Lithium metal composite negative electrode and preparation method thereof, lithium ion battery
By using three-dimensional skeleton materials doped with inorganic solid electrolytes in lithium-ion batteries, the problem of poor compatibility between lithium metal negative electrodes and electrolytes is solved through the combination technology of different particle sizes, and the electrochemical performance and safety of the battery are improved. , achieving more efficient lithium ion transmission and more stable cycling performance.
Patent Information
- Application Number
- CN202411083259.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-08
AI Technical Summary
The prior art is difficult to take into account the compatibility between the lithium metal negative electrode and the electrolyte in lithium-ion batteries, resulting in problems of lithium dendrites growing and volume expansion, affecting the safety and electrochemical performance of the battery.
Using three-dimensional framework materials doped with inorganic solid electrolytes, the inorganic solid electrolyte complexes with different particle sizes can form uniform electrolyte particle distribution, increase the contact area between the electrode and the electrolyte, optimize the lithium ion transmission channel, reduce interface polarization, and improve Material bulk density and cyclic properties.
The structural stability and safety of lithium metal negative electrodes are improved, the charging and discharging efficiency and cycling performance of lithium-ion batteries are improved, the risks of structural damage and active substances are reduced, and the mechanical properties of the batteries are enhanced.
Smart Images

Figure CN118658964B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of new energy technology, and in particular to a lithium metal composite negative electrode and a preparation method thereof, and a lithium ion battery. Background Art
[0002] Lithium metal anode is considered to be a key material for next-generation high-energy density batteries due to its high theoretical specific capacity and low electrode potential. However, lithium metal has problems with lithium dendrite growth and volume expansion in traditional liquid electrolytes, which may lead to battery short circuits and safety risks.
[0003] In the existing technology, strategies such as designing porous nanostructures, constructing artificial interface layers, using modified current collectors, and preparing composite negative electrodes can guide the uniform deposition of lithium, reduce the formation of dendrites, and improve the structural stability and safety of lithium metal negative electrodes. However, the existing technology is difficult to take into account the compatibility between the electrolyte and the lithium metal negative electrode, and the electrochemical performance needs to be further improved. Summary of the invention
[0004] The purpose of this application is to provide a lithium metal composite negative electrode and a preparation method thereof, and a lithium ion battery, aiming to solve the problems existing in the prior art.
[0005] To achieve the above objectives, the present application provides a lithium metal composite negative electrode, comprising:
[0006] current collector;
[0007] A three-dimensional skeleton material doped with an inorganic solid electrolyte coated on the surface of the current collector, such as Figure 1 As shown, the three-dimensional skeleton material is a porous structure, the inorganic solid electrolyte contains a tetravalent or higher titanium element, and the inorganic solid electrolyte includes an inorganic solid electrolyte of a first particle size and an inorganic solid electrolyte of a second particle size, and the second particle size is larger than the first particle size;
[0008] Lithium metal is composited on the surface of the three-dimensional skeleton material doped with the inorganic solid electrolyte.
[0009] Among them, the inorganic solid electrolyte of the first particle size can be an inorganic solid electrolyte of one particle size, or an inorganic solid electrolyte of two particle sizes, or an inorganic solid electrolyte of multiple particle sizes. The inorganic solid electrolyte of the second particle size can also be an inorganic solid electrolyte of one particle size, or an inorganic solid electrolyte of two particle sizes, or an inorganic solid electrolyte of multiple particle sizes. As long as the second particle size is greater than the first particle size, that is, the inorganic solid electrolytes of large and small particle sizes are compounded.
[0010] In some embodiments, the first particle size is greater than or equal to 100nm and less than 600nm, for example, it can be 100nm, 200nm, 300nm, 400nm, 500nm, 550nm or any value between greater than or equal to 100nm and less than 600nm; the second particle size is 600nm-2μm, for example, it can be 600nm, 700nm, 800nm, 900nm, 1μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm, 1.5μm, 1.6μm, 1.7μm, 1.8μm, 1.9μm, 2μm or any value between 600nm-2μm.
[0011] In some embodiments, the mass ratio of the inorganic solid electrolyte of the second particle size to the inorganic solid electrolyte of the first particle size is 1:2~4:1, for example, it can be 1:2, 1:1, 2:3, 2:1, 3:2, 4:1, or any value between 1:2~4:1.
[0012] In some embodiments, the inorganic solid electrolyte of the first particle size is distributed in the pores and on the outer surface of the three-dimensional skeleton material, and the inorganic solid electrolyte of the second particle size is distributed on the outer surface of the three-dimensional skeleton material;
[0013] There are van der Waals forces and chemical bonds between the inorganic solid electrolyte of the first particle size and the inorganic solid electrolyte of the second particle size.
