristics in the plural sense. Additionally, the term "based on" can be understood as not necessarily intended to convey an exclusive set of factors, but can instead, depending, at least in part, on the context, allow for the presence of other factors that are not necessarily explicitly described.
[0023] It will be understood that the meaning of “on,” “over,” and “above” in this disclosure should be interpreted in the broadest manner, so that “on” not only means “directly on” something, but also includes the meaning of being “on” something with intervening features or layers therebetween, and “on” or “over” not only means “on” or “above” something, but also includes the meaning of being “on” or “above” something with no intervening features or layers therebetween.
[0024] Additionally, spatially relative terms such as "under," "beneath," "lower," "above," "upper," and the like may be used herein for descriptive convenience to describe the relationship of one element or feature to another element or features, as shown in the accompanying drawings. Spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the accompanying drawings. The device may be oriented in other ways, and the spatially relative descriptors used herein may be similarly interpreted accordingly. Example 1
[0025] An embodiment of the present invention provides a high-strength zirconium silicate composite ceramic grinding medium, which includes, in percentage, 65% zircon, 10% ceramic waste, 5% silicon carbide powder, 5% dolomite, 2% barium carbonate, 3% yttrium oxide, 3% montmorillonite, 3% magnesium oxide, 1% dispersant, and 3% binder.
[0026] It should be further explained in this embodiment that the binder is made of a mixture of zirconium oxide and aluminum silicate.
[0027] It should be further explained in this embodiment that the dispersant is one of sodium dodecyl sulfate, alkyl polyoxyethylene ether, alkyl benzene sulfonate or a mixture thereof, the ceramic waste is ceramic waste containing zirconium oxide, aluminum oxide and silicon dioxide, and the zircon should be a zircon raw material containing not less than 60wt% of zirconium oxide.
[0028] like Figure 1 As shown, a method for preparing a high-strength zirconium silicate composite ceramic grinding medium comprises the following steps; S1. Preparation of zirconium silicate composite ceramic grinding medium raw materials; S101, the finished zircon and ceramic waste are mixed and crushed, and then water is added to pulp and filter to obtain a slurry with large particles of impurities filtered out; the slurry with large particles of impurities filtered out is de-ironized and then ground to D 50 ≤0.6μm, obtaining a first mixed slurry; S102, drying the ground first mixed slurry to obtain a first mixed powder; S103, mixing the first mixed powder with silicon carbide powder, bauxite, dolomite, barium carbonate, yttrium oxide, montmorillonite and aluminum oxide or magnesium oxide weighed in proportion, and then grinding the mixture in a sand mill until D 50 ≤0.4μm, and obtain the second mixed slurry; S104, drying the second mixed slurry to obtain a second mixed powder; S105, mixing the first mixed powder with the second mixed powder to obtain a third mixed powder for standby use; S2, preparation of zirconium silicate composite ceramic grinding medium spheres; S201, mixing the prepared third mixed powder with a binder and a dispersant, adding adhesive glue to wet the powder, and putting the powder into a mud mixer to mix the powder into wet particles; S202, pressing the wet particles into blocks by pressing, and then drying the block ceramic grinding medium, crushing it by a crusher after drying, and sieving it through a 200-mesh sieve, and putting the sieved particles into a ball rolling machine; S203, evenly adding water and the third mixed powder into the ball rolling machine, so that the ceramic grinding medium in the ball rolling machine forms spheres of uniform size; S3, sintering, grinding and quality inspection of spheres; S301, placing the prepared sphere in a cool place for shade drying to reduce its moisture content to ≤3%, and then sintering the sphere; S302. After sintering, the sphere is cooled at room temperature. After being sufficiently cooled, the sphere is ground and polished. The ceramic grinding media of each sphere is quality inspected and stored after passing the inspection.
[0029] It should be further explained in this embodiment that the slurry in S101 is de-ironed by an electromagnetic de-ironing device, and the de-ironing step needs to be repeated three times before grinding can be performed. The drying temperature in S102 and S104 is 160° C. and the drying time is 5 hours.
[0030] What needs to be further explained in this embodiment is that the bonding glue of S201 is a mixture of 13% sodium fatty alcohol alkyl sulfonate, 12% maltodextrin aqueous solution and 75% deionized water, the mass ratio of the bonding glue to the sphere is 20:80, the drying temperature of the block ceramic grinding medium in S202 is 160°C, the drying time is 5h, and the crushing of the block ceramic grinding medium in S202 is carried out by roller crushing or steel crushing.
