Preparation method of nano boron carbide reinforced high-thermal-conductivity compact silica brick

The preparation method enhanced by nano boron carbide solves the problem of silica bricks being prone to fission in high-temperature environments, improves the strength and plasticity of silica bricks, and achieves more efficient molding and longer-life silica brick production.

CN118771899AInactive Publication Date: 2024-10-15HUNAN UNIV OF SCI & TECH +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410806204.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing silica bricks are prone to fission in high-temperature environments and lack strength and plasticity, resulting in cumbersome equipment disassembly and low production efficiency.

Method used

Using the preparation method of nano boron carbide reinforcement, by mixing raw materials such as silica coarse powder, silica fine powder, boric acid and urea, and then going through steps such as ball milling, molding, drying, pre-sintering and sintering, nano-sheet boron carbide is generated, which improves silicon Bulk density and strength of bricks.

Benefits of technology

It improves the strength and plasticity of silica bricks, reduces the cracking phenomenon of molded products, enhances the internal structural density of blank products, and extends the service life of silica bricks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a preparation method of a nano boron carbide reinforced high-thermal-conductivity compact silica brick. The preparation method comprises the following steps: step 1, putting a proper amount of main raw materials, a composite mineralizing agent and a binding agent into ball milling equipment, and mixing; 2, putting the mixed powder manufactured in the step 1 into forming equipment, and performing compression molding by using the forming equipment; step 3, drying the formed silica brick manufactured in the step 2 in an environment of 60-100 DEG C for 24-48 hours; step 4, pre-sintering the silica bricks dried in the step 3 in an environment of 400-800 DEG C for 3-6 hours; step five, sintering the pre-sintered silica brick in the step four in an environment of 1400-1600 DEG C for 5-8 hours; and 6, cooling the silica brick sintered in the step 5 to normal temperature. After the boric acid and the urea are added as binding agents, the adhesion between the raw materials is enhanced, extrusion forming through forming equipment is facilitated, in a high-temperature environment, the boric acid and the urea react to produce nano flaky boron carbide, the volume density of a blank product is improved, the internal structure of the blank product is further densified, and the strength of the silica brick is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of silicon bricks, in particular to a method for preparing nano boron carbide reinforced high thermal conductivity dense silicon bricks. Background Art

[0002] As important refractory materials, high alumina bricks and silica bricks are mainly used in the partition walls of the carbonization chamber and combustion chamber of the coking oven, the heat storage chamber and slag chamber of the steelmaking flat furnace, the soaking furnace, the refractory materials of the glass melting furnace and the vault and other load-bearing parts of the ceramic firing kiln, to enhance the refractory performance of the above-mentioned devices.

[0003] In order to meet different production needs, there are different refractory materials on the market. For example, a Chinese patent with the patent publication number CN101117294A discloses a 7m coke oven silica brick, whose raw material formula contains 25-35% coarse silica powder, 41-47% medium silica powder, 10-20% fine powder composed of 50% silica and 50% residual silica brick, and 10-20% residual silica brick. It also includes auxiliary materials, a mineralizer 1.9-2.1% made of manganese powder, iron scale powder and potassium feldspar in a ratio of 0.5:0.5:1, and lime milk 7 .5-8.5%, pulp 0.9-1.1%, etc., and a silicon carbide brick disclosed in a Chinese patent with patent publication number CN205425827U, including a main brick and a sub-body brick. The main brick is a square structure with convex strips on the upper surface and corresponding grooves on the lower surface. The convex strips and grooves of the upper and lower adjacent main bricks are engaged with each other; the two sides of the main brick also have vertical T-shaped slots, and the sub-body brick is an I-shaped structure, and the two ends of the sub-body brick are respectively inserted into the slots of two adjacent main bricks to connect the two adjacent main bricks.