[0014] In some embodiments, at least one of the following conditions is met:
[0015] A. The inorganic solid electrolyte is LATP and / or LLTO;
[0016] B. The particle size D50 of the three-dimensional framework material is 1 μm to 50 μm;
[0017] C. The specific surface area of the three-dimensional skeleton material is 10-1500 m 2 / g;
[0018] D. The three-dimensional skeleton material is one or more of polyaniline, polypyrrole, polythiophene, polyacetylene, phenolic resin, urea-formaldehyde resin, formaldehyde resin, furfural resin, and melamine resin;
[0019] E. The three-dimensional skeleton material contains a conductive agent, which includes one or more of SP, graphite, acetylene black, carbon nanotubes, graphene, Ketjen black, biomass hard carbon, and resin hard carbon; the content of the conductive agent is 5% to 30% of the mass of the three-dimensional skeleton material.
[0020] In some embodiments, at least one of the following conditions is met:
[0021] F. The particle size of the three-dimensional framework material doped with the inorganic solid electrolyte is 1 μm to 60 μm;
[0022] G. The specific surface area of the three-dimensional skeleton material doped with the inorganic solid electrolyte is 10 to 500 m 2 / g;
[0023] H. The pore size of the three-dimensional skeleton material doped with the inorganic solid electrolyte is 10-50 nm.
[0024] The present application also provides a method for preparing the above-mentioned lithium metal composite negative electrode, comprising:
[0025] Mixing an inorganic solid electrolyte of a first particle size and an inorganic solid electrolyte of a second particle size with a three-dimensional framework material to obtain a three-dimensional framework material doped with an inorganic solid electrolyte;
[0026] The three-dimensional skeleton material doped with the inorganic solid electrolyte is formulated into a slurry and coated on a current collector to obtain a three-dimensional skeleton material current collector compounded with an inorganic solid electrolyte;
[0027] The three-dimensional skeleton material current collector compounded with the inorganic solid electrolyte is compounded with lithium metal to obtain a lithium metal composite negative electrode.
[0028] In some embodiments, mixing an inorganic solid electrolyte of a first particle size and an inorganic solid electrolyte of a second particle size with a three-dimensional framework material comprises:
[0029] The inorganic solid electrolyte of the first particle size is first mixed with the three-dimensional framework material to obtain the three-dimensional framework material doped with the inorganic solid electrolyte of the first particle size;
[0030] Performing a second mixing of the three-dimensional skeleton material doped with the inorganic solid electrolyte of the first particle size and the inorganic solid electrolyte of the second particle size to obtain the three-dimensional skeleton material doped with the inorganic solid electrolyte;
[0031] The preparation method satisfies at least one of the following conditions:
[0032] a. The first mixing time is 30min-60min;
[0033] b. The second mixing time is 10min~60min;
[0034] c. the mass ratio of the second particle size inorganic solid electrolyte to the first particle size inorganic solid electrolyte is 1:2~4:1;
[0035] d. The mass ratio of the inorganic solid electrolyte to the three-dimensional framework material is 1:3~1:50;
[0036] e. The first mixing and the second mixing are independently selected from any one of direct mixing, VC mixing, wet mixing, and ball milling;
[0037] f. The inorganic solid electrolyte and the three-dimensional skeleton material account for 60% to 95% of the solid matter in the slurry;
[0038] g. The solid content of the slurry is 8% to 20%.
[0039] In some embodiments, the three-dimensional skeleton material doped with the inorganic solid electrolyte, a binder, a conductive agent, and a solvent are mixed to obtain a slurry.
[0040] In some embodiments, the binder is any one or more of polyvinylidene fluoride, polyacrylic acid, polyamide, LA133, polyvinyl alcohol, polyethyleneimine, polyimide, polyethylene, SBR (styrene-butadiene latex), and carboxymethyl cellulose; the binder accounts for 5% to 10% of the solid matter in the slurry.
[0041] In some embodiments, the conductive agent is selected from any one or more of SP (conductive carbon black), graphite, acetylene black, carbon nanotubes, graphene, and Ketjen black; the conductive agent accounts for 5% to 10% of the solid matter in the slurry.
[0042] In some embodiments, the solvent is any one of NMP (N-methylpyrrolidone), DMF (N,N-dimethylformamide), and water.
[0043] In some embodiments, the method for preparing the three-dimensional skeleton material comprises:
[0044] Monomer one, monomer two, a conductive agent and a dispersant are added into water to mix and dissolve, and a catalyst is added to adjust the pH value, and the three-dimensional skeleton material is obtained by reaction.
[0045] In some embodiments, the compounding method includes any one of cold rolling, hot rolling, calendering, and extrusion.