[0031] It should be further explained in this embodiment that the shade drying time of S301 is 35 hours, the sintering temperature in S301 is 1300° C., and the sintering time is controlled within 10 hours. Example 2
[0032] A high-strength zirconium silicate composite ceramic grinding medium comprises, in percentage, 60% zircon, 10% ceramic waste, 5% silicon carbide powder, 5% bauxite, 5% dolomite, 2% barium carbonate, 2% yttrium oxide, 2% montmorillonite, 1% aluminum oxide, 3% magnesium oxide, 2% dispersant and 3% binder.
[0033] It should be further explained in this embodiment that the binder is a mixture of one or more of zirconium oxide, aluminum oxide or aluminum silicate.
[0034] It should be further explained in this embodiment that the dispersant is one of sodium dodecyl sulfate, alkyl polyoxyethylene ether, alkyl benzene sulfonate or a mixture thereof, the ceramic waste is ceramic waste containing zirconium oxide, aluminum oxide and silicon dioxide, and the zircon should be a zircon raw material containing not less than 60wt% of zirconium oxide.
[0035] A method for preparing a high-strength zirconium silicate composite ceramic grinding medium comprises the following steps: S1. Preparation of zirconium silicate composite ceramic grinding medium raw materials; S101, the finished zircon and ceramic waste are mixed and crushed, and then water is added to pulp and filter to obtain a slurry with large particles of impurities filtered out; the slurry with large particles of impurities filtered out is de-ironized and then ground to D 50 ≤0.6μm, obtaining a first mixed slurry; S102, drying the ground first mixed slurry to obtain a first mixed powder; S103, mixing the first mixed powder with silicon carbide powder, bauxite, dolomite, barium carbonate, yttrium oxide, montmorillonite and aluminum oxide or magnesium oxide weighed in proportion, and then grinding the mixture in a sand mill until D 50 ≤0.4μm, and obtain the second mixed slurry; S104, drying the second mixed slurry to obtain a second mixed powder; S105, mixing the first mixed powder with the second mixed powder to obtain a third mixed powder for standby use; S2, preparation of zirconium silicate composite ceramic grinding medium spheres; S201, mixing the prepared third mixed powder with a binder and a dispersant, adding adhesive glue to wet the powder, and putting the powder into a mud mixer to mix the powder into wet particles; S202, pressing the wet particles into blocks by pressing, and then drying the block ceramic grinding medium, crushing it by a crusher after drying, and sieving it through a 150-mesh sieve, and putting the sieved particles into a ball rolling machine; S203, evenly adding water and the third mixed powder into the ball rolling machine, so that the ceramic grinding medium in the ball rolling machine forms spheres of uniform size; S3, sintering, grinding and quality inspection of spheres; S301, placing the prepared sphere in a cool place for shade drying to reduce its moisture content to ≤3%, and then sintering the sphere; S302. After sintering, the sphere is cooled at room temperature. After being sufficiently cooled, the sphere is ground and polished. The ceramic grinding media of each sphere is quality inspected and stored after passing the inspection.
[0036] It should be further explained in this embodiment that the slurry is de-ironed by an electromagnetic de-ironing device in S101, and the de-ironing step needs to be repeated three times before grinding can be performed. The drying temperature in S102 and S104 is 200° C. and the drying time is 3 hours.
[0037] It should be further explained in this embodiment that the slurry in S101 is de-ironed by an electromagnetic de-ironing device, and the de-ironing step needs to be repeated three times before grinding can be performed. The drying temperature in S102 and S104 is 200° C. and the drying time is 3 hours.
[0038] It should be further explained in this embodiment that the bonding glue of S201 is mixed with 15% sodium fatty alcohol alkyl sulfonate, 15% maltodextrin aqueous solution and 70% deionized water, the mass ratio of the bonding glue to the sphere is 15:80, the drying temperature of the block ceramic grinding medium in S202 is 200°C, the drying time is 3h, and the crushing of the block ceramic grinding medium in S202 is carried out by roller crushing or steel crushing.
[0039] What needs to be further explained in this embodiment is that, it is characterized in that, the shade drying time of S301 is 40 hours, the sintering temperature in S301 is 1500°C, and the sintering time is controlled between 7 hours. Example 3
[0040] An embodiment of the present invention provides a high-strength zirconium silicate composite ceramic grinding medium, which includes, in percentage, 60% zircon, 10% ceramic waste, 5% silicon carbide powder, 5% bauxite, 2% dolomite, 3% barium carbonate, 2% yttrium oxide, 3% montmorillonite, 3% magnesium oxide, 3% dispersant, and 4% binder.
[0041] It should be further explained in this embodiment that the binder is made of a mixture of zirconium oxide and aluminum oxide.
[0042] It should be further explained in this embodiment that the dispersant is one of sodium dodecyl sulfate, alkyl polyoxyethylene ether, alkyl benzene sulfonate or a mixture thereof, the ceramic waste is ceramic waste containing zirconium oxide, aluminum oxide and silicon dioxide, and the zircon should be a zircon raw material containing not less than 60wt% of zirconium oxide.