[0004] When using the silica brick refractory materials provided by the above patents, or other similar refractory materials, although it can assist the heat storage chamber, slag chamber, soaking furnace and other equipment to complete production, the silica bricks need to withstand large changes in temperature because they are in a high temperature environment of more than 1300°C for a long time, which may cause the silica bricks to fission, that is, the strength of the silica bricks needs to be improved. Otherwise, the damaged silica bricks need to be replaced after the heat storage chamber, slag chamber, soaking furnace and other equipment work. Because the disassembly of the above equipment is cumbersome, time-consuming and labor-intensive, and the replacement of silica bricks requires stopping its work, affecting the production of silica bricks. In addition, when producing silica bricks, it is necessary to mix and stir a variety of raw materials and then pressurize them through a molding machine. The molded products have low plasticity, which causes the products to crack, affecting the production of silica bricks. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a nano boron carbide reinforced high thermal conductivity dense silicon brick, aiming to improve the problem that the strength and plasticity of silicon bricks still need to be improved.

[0006] The present invention is achieved by: a method for preparing a nano boron carbide reinforced high thermal conductivity dense silicon brick, comprising: Step 1: Add appropriate amount of main raw materials, composite mineralizer and binder into the ball mill and mix; Step 2: putting the mixed powder produced in step 1 into a molding device, and using the molding device to perform compression molding; Step 3: Dry the molded silica bricks manufactured in step 2 in an environment of 60-100°C for 24-48 hours; Step 4: The dried silica bricks in step 3 are pre-sintered at 400-800°C for 3-6h; Step 5: The pre-sintered silicon bricks in step 4 are sintered at 1400-1600°C for 5-8h; Step 6: The silicon brick sintered in step 5 is cooled to room temperature to obtain the product.

[0007] Preferably, the pre-sintered silicon bricks in step 4 generate nano-flaky boron carbide.

[0008] Preferably, the main raw materials in step one are set to be silica coarse powder and silica fine powder, wherein the content of silica coarse powder is 40-70wt% and the content of silica fine powder is 30-50wt%.

[0009] Preferably, the binder in step one is set to be boric acid and urea, wherein the boric acid content is 1-5wt% and the urea content is 1-3wt%.

[0010] Preferably, boric acid and urea generate nano-sheet boron carbide under high temperature conditions.

[0011] Preferably, the content of the composite mineralizer in step 1 is 1-3wt%, and the composite mineralizer can be magnesium oxide.

[0012] Preferably, the content of the composite mineralizer in step 1 is 1-3wt%, and the composite mineralizer can be set as calcium oxide.

[0013] Preferably, the content of the composite mineralizer in step 1 is 1-3 wt%, and the composite mineralizer can be silicon carbide.

[0014] Compared with the prior art, the beneficial effects of the present invention are: after adding boric acid and urea as binders, the adhesion between the raw materials is enhanced, which facilitates extrusion molding through molding equipment, and under high temperature environment, boric acid and urea react to produce nano-flaky boron carbide, thereby increasing the volume density of the green product, further densifying its internal structure, and improving the strength of the silicon brick. Specific implementation method: In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0016] The following is further described in conjunction with specific embodiments: Example 1 A nano boron carbide reinforced high thermal conductivity dense silica brick comprises main raw materials, a composite mineralizer, a binder, etc. Specifically, the main raw materials are set to silica coarse powder and silica fine powder, wherein the content of silica coarse powder is 40wt% and the content of silica fine powder is 30wt%. The binder is set to boric acid and urea, wherein the content of boric acid is 1wt% and the content of urea is 1wt%. Before sintering, the plasticity of the brick body can be enhanced in cooperation with boric acid and urea, that is, various raw materials can be bonded together to avoid cracking of the formed brick body due to low plasticity. In addition, boric acid and urea generate nano flaky boron carbide under high temperature environment, and the nano flaky boron carbide can increase the volume density of the blank product, further densify its internal structure, and thus improve the strength of the silica brick. The content of the composite mineralizer is 1wt%, and the composite mineralizer can be set to magnesium oxide, calcium oxide, silicon carbide, etc.

[0017] To prepare silica bricks using the above raw materials, it is necessary to follow the following preparation methods one by one. Step 1: Add appropriate amount of main raw materials, composite mineralizer and binder into the ball mill and mix them.