[0046] In some embodiments, the method for preparing the three-dimensional skeleton material satisfies at least one of the following conditions:
[0047] (1) The monomer 1 includes one or more of cresol, nonylphenol, urea, melamine, phenol, aralkylphenol, furfuryl alcohol, acrylic acid, phthalic acid, and aniline;
[0048] (2) The monomer II includes one or more of formaldehyde, pentamethylenediamine, propylene, acrylonitrile, methacrylic acid, acetaldehyde, and vinyl alcohol;
[0049] (3) The molar ratio of the monomer 2 to the monomer 1 is 0.2-2;
[0050] (4) The mass ratio of the water to the monomer is 5 to 500;
[0051] (5) The conductive agent includes one or more of SP, graphite, acetylene black, carbon nanotubes, graphene, Ketjen black, biomass hard carbon, and resin hard carbon;
[0052] (6) The mass ratio of the conductive agent to the monomer is 0.05-1;
[0053] (7) The dispersant includes any one of polyacrylate, polyvinyl ester, sodium tripolyphosphate, sodium pyrophosphate, sodium citrate, cellulose, polyvinyl pyrrolidone, polyvinyl alcohol, polycarboxylic acid, and ethanol;
[0054] (8) The catalyst is selected from one or more of hydrochloric acid, formic acid, ammonia water, sulfuric acid, oxalic acid, carbonic acid, citric acid, acetic acid, and sodium hydroxide;
[0055] (9) The pH range is 1 to 5;
[0056] (10) The reaction time of the three-dimensional skeleton material is 10-60 minutes.
[0057] The present application also provides a lithium-ion battery, comprising the above-mentioned lithium metal composite negative electrode.
[0058] Compared with the prior art, the beneficial effects of this application include:
[0059] The lithium metal composite negative electrode provided in the present application includes a current collector and a three-dimensional skeleton material coated on the surface of the current collector and lithium metal composited with the three-dimensional skeleton material. The three-dimensional skeleton material is doped with inorganic solid electrolytes of large and small particle sizes. After mixing with inorganic solid electrolytes with compounded particle sizes, the specific surface area of the three-dimensional skeleton material is reduced, and the external pores contain uniform inorganic solid electrolyte particles. After coating, it can be ensured that the three-dimensional skeleton material particles are filled with inorganic solid electrolytes of different particle sizes. Due to the different particle sizes of the inorganic solid electrolytes, the contact area between the electrode and the electrolyte can be increased after compounding, thereby improving the physical contact of the interface and facilitating the efficient transmission of electrons and ions.
[0060] At the same time, the compounding of large and small particle sizes can optimize the lithium ion transmission channel in the inorganic solid electrolyte, reduce the pores between the three-dimensional skeleton materials, improve the ion mobility, reduce the interface polarization, and improve the battery's charge and discharge efficiency. In addition, since the inorganic solid electrolyte reacts with lithium metal to form a solid electrolyte interface layer, through the compounding of large and small particle sizes, during the compounding process, the smaller particles can be filled into the gaps between the larger particles, increasing the packing density of the material, shortening the lithium ion transmission path, and thus improving the mechanical properties of the material and the cycle performance of the battery, avoiding the shedding of active substances due to structural damage during the charge and discharge process, affecting the battery's cycle performance and safety. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0062] Figure 1 A schematic diagram of a three-dimensional skeleton material electrode and ion transport doped with an inorganic solid electrolyte of the present application;
[0063] Figure 2 This is a SEM image of the three-dimensional skeleton material of the inorganic solid electrolyte with large and small particle sizes as in Example 2;
[0064] Figure 3 This is the SEM image of the porous carbon three-dimensional framework material of Example 5;
[0065] Figure 4 The full battery cycle performance results of Examples 1 to 4 are shown;
[0066] Figure 5 This is a comparison diagram of the full battery cycle performance of Example 2 and Example 5;
[0067] Figure 6 The figure is a comparison result of the full battery cycle performance of Example 1, Comparative Example 1 and Comparative Example 2;
[0068] Figure 7 This is a comparison chart of the full battery cycle performance of Example 4 and Comparative Example 3. DETAILED DESCRIPTION
[0069] As used herein:
[0070] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0071] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0072] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0073] In these examples, parts and percentages are by mass unless otherwise indicated.
[0074] "Mass parts" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass parts of component A are a parts and the mass parts of component B are b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass parts of all components is not limited to 100 parts.
[0075] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0076] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0077] Example 1
[0078] Dissolve 200g melamine and 245g formaldehyde in 1L water, stir until completely dissolved, then add 15g SP and 40g polyvinyl pyrrolidone and stir until the solid matter is completely dissolved and then ultrasonically disperse for 30min. Then add a certain amount of citric acid to adjust the pH to 3, and stir for another 1h. After stirring, let it stand for 24h and separate the solid and liquid, wash until neutral, and dry to obtain a three-dimensional skeleton material. The specific surface of the three-dimensional skeleton material measured by BET is 110.3m 2 / g.