[0043] like Figure 1 As shown, a method for preparing a high-strength zirconium silicate composite ceramic grinding medium comprises the following steps; S1. Preparation of zirconium silicate composite ceramic grinding medium raw materials; S101, the finished zircon and ceramic waste are mixed and crushed, and then water is added to pulp and filter to obtain a slurry with large particles of impurities filtered out; the slurry with large particles of impurities filtered out is de-ironized and then ground to D 50 ≤0.6μm, obtaining a first mixed slurry; S102, drying the ground first mixed slurry to obtain a first mixed powder; S103, mixing the first mixed powder with silicon carbide powder, bauxite, dolomite, barium carbonate, yttrium oxide, montmorillonite and aluminum oxide or magnesium oxide weighed in proportion, and then grinding the mixture in a sand mill until D 50 ≤0.4μm, and obtain the second mixed slurry; S104, drying the second mixed slurry to obtain a second mixed powder; S105, mixing the first mixed powder with the second mixed powder to obtain a third mixed powder for standby use; S2, preparation of zirconium silicate composite ceramic grinding medium spheres; S201, mixing the prepared third mixed powder with a binder and a dispersant, adding adhesive glue to wet the powder, and putting the powder into a mud mixer to mix the powder into wet particles; S202, pressing the wet particles into blocks by pressing, and then drying the block ceramic grinding medium, crushing it by a crusher after drying, and sieving it through a 100-mesh sieve, and putting the sieved particles into a ball rolling machine; S203, evenly adding water and the third mixed powder into the ball rolling machine, so that the ceramic grinding medium in the ball rolling machine forms spheres of uniform size; S3, sintering, grinding and quality inspection of spheres; S301, placing the prepared sphere in a cool place for shade drying to reduce its moisture content to ≤3%, and then sintering the sphere; S302. After sintering, the sphere is cooled at room temperature. After being sufficiently cooled, the sphere is ground and polished. The ceramic grinding media of each sphere is quality inspected and stored after passing the inspection.
[0044] It should be further explained in this embodiment that the slurry in S101 is de-ironed by an electromagnetic de-ironing device, and the de-ironing step needs to be repeated three times before grinding can be performed. The drying temperature in S102 and S104 is 150° C. and the drying time is 4 hours.
[0045] It should be further explained in this embodiment that the bonding glue of S201 is mixed with 10% sodium fatty alcohol alkyl sulfonate, 10% maltodextrin aqueous solution and 80% deionized water, the mass ratio of the bonding glue to the sphere is 10:90, the drying temperature of the block ceramic grinding medium in S202 is 150°C, the drying time is 4h, and the crushing of the block ceramic grinding medium in S202 is carried out by roller crushing or steel crushing.
[0046] It should be further explained in this embodiment that the shade drying time of S301 is 38 hours, the sintering temperature in S301 is 1400° C., and the sintering time is controlled at 8 hours.
[0047] The technical solution provided by the present invention reduces the consumption of zircon and the production cost of the enterprise by replacing a part of the zircon with ceramic waste, and the raw material cost is low and the preparation method is simple. The prepared high-strength zirconium silicate composite ceramic has high grinding medium strength, high toughness, wear resistance, erosion resistance, corrosion resistance and abrasion resistance, and its wear is better than that of conventional zirconium silicate beads; the service life is longer than that of conventional zirconium silicate beads, the cost is greatly reduced compared with conventional zirconium silicate beads, and a new utilization method is provided for ceramic waste, so that ceramic waste can be reused.
[0048] The present invention covers any substitution, modification, equivalent method and scheme made on the essence and scope of the present invention. In order to make the public have a thorough understanding of the present invention, specific details are described in detail in the following preferred embodiments of the present invention, but those skilled in the art can fully understand the present invention without the description of these details. In addition, in order to avoid unnecessary confusion about the essence of the present invention, well-known methods, processes, procedures, components and circuits are not described in detail.
[0049] A person skilled in the art will appreciate that all or part of the steps in the above-mentioned embodiment method can be completed by instructing related hardware through a program, and the program can be stored in a computer-readable storage medium, such as ROM / RAM, a disk, an optical disk, etc.
[0050] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A high-strength zirconium silicate composite ceramic grinding medium, characterized in that: In terms of percentage, it includes: zircon 60%-75%, ceramic waste 10%-15%, silicon carbide powder 5%-10%, bauxite 0%-8%, dolomite 2%-5%, barium carbonate 1%-3%, yttrium oxide 1%-2%, montmorillonite 2%-3%, aluminum oxide 0%-3%, magnesium oxide 0%-3%, dispersant 2%-4%, and binder 2%-4%.