[0018] Step 2: Put the mixed powder prepared in step 1 into the molding equipment, and use the molding equipment to perform compression molding.

[0019] Step 3: The molded silica bricks manufactured in step 2 are dried in an environment of 60°C for 24 hours.

[0020] Step 4: The silica bricks dried in step 3 are pre-sintered at 400°C for 3 hours.

[0021] Step 5: The pre-sintered silicon bricks in step 4 are sintered at 1400°C for 5 hours.

[0022] Step 6: The silicon bricks sintered in step 5 are cooled to room temperature to obtain the product.

[0023] Example 2 A nano boron carbide reinforced high thermal conductivity dense silica brick comprises main raw materials, a composite mineralizer, a binder, etc. Specifically, the main raw materials are set to silica coarse powder and silica fine powder, wherein the content of silica coarse powder is 70wt% and the content of silica fine powder is 50wt%. The binder is set to boric acid and urea, wherein the content of boric acid is 5wt% and the content of urea is 3wt%. Before sintering, the plasticity of the brick body can be enhanced in combination with boric acid and urea, that is, various raw materials can be bonded together to avoid cracking of the formed brick body due to low plasticity. In addition, boric acid and urea generate nano flaky boron carbide under high temperature environment, and the nano flaky boron carbide can increase the volume density of the blank product, further densify its internal structure, and thus improve the strength of the silica brick. The content of the composite mineralizer is 3wt%, and the composite mineralizer can be set to magnesium oxide, calcium oxide, silicon carbide, etc.

[0024] To prepare silica bricks using the above raw materials, it is necessary to follow the following preparation methods one by one. Step 1: Add appropriate amount of main raw materials, composite mineralizer and binder into the ball mill and mix them.

[0025] Step 2: Put the mixed powder prepared in step 1 into the molding equipment, and use the molding equipment to perform compression molding.

[0026] Step 3: The molded silica bricks manufactured in step 2 are dried in an environment of 100° C. for 48 hours.

[0027] Step 4: The silica bricks dried in step 3 are pre-sintered at 800°C for 6 hours.

[0028] Step 5: The pre-sintered silicon bricks in step 4 are sintered at 1600°C for 8 hours.

[0029] Step 6: The silicon bricks sintered in step 5 are cooled to room temperature to obtain the product.

[0030] Example 3 A nano boron carbide reinforced high thermal conductivity dense silica brick comprises main raw materials, a composite mineralizer, a binder, etc. Specifically, the main raw materials are set to silica coarse powder and silica fine powder, wherein the content of silica coarse powder is 40wt% and the content of silica fine powder is 30wt%. The binder is set to boric acid and urea, wherein the content of boric acid is 1wt% and the content of urea is 1wt%. Before sintering, the plasticity of the brick body can be enhanced in cooperation with boric acid and urea, that is, various raw materials can be bonded together to avoid cracking of the formed brick body due to low plasticity. In addition, boric acid and urea generate nano flaky boron carbide under high temperature environment, and the nano flaky boron carbide can increase the volume density of the blank product, further densify its internal structure, and thus improve the strength of the silica brick. The content of the composite mineralizer is 1wt%, and the composite mineralizer can be set to magnesium oxide, calcium oxide, silicon carbide, etc.

[0031] To prepare silica bricks using the above raw materials, it is necessary to follow the following preparation methods one by one. Step 1: Add appropriate amount of main raw materials, composite mineralizer and binder into the ball mill and mix them.

[0032] Step 2: Put the mixed powder prepared in step 1 into the molding equipment, and use the molding equipment to perform compression molding.

[0033] Step 3: The molded silica bricks manufactured in step 2 are dried in an environment of 100° C. for 48 hours.

[0034] Step 4: The silica bricks dried in step 3 are pre-sintered at 800°C for 6 hours.

[0035] Step 5: The pre-sintered silicon bricks in step 4 are sintered at 1600°C for 8 hours.