[0079] 30g of three-dimensional skeleton material and 2.14g of 300nm small-particle inorganic solid electrolyte (LATP) material were dissolved in an appropriate amount of ethanol and stirred for 30min, then filtered, washed and dried to obtain a three-dimensional skeleton material doped with a small-particle inorganic solid electrolyte. The dried three-dimensional skeleton material doped with a small-particle inorganic solid electrolyte and 2.14g of 600nm large-particle inorganic solid electrolyte (LATP) VC were mixed for 30min at a speed of 70r / min to obtain a three-dimensional skeleton material with a large-particle inorganic solid electrolyte. The BET measured the specific surface area of the material to be 108m 2 / g, Malvern measured the particle size of the material as D50=31.5μm.
[0080] The three-dimensional skeleton material of the inorganic solid electrolyte with large and small particle sizes, SP and 5% LA133 were mixed in a mass ratio of 80:10:10, and an appropriate amount of water was added to prepare a slurry in a degassing machine. Then the slurry was coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 46μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0081] Example 2
[0082] Dissolve 98g urea and 132g formaldehyde in 800mL water, stir until completely dissolved, then add 10g SP and 20g polyvinyl pyrrolidone and stir until the solid matter is completely dissolved, then ultrasonically disperse for 30min, then add a certain amount of hydrochloric acid to adjust the pH to 4, and stir for another hour. After stirring, let it stand for 24h and separate the solid and liquid, wash until neutral, and dry to obtain a three-dimensional skeleton material.
[0083] Dissolve 10g of three-dimensional skeleton material and 0.3g of 200nm and 0.77g of 300nm small-particle inorganic solid electrolyte (LATP) material in an appropriate amount of water and stir for 30min, then filter, wash and dry to obtain a three-dimensional skeleton material doped with a small-particle inorganic solid electrolyte. Mix the dried three-dimensional skeleton material doped with a small-particle inorganic solid electrolyte and 1.23g of 600nm large-particle inorganic solid electrolyte (LATP) VC for 30min at a speed of 70r / min to obtain a three-dimensional skeleton material with a large-particle inorganic solid electrolyte. Its SEM image is as follows: Figure 2 As shown, the BET measured the specific surface area of the material to be 95.2m 2 / g, Malvern measured the particle size of the material as D50=26.5μm.
[0084] The three-dimensional skeleton material, SP, carbon nanotubes, CMC, and SBR of the large and small particle size inorganic solid electrolyte were mixed in a mass ratio of 83.7:9.5:0.5:1.3:5, and an appropriate amount of water was added to prepare the slurry in a degassing machine. Then the slurry was coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 46μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, and 1MLiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0085] Example 3
[0086] Dissolve 120g urea and 324g formaldehyde in 1.5L water, stir until completely dissolved, then add 18g carbon nanotubes and 36g cellulose and stir until the solid matter is completely dissolved, then ultrasonically disperse for 30min, then add a certain amount of hydrochloric acid to adjust the pH to 3, and stir for another hour. After stirring, let it stand for 24h and separate the solid and liquid, wash until neutral, and dry to obtain a three-dimensional skeleton material.
[0087] Dissolve 30g of three-dimensional skeleton material and 1.2g of 200nm and 1.2g of 300nm small-particle inorganic solid electrolyte (LATP) material in an appropriate amount of water, add an appropriate amount of polyvinyl pyrrolidone and stir for 30min, then filter, wash and dry to obtain a three-dimensional skeleton material doped with a small-particle inorganic solid electrolyte. Mix the dried three-dimensional skeleton material doped with a small-particle inorganic solid electrolyte and 1.6g of 600nm and 2g of 1μm large-particle inorganic solid electrolyte (LATP) VC for 60min at a speed of 60r / min to obtain a three-dimensional skeleton material with a large-particle inorganic solid electrolyte. The BET measured the specific surface area of the material to be 71m 2 / g, Malvern measured the particle size of the material as D50 = 22.6μm.
[0088] The three-dimensional skeleton material, SP, CMC, and SBR of the large and small particle size inorganic solid electrolyte were mixed in a mass ratio of 83.7:10:1.3:5, and an appropriate amount of water was added to prepare the slurry in a degassing machine. Then the slurry was coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 46μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, and 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0089] Example 4
[0090] The same scheme as in Example 2 was used to prepare the three-dimensional skeleton material.