2. A high-strength zirconium silicate composite ceramic grinding medium according to claim 1, characterized in that: The binder is a mixture of one or more of zirconium oxide, aluminum oxide or aluminum silicate.
3. The high-strength zirconium silicate composite ceramic grinding medium according to claim 1, characterized in that: The dispersant is one of sodium dodecyl sulfate, alkyl polyoxyethylene ether, alkyl benzene sulfonate or a mixture thereof; the ceramic waste is ceramic waste containing zirconium oxide, aluminum oxide and silicon dioxide; and the zircon is zircon raw material containing zirconium oxide of not less than 60wt%.
4. The method for preparing a high-strength zirconium silicate composite ceramic grinding medium according to claim 1, applied to a high-strength zirconium silicate composite ceramic grinding medium according to any one of claims 1 to 3, characterized in that: The steps include: S1. Preparation of zirconium silicate composite ceramic grinding medium raw materials; S2, preparation of zirconium silicate composite ceramic grinding medium spheres; S3. Sintering, grinding and quality inspection of spheres.
5. The method for preparing a high-strength zirconium silicate composite ceramic grinding medium according to claim 4, characterized in that: The specific steps of S1 are: S101, the finished zircon and ceramic waste are mixed and crushed, and then water is added to pulp and filter to obtain a slurry with large particles of impurities filtered out; the slurry with large particles of impurities filtered out is de-ironized and then ground to D 50 ≤0.6μm, obtaining a first mixed slurry; S102, drying the ground first mixed slurry to obtain a first mixed powder; S103, mixing the first mixed powder with silicon carbide powder, bauxite, dolomite, barium carbonate, yttrium oxide, montmorillonite and aluminum oxide or magnesium oxide weighed in proportion, and then grinding the mixture in a sand mill until D 50 ≤0.4μm, and obtain the second mixed slurry; S104, drying the second mixed slurry to obtain a second mixed powder; S105, mixing the first mixed powder and the second mixed powder to obtain a third mixed powder for later use.
6. The method for preparing a high-strength zirconium silicate composite ceramic grinding medium according to claim 4, characterized in that: The specific steps of S2 are: S201, mixing the prepared third mixed powder with a binder and a dispersant, adding adhesive glue to wet the powder, and putting the powder into a mud mixer to mix the powder into wet particles; S202, pressing the wet particles into blocks by pressing, and then drying the block ceramic grinding medium, crushing it by a crusher after drying, and sieving it through a 100-200 mesh sieve, and putting the sieved particles into a ball rolling machine; S203, evenly adding water and the third mixed powder into the ball rolling machine, so that the ceramic grinding medium in the ball rolling machine forms spheres of uniform size.
7. The method for preparing a high-strength zirconium silicate composite ceramic grinding medium according to claim 4, characterized in that: The specific steps of S3 are: S301, placing the prepared sphere in a cool place for shade drying to reduce its moisture content to ≤3%, and then sintering the sphere; S302. After sintering, the sphere is cooled at room temperature. After being sufficiently cooled, the sphere is ground and polished. The ceramic grinding media of each sphere is quality inspected and stored after passing the inspection.
8. The method for preparing a high-strength zirconium silicate composite ceramic grinding medium according to claim 5, characterized in that: In the S101, the slurry is deironed by an electromagnetic deironing device, and the deironing step needs to be repeated three times before grinding can be performed. The drying temperature in the S102 and S104 is 150° C.-200° C., and the drying time is 3h-6h.
9. The method for preparing a high-strength zirconium silicate composite ceramic grinding medium according to claim 6, characterized in that: The bonding glue of S201 is mixed with 10%-15% sodium fatty alcohol alkyl sulfonate, 10%-15% maltodextrin aqueous solution and 70%-80% deionized water. The drying temperature of the block ceramic grinding medium in S202 is 150℃-200℃, and the drying time is 3h-6h. The crushing of the block ceramic grinding medium in S202 is carried out by roller crushing or steel crushing.
10. The method for preparing a high-strength zirconium silicate composite ceramic grinding medium according to claim 7, characterized in that: The shade drying time of S301 is 24h-48h, the sintering temperature in S301 is 1300°C-1600°C, and the sintering time is controlled between 6h-10h.
Citation Information
Patent Citations
High-strength and high-toughness graphene composite ceramics
CN108546105A
Alumina-reinforced zirconia ceramic grinding medium and preparation method thereof
CN110642618A
Preparation method of waste continuous silicon carbide fiber reinforced silicate ceramic
CN114085089A
High-strength zirconium silicate composite ceramic grinding medium and preparation method thereof
CN116177989A
In situ production of silicon carbide reinforced ceramic composites
US5096858A