[0036] Step 6: The silicon bricks sintered in step 5 are cooled to room temperature to obtain the product.

[0037] Example 4 A nano boron carbide reinforced high thermal conductivity dense silica brick comprises main raw materials, a composite mineralizer, a binder, etc. Specifically, the main raw materials are set to silica coarse powder and silica fine powder, wherein the content of silica coarse powder is 70wt% and the content of silica fine powder is 50wt%. The binder is set to boric acid and urea, wherein the content of boric acid is 5wt% and the content of urea is 3wt%. Before sintering, the plasticity of the brick body can be enhanced in combination with boric acid and urea, that is, various raw materials can be bonded together to avoid cracking of the formed brick body due to low plasticity. In addition, boric acid and urea generate nano flaky boron carbide under high temperature environment, and the nano flaky boron carbide can increase the volume density of the blank product, further densify its internal structure, and thus improve the strength of the silica brick. The content of the composite mineralizer is 3wt%, and the composite mineralizer can be set to magnesium oxide, calcium oxide, silicon carbide, etc.

[0038] To prepare silica bricks using the above raw materials, it is necessary to follow the following preparation methods one by one. Step 1: Add appropriate amount of main raw materials, composite mineralizer and binder into the ball mill and mix them.

[0039] Step 2: Put the mixed powder prepared in step 1 into the molding equipment, and use the molding equipment to perform compression molding.

[0040] Step 3: The molded silica bricks manufactured in step 2 are dried in an environment of 60°C for 24 hours.

[0041] Step 4: The silica bricks dried in step 3 are pre-sintered at 400°C for 3 hours.

[0042] Step 5: The pre-sintered silicon bricks in step 4 are sintered at 1400°C for 5 hours.

[0043] Step 6: The silicon bricks sintered in step 5 are cooled to room temperature to obtain the product.

[0044] Example 5 A nano boron carbide reinforced high thermal conductivity dense silica brick comprises main raw materials, composite mineralizer, binder and the like. Specifically, the main raw materials are silica coarse powder and silica fine powder, wherein the content of silica coarse powder is 60wt% and the content of silica fine powder is 40wt%. The binder is boric acid and urea, wherein the content of boric acid is 3wt% and the content of urea is 2wt%. Before sintering, the plasticity of the brick body can be enhanced by the cooperation of boric acid and urea, that is, a variety of raw materials can be bonded together to avoid cracking of the formed brick body due to low plasticity. In addition, boric acid and urea generate nano flaky boron carbide under high temperature environment, and the nano flaky boron carbide can increase the volume density of the blank product, further densify its internal structure, and thus improve the strength of the silica brick. The content of the composite mineralizer is 2wt%, and the composite mineralizer can be magnesium oxide, calcium oxide, silicon carbide and the like.

[0045] To prepare silica bricks using the above raw materials, it is necessary to follow the following preparation methods one by one. Step 1: Add appropriate amount of main raw materials, composite mineralizer and binder into the ball mill and mix them.

[0046] Step 2: Put the mixed powder prepared in step 1 into the molding equipment, and use the molding equipment to perform compression molding.

[0047] Step 3: The molded silica bricks manufactured in step 2 are dried in an environment of 80°C for 36 hours.

[0048] Step 4: The dried silica bricks in step 3 are pre-sintered at 600°C for 5 hours.

[0049] Step 5: The pre-sintered silicon bricks in step 4 are sintered at 1500°C for 7 hours.

[0050] Step 6: The silicon bricks sintered in step 5 are cooled to room temperature to obtain the product.