[0091] Dissolve 20g of three-dimensional framework material and 0.57g of 300nm small-particle inorganic solid electrolyte (LATP) material in an appropriate amount of water, add an appropriate amount of polyvinyl pyrrolidone and stir for 30min, then filter, wash and dry to obtain a three-dimensional framework material doped with a small-particle inorganic solid electrolyte. Mix the dried three-dimensional framework material doped with a small-particle inorganic solid electrolyte and 0.857g of 600nm and 1.43g of 1μm large-particle inorganic solid electrolyte (LATP) VC for 30min at a speed of 70r / min to obtain a three-dimensional framework material with a large-particle inorganic solid electrolyte.
[0092] The three-dimensional skeleton material of the inorganic solid electrolyte with large and small particle sizes, SP, carbon nanotubes and 5% LA133 were mixed in a mass ratio of 80:9.5:0.5:10, and an appropriate amount of water was added to prepare a slurry in a degassing machine. Then the slurry was coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 46μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0093] Example 5
[0094] The existing commercially available porous carbon is used as the three-dimensional skeleton material, and its SEM image is as follows Figure 3 shown.
[0095] Dissolve 10g of porous carbon three-dimensional framework material and 0.3g of 200nm and 0.77g of 300nm small-particle inorganic solid electrolyte (LATP) material in an appropriate amount of water and stir for 30min, then filter, wash and dry to obtain a three-dimensional framework material doped with a small-particle inorganic solid electrolyte. Mix the dried three-dimensional framework material doped with a small-particle inorganic solid electrolyte and 1.23g of 600nm large-particle inorganic solid electrolyte (LATP) VC for 30min at a speed of 70r / min to obtain a three-dimensional framework material with a large-particle inorganic solid electrolyte.
[0096] The three-dimensional skeleton material of the inorganic solid electrolyte with large and small particle sizes, SP and 5% LA133 were mixed in a mass ratio of 90:5:5, and an appropriate amount of water was added to prepare a slurry in a degassing machine. Then the slurry was coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 46μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was carried out on it.
[0097] Example 6
[0098] The three-dimensional skeleton material was prepared using the same scheme as in Example 3.
[0099] Dissolve 20g of three-dimensional skeleton material and 1.54g of 200nm and 1.54g of 500nm small-particle inorganic solid electrolyte (LATP) materials in an appropriate amount of water, add an appropriate amount of polyvinyl pyrrolidone and stir for 30 minutes, then filter, wash and dry to obtain a three-dimensional skeleton material doped with a small-particle inorganic solid electrolyte. Mix the dried three-dimensional skeleton material doped with a small-particle inorganic solid electrolyte and 1.54g of 1μm large-particle inorganic solid electrolyte (LATP) VC for 30 minutes at a speed of 60r / min to obtain a three-dimensional skeleton material with a large-particle inorganic solid electrolyte.
[0100] The three-dimensional skeleton material, SP, CMC, and SBR of the large and small particle size inorganic solid electrolyte were mixed in a mass ratio of 83.7:10:1.3:5, and an appropriate amount of water was added to prepare the slurry in a degassing machine. Then the slurry was coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 46μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, and 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0101] Example 7
[0102] The three-dimensional skeleton material was prepared using the same scheme as in Example 1.
[0103] 20g of the three-dimensional skeleton material and 0.57g of 200nm small-particle inorganic solid electrolyte (LLTO) material VC were mixed for 30min at a speed of 90r / min to obtain a three-dimensional skeleton material doped with a small-particle inorganic solid electrolyte. The dried three-dimensional skeleton material doped with a small-particle inorganic solid electrolyte and 2.28g of 600nm large-particle inorganic solid electrolyte (LLTO) VC were mixed for 30min at a speed of 60r / min to obtain a three-dimensional skeleton material with a large-particle inorganic solid electrolyte.
[0104] The three-dimensional skeleton material, SP, CMC, and SBR of the large and small particle size inorganic solid electrolyte were mixed in a mass ratio of 83.7:10:1.3:5, and an appropriate amount of water was added to prepare the slurry in a degassing machine. Then the slurry was coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 46μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, and 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0105] Comparative Example 1
[0106] The same scheme as in Example 2 was used to prepare the three-dimensional skeleton material.
[0107] 15g of three-dimensional framework material and 2.14g of 200nm small-particle inorganic solid electrolyte (LATP) material were dissolved in a proper amount of water and stirred for 30min, then filtered, washed and dried to obtain a three-dimensional framework material doped with a small-particle inorganic solid electrolyte.
[0108] The three-dimensional skeleton material doped with small-particle inorganic solid electrolyte, SP and 5% LA133 were mixed in a mass ratio of 80:10:10, and an appropriate amount of water was added to prepare a slurry in a degassing machine. The slurry was then coated on a copper foil with a scraper, and after it dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 46μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0109] Comparative Example 2
[0110] The same scheme as in Example 2 was used to prepare the three-dimensional skeleton material.
[0111] 15g of three-dimensional framework material and 2.14g of 600nm large-particle inorganic solid electrolyte (LATP) material were dissolved in a proper amount of water and stirred for 30min, then filtered, washed and dried to obtain a three-dimensional framework material doped with a large-particle inorganic solid electrolyte.
[0112] The three-dimensional skeleton material doped with large-particle inorganic solid electrolyte, SP, carbon nanotubes and 5% LA133 were mixed in a mass ratio of 80:9.5:0.5:10, and an appropriate amount of water was added to prepare a slurry in a degassing machine. The slurry was then coated on a copper foil with a scraper, and after it dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 46μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0113] Comparative Example 3
[0114] The three-dimensional skeleton material was prepared using the same scheme as in Example 3.
[0115] Dissolve 20g of three-dimensional skeleton material and 2.28g of 300nm small-particle inorganic solid electrolyte (LATP) material in an appropriate amount of water, add an appropriate amount of polyvinyl pyrrolidone and stir for 30min, then filter, wash and dry to obtain a three-dimensional skeleton material doped with a small-particle inorganic solid electrolyte. Mix the dried three-dimensional skeleton material doped with a small-particle inorganic solid electrolyte and 0.57g of 600nm large-particle inorganic solid electrolyte (LATP) VC for 30min at a speed of 60r / min to obtain a three-dimensional skeleton material with a large-particle inorganic solid electrolyte.
[0116] The three-dimensional skeleton material of the inorganic solid electrolyte with large and small particle sizes, SP and 5% LA133 were mixed in a mass ratio of 80:10:10, and an appropriate amount of water was added to prepare a slurry in a degassing machine. Then the slurry was coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 46μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was carried out on it.
[0117] Comparative Example 4
[0118] The three-dimensional skeleton material was prepared using the same scheme as in Example 1.
[0119] 15g of the three-dimensional skeleton material and 0.6g of 300nm small-particle inorganic solid electrolyte (LLZTO) material VC were mixed for 30min at a speed of 80r / min to obtain a three-dimensional skeleton material doped with a small-particle inorganic solid electrolyte. The dried three-dimensional skeleton material doped with a small-particle inorganic solid electrolyte and 0.4g of 600nm large-particle inorganic solid electrolyte (LLZTO) VC were mixed for 30min at a speed of 60r / min to obtain a three-dimensional skeleton material with a large-particle inorganic solid electrolyte.
[0120] The three-dimensional skeleton material of the inorganic solid electrolyte with large and small particle sizes, SP, carbon nanotubes and 5% LA133 were mixed in a mass ratio of 80:9.5:0.5:10, and an appropriate amount of water was added to prepare a slurry in a degassing machine. Then the slurry was coated on the copper foil with a scraper, and after it was dried, a lithium foil with a thickness of 20μm was rolled onto the pole piece. The total thickness of the pole piece measured by a micrometer was 46μm. The pole piece was cut into a disc with a diameter of 12mm as the negative electrode, and a button-type full battery was assembled with an NCM with a diameter of 8.4mm as the positive electrode, 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 as the electrolyte, and the charge and discharge test was performed on it.
[0121] The three-dimensional skeleton materials doped with inorganic solid electrolytes obtained in the above embodiments and comparative examples were tested for specific surface area and pore size distribution using a Gaobo BK300C specific surface area meter and an American Mack TriStar-3030 pore size analyzer, and the particle size range of the samples was tested using a Malvern 3000 laser particle size analyzer. The surface, cross-section SEM and element distribution of the samples were tested using a Zeiss SEM 460 thermal field emission scanning electron microscope and an Oxford Ultim Max170 energy spectrometer. The electrochemical properties of the samples were tested using a Blue Electric M340A test cabinet, and the battery assembly was carried out in a German Braun glove box.
[0122] The specific button-type full battery is prepared by a method known in the art: NCM polycrystal is used as the positive electrode, the above-mentioned three-dimensional skeleton material pole piece with large and small particle size inorganic solid electrolyte is used as the negative electrode, 1M LiTFSI+DOL / DME (v / v=1:1)+2wt% LiNO3 is used as the electrolyte, Celgard2400 is used as the diaphragm, and the shell adopts a 2016 button-type battery shell to assemble the button-type full battery. The test conditions are: at room temperature, first use 0.05C constant rate charge and discharge for two weeks, the voltage range is 2.75-4.2V, and then use 1C / 5C charge and discharge system for cycling. The designed gram capacity of the three-dimensional skeleton material pole piece with large and small particle size inorganic solid electrolyte in all embodiments and comparative examples is greater than 2000mAh / g.