[0051] Example 6 A nano boron carbide reinforced high thermal conductivity dense silica brick comprises main raw materials, composite mineralizer, binder and the like. Specifically, the main raw materials are silica coarse powder and silica fine powder, wherein the content of silica coarse powder is 50wt% and the content of silica fine powder is 45wt%. The binder is boric acid and urea, wherein the content of boric acid is 2wt% and the content of urea is 1wt%. Before sintering, the plasticity of the brick body can be enhanced by the cooperation of boric acid and urea, that is, a variety of raw materials can be bonded together to avoid cracking of the formed brick body due to low plasticity. In addition, boric acid and urea generate nano flaky boron carbide under high temperature environment, and the nano flaky boron carbide can increase the volume density of the blank product, further densify its internal structure, and thus improve the strength of the silica brick. The content of the composite mineralizer is 3wt%, and the composite mineralizer can be magnesium oxide, calcium oxide, silicon carbide and the like.

[0052] To prepare silica bricks using the above raw materials, it is necessary to follow the following preparation methods one by one. Step 1: Add appropriate amount of main raw materials, composite mineralizer and binder into the ball mill and mix them.

[0053] Step 2: Put the mixed powder prepared in step 1 into the molding equipment, and use the molding equipment to perform compression molding.

[0054] Step 3: The molded silica bricks manufactured in step 2 are dried in an environment of 70° C. for 40 hours.

[0055] Step 4: The silica bricks dried in step 3 are pre-sintered at 700°C for 5 hours.

[0056] Step 5: The pre-sintered silicon bricks in step 4 are sintered at 1600°C for 5 hours.

[0057] Step 6: The silicon bricks sintered in step 5 are cooled to room temperature to obtain the product.

[0058] Table sintered silicon brick physical and chemical indicators The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a nano boron carbide reinforced high thermal conductivity dense silicon brick, characterized in that: include Step 1: Add appropriate amount of main raw materials, composite mineralizer and binder into the ball mill and mix; Step 2: putting the mixed powder prepared in step 1 into a molding device and molding it by molding the mixed powder; Step 3: Dry the molded silica bricks manufactured in step 2 in an environment of 60-100°C for 24-48 hours; Step 4: The dried silica bricks in step 3 are pre-sintered at 400-800°C for 3-6h; Step 5: The pre-sintered silicon bricks in step 4 are sintered at 1400-1600°C for 5-8h; Step 6: The silicon bricks sintered in step 5 are cooled to room temperature to obtain the product.

2. The method for preparing a nano boron carbide reinforced high thermal conductivity dense silicon brick according to claim 1, characterized in that: In step 4, the pre-sintered silicon bricks generate nano-flaky boron carbide.

3. The method for preparing a nano boron carbide reinforced high thermal conductivity dense silicon brick according to claim 1, characterized in that: The main raw materials in step 1 are set to be silica coarse powder and silica fine powder, wherein the content of silica coarse powder is 40-70wt% and the content of silica fine powder is 30-50wt%.

4. The method for preparing a nano boron carbide reinforced high thermal conductivity dense silicon brick according to claim 1, characterized in that: The binder in step 1 is set to be boric acid and urea, wherein the boric acid content is 1-5wt% and the urea content is 1-3wt%.

5. The method for preparing a nano boron carbide reinforced high thermal conductivity dense silicon brick according to claim 4, characterized in that: Boric acid and urea generate nano-sheet boron carbide under high temperature.

6. The method for preparing a nano boron carbide reinforced high thermal conductivity dense silicon brick according to claim 1, characterized in that: The content of the composite mineralizer in step 1 is 1-3wt%, and the composite mineralizer can be magnesium oxide.

7. The method for preparing a nano boron carbide reinforced high thermal conductivity dense silicon brick according to claim 1, characterized in that: The content of the composite mineralizer in step 1 is 1-3wt%, and the composite mineralizer can be set to calcium oxide.

8. The method for preparing a nano boron carbide reinforced high thermal conductivity dense silicon brick according to claim 1, characterized in that: The content of the composite mineralizer in step 1 is 1-3wt%, and the composite mineralizer can be silicon carbide.

Citation Information

Patent Citations

  • Preparation method of long-service-life zero-expansion thermal-shock-resistant silicon brick

    CN111018502A

  • Toughness enhanced silicon-containing composite bodies, and methods for making same

    EP1438261A2

  • Material for infectious incinerating furnace

    JP1996121733A