[0123] The test results are shown in Table 1. Figures 4 to 7 shown.
[0124] Table 1 Full battery capacity retention rate and pole piece expansion rate after cycling of the embodiments and comparative examples
[0125]
[0126] From Table 1, Figure 1 and Figure 4 It can be seen that the combination of inorganic solid electrolytes with different particle sizes can optimize the transmission path of lithium ions, reduce the circuitous transmission of lithium ions in the electrode material, and improve the rate performance. When the mass ratio of inorganic solid electrolytes with large and small particle sizes is increased from 1:1 (Example 1) to 4:1 (Example 4), and the types of inorganic solid electrolytes with large and small particle sizes are increased from 2 to 3 or 4, the capacity retention rate of the full battery after 200 cycles can reach more than 90%.
[0127] This is because when the content of large-particle inorganic solid electrolyte increases or the particle size types of solid electrolyte are more, the agglomeration between the three-dimensional skeleton materials can be reduced, and a uniform filling can be formed between the three-dimensional skeleton materials, thereby improving the conductivity of ions during the cycle. Moreover, as the electrolyte infiltration and circulation proceed, this uniform filling can avoid the appearance of gaps between the electrode materials and the shedding of active substances, thereby improving the cycle performance of the battery.
[0128] Depend on Figure 5 It can be seen that the whole battery can be cycled for more than 200 cycles by using different three-dimensional skeleton materials for particle size compounding. This shows that for different porous materials, the use of inorganic solid electrolytes with various particle sizes for compounding can improve the pore structure of the electrode material and facilitate the rapid diffusion of lithium ions in the material. However, due to the difference in the structure of the three-dimensional skeleton material, the expansion rate of the electrode after the cycle is different.
[0129] Depend on Figure 6 and Figure 7 It can be seen that the use of inorganic solid electrolytes with a single particle size or inorganic solid electrolytes with inappropriate compounding ratios will affect the cycle performance of the battery. This is because too small a particle size will increase the contact area between the electrolyte and the electrode, resulting in more solid electrolytes being required to achieve better cycle effects, thereby increasing production costs. In addition, small-particle inorganic solid electrolyte materials are prone to agglomeration, which will affect their dispersibility and interface impedance in the composite material and affect the overall performance of the battery. Large-particle inorganic solid electrolyte materials have a smaller specific surface area, which reduces the contact area between the electrolyte and the electrode, and large-particle inorganic solid electrolytes will also lead to the formation of more voids during the material composite process, affecting the transmission efficiency of lithium ions.
[0130] When the ratio of large and small particle size inorganic solid electrolytes is not appropriate, the composite material may have more voids, affecting the stability of the electrode material during the cycle; it may also cause the solid electrolyte material to be unevenly distributed, unable to form a uniform and continuous ion transmission path, affecting the battery's cycle performance. If there are too few large particle size inorganic solid electrolytes, the large and small particles are not tightly connected, and some ion channels on the three-dimensional skeleton material may not be connected; if there are more large particle size inorganic solid electrolytes, the voids are filled with small particle size inorganic solid electrolytes, which can ensure more available ion channels.
[0131] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0132] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A lithium metal composite negative electrode, characterized in that: include: current collector; A three-dimensional skeleton material doped with an inorganic solid electrolyte coated on the surface of the current collector, wherein the three-dimensional skeleton material is a porous structure, the inorganic solid electrolyte contains a titanium element with a valence of four or more, the inorganic solid electrolyte comprises an inorganic solid electrolyte of a first particle size and an inorganic solid electrolyte of a second particle size, the second particle size being larger than the first particle size; the first particle size is greater than or equal to 100 nm and less than 600 nm, and the second particle size is 600 nm-2 μm; the mass ratio of the inorganic solid electrolyte of the second particle size to the inorganic solid electrolyte of the first particle size is 1:1-4:1; the inorganic solid electrolyte of the first particle size is distributed in the pores and on the outer surface of the three-dimensional skeleton material, and the inorganic solid electrolyte of the second particle size is distributed on the outer surface of the three-dimensional skeleton material; there is a van der Waals force and a chemical bond between the inorganic solid electrolyte of the first particle size and the inorganic solid electrolyte of the second particle size; the inorganic solid electrolyte is LATP and / or LLTO; Lithium metal is composited on the surface of the three-dimensional skeleton material doped with the inorganic solid electrolyte.
2. The lithium metal composite negative electrode according to claim 1, characterized in that At least one of the following conditions is met: A. The particle size D50 of the three-dimensional framework material is 1 μm to 50 μm; B. The specific surface area of the three-dimensional skeleton material is 10-1500 m 2 / g; C. The three-dimensional skeleton material is one or more of polyaniline, polypyrrole, polythiophene, polyacetylene, phenolic resin, urea-formaldehyde resin, formaldehyde resin, furfural resin, and melamine resin; D. The three-dimensional skeleton material contains a conductive agent, and the content of the conductive agent is 5% to 30% of the mass of the three-dimensional skeleton material.
3. The lithium metal composite negative electrode according to claim 1, characterized in that At least one of the following conditions is met: F. The particle size of the three-dimensional framework material doped with the inorganic solid electrolyte is 1 μm to 60 μm; G. The specific surface area of the three-dimensional skeleton material doped with the inorganic solid electrolyte is 10 to 500 m 2 / g; H. The pore size of the three-dimensional skeleton material doped with the inorganic solid electrolyte is 10-50 nm.
4. A method for preparing a lithium metal composite negative electrode according to any one of claims 1 to 3, characterized in that: include: Mixing an inorganic solid electrolyte of a first particle size and an inorganic solid electrolyte of a second particle size with a three-dimensional framework material to obtain a three-dimensional framework material doped with an inorganic solid electrolyte; The three-dimensional skeleton material doped with the inorganic solid electrolyte is formulated into a slurry and coated on a current collector to obtain a three-dimensional skeleton material current collector compounded with an inorganic solid electrolyte; The three-dimensional skeleton material current collector compounded with the inorganic solid electrolyte is compounded with lithium metal to obtain a lithium metal composite negative electrode.
5. The method for preparing a lithium metal composite negative electrode according to claim 4, characterized in that: Mixing an inorganic solid electrolyte having a first particle size and an inorganic solid electrolyte having a second particle size with a three-dimensional framework material comprises: The inorganic solid electrolyte of the first particle size is first mixed with the three-dimensional framework material to obtain the three-dimensional framework material doped with the inorganic solid electrolyte of the first particle size; Performing a second mixing of the three-dimensional skeleton material doped with the inorganic solid electrolyte of the first particle size and the inorganic solid electrolyte of the second particle size to obtain the three-dimensional skeleton material doped with the inorganic solid electrolyte; The preparation method satisfies at least one of the following conditions: a. The first mixing time is 30min-60min; b. The second mixing time is 10min~60min; c. the mass ratio of the second particle size of the inorganic solid electrolyte to the first particle size of the inorganic solid electrolyte is 1:1~4:1; d. The mass ratio of the inorganic solid electrolyte to the three-dimensional framework material is 1:3~1:50; e. The first mixing and the second mixing are independently selected from any one of direct mixing, VC mixing, wet mixing, and ball milling; f. The inorganic solid electrolyte and the three-dimensional skeleton material account for 60% to 95% of the solid matter in the slurry; g. The solid content of the slurry is 8% to 20%.
6. The method for preparing a lithium metal composite negative electrode according to claim 4, characterized in that: The preparation method of the three-dimensional skeleton material comprises: Adding monomer 1, monomer 2, a conductive agent and a dispersant into water to mix and dissolve, adding a catalyst to adjust the pH, and reacting to obtain a three-dimensional skeleton material; The preparation method of the three-dimensional skeleton material meets at least one of the following conditions: (1) The monomer 1 includes one or more of cresol, nonylphenol, urea, melamine, phenol, aralkylphenol, furfuryl alcohol, acrylic acid, phthalic acid, and aniline; (2) The monomer II includes one or more of formaldehyde, pentamethylenediamine, propylene, acrylonitrile, methacrylic acid, acetaldehyde, and vinyl alcohol; (3) The molar ratio of the monomer 2 to the monomer 1 is 0.2-2; (4) The mass ratio of the water to the monomer is 5 to 500; (5) The conductive agent includes one or more of SP, graphite, acetylene black, carbon nanotubes, graphene, Ketjen black, biomass hard carbon, and resin hard carbon; (6) The mass ratio of the conductive agent to the monomer is 0.05-1; (7) The dispersant includes any one of polyacrylate, polyvinyl ester, sodium tripolyphosphate, sodium pyrophosphate, sodium citrate, cellulose, polyvinyl pyrrolidone, polyvinyl alcohol, polycarboxylic acid, and ethanol; (8) The catalyst is selected from one or more of hydrochloric acid, formic acid, ammonia water, sulfuric acid, oxalic acid, carbonic acid, citric acid, acetic acid, and sodium hydroxide; (9) The pH range is 1 to 5; (10) The reaction time of the three-dimensional skeleton material is 10-60 minutes.
7. A lithium ion battery, characterized in that: The invention comprises the lithium metal composite negative electrode as claimed in any one of claims 1 to 3.
Citation Information
Cited By
Three-dimensional polymer-based composite material for lithium metal battery and preparation method of three-dimensional polymer-based composite material
CN121331776A