Monomer simultaneously containing tri-quaternary ammonium salt ions and trivinyl benzene structure, preparation method and application of monomer, anion exchange resin and preparation method and application of anion exchange resin

By preparing monomers containing both triquaternary ammonium ions and trivinylbenzene structures in the anion exchange resin, the problem of difficulty in the synergistic introduction of multiple quaternary ammonium ions and vinylbenzene structures in the existing technology is solved, and high cross-linking is achieved. Anion exchange resin with high density and high ion exchange capacity, suitable for environmental protection and new energy fields.

CN118771990AActive Publication Date: 2024-10-15SHANDONG XINGSHUN NEW MATERIAL JOINT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410749013.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-15
Estimated Expiration
2044-06-11

AI Technical Summary

Technical Problem

It is difficult to prepare monomers containing multiple quaternary ammonium ions and multiple vinyl benzene structures simultaneously with the existing technology, which limits the cross-linking density and ion exchange capacity of anion exchange resins, affecting its use in environmentally friendly water treatment, new energy batteries and other fields. application.

Method used

By performing a quaternization reaction between tris(N,N-dimethylaminopropyl)amine and p-chloromethylstyrene in a polar organic solvent, a structural monomer containing both triquaternary ammonium salt ions and trivinylbenzene was prepared. The anion exchange resin with high cross-linking density and high ion exchange capacity is prepared through free radical polymerization initiated by the initiator.

Benefits of technology

It achieves high cross-linking density and high ion exchange capacity of anion exchange resin, simplifies the synthesis process, improves yield and lowers production cost, is suitable for industrial production, and has great application in the fields of water treatment, electrolyte, material purification and oil extraction. important application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771990A_ABST
    Figure CN118771990A_ABST
Patent Text Reader

Abstract

The invention provides a monomer simultaneously containing tri-quaternary ammonium salt ions and a trivinyl benzene structure, a preparation method and application of the monomer, anion exchange resin and a preparation method and application of the anion exchange resin, and relates to the technical field of ion exchange resin. The monomer provided by the invention simultaneously contains tri-quaternary ammonium salt ions and a trivinyl benzene structure, has very high reaction activity, and can be subjected to free radical polymerization under the initiation of an initiator to prepare anion exchange resin, and three active styrene in the monomer structure endows the anion exchange membrane resin with high crosslinking density, so that the anion exchange membrane resin has high cross-linking strength. The three quaternary ammonium salt ion structures ensure that the prepared anion exchange resin has high ion exchange capacity, and the prepared anion exchange resin has important potential application value in the fields of environmental protection, new energy and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ion exchange resins, and in particular to a monomer containing triquaternary ammonium salt ions and trivinylbenzene structures, a preparation method and application thereof, and an anion exchange resin, a preparation method and application thereof. Background Art

[0002] Anion exchange resin is an important functional polymer material with important application value in environmental water treatment, new energy battery electrolyte, natural drug purification, oil extraction and other fields. Ionized vinylbenzene monomer is a key monomer for the preparation of anion exchange resin. This type of monomer can be prepared by free radical polymerization under the action of an initiator to obtain the corresponding anion exchange resin.

[0003] Quaternary ammonium salt-type vinylbenzene monomers are an important component of ionized vinylbenzene monomers. The quaternary ammonium salt-type vinylbenzene monomers reported so far usually contain only one quaternary ammonium ion and one active vinylbenzene structure, such as (4-vinylbenzyl)trimethylammonium chloride, 1-(p-vinylbenzyl)-1-methylpiperidinium chloride, etc. Due to the difficulty in the synthesis process, there are few reports of monomers containing two or more quaternary ammonium ions and vinylbenzene structures at the same time, and the synergistic introduction of multiple vinylbenzenes and quaternary ammonium ions can further increase the ion exchange capacity of the resin while increasing the cross-linking density of the corresponding anion exchange resin. Therefore, the design and preparation of ionized monomers containing multiple quaternary ammonium ions and multiple vinylbenzene structures at the same time has important academic research and practical application value. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a monomer containing triquaternary ammonium salt ions and trivinylbenzene structures at the same time, and a preparation method and application thereof, an anion exchange resin and a preparation method and application thereof. The present invention provides a monomer containing triquaternary ammonium salt ions and trivinylbenzene structures at the same time, and the synthesis process is convenient and has a high yield. The monomer can be initiated by an initiator and free radical polymerization to prepare an anion exchange resin with high crosslinking density and high ion exchange capacity.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a monomer containing triquaternary ammonium salt ions and trivinylbenzene structure, which has a structure shown in Formula I:

[0007]

[0008] The present invention provides a method for preparing a monomer containing triquaternary ammonium salt ions and trivinylbenzene structures as described in the above technical solution, comprising the following steps:

[0009] The tri(N,N-dimethylaminopropyl)amine, p-chloromethylstyrene and a polar organic solvent are mixed and subjected to a quaternization reaction to obtain the monomer containing both triquaternary ammonium salt ions and trivinylbenzene structures.

[0010] Preferably, the molar ratio of tris(N,N-dimethylaminopropyl)amine to p-chloromethylstyrene is 1:3-4;

[0011] The polar organic solvent includes at least one of N-methylpyrrolidone, N,N-dimethylacetamide and N,N-dimethylformamide.

[0012] Preferably, the temperature of the quaternization reaction is 40-60° C., and the time is 1-3 hours.

[0013] The present invention provides the use of the monomer containing triquaternary ammonium salt ions and trivinylbenzene structures at the same time as described in the above technical solution or the monomer containing triquaternary ammonium salt ions and trivinylbenzene structures at the same time as described in the above technical solution prepared by the preparation method in preparing anion exchange resin.

[0014] The invention provides an anion exchange resin, wherein the preparation raw materials include a vinyl monomer, an initiator and a solvent; the vinyl monomer includes the monomer containing triquaternary ammonium salt ions and trivinylbenzene structures as described in the above technical scheme or the monomer containing triquaternary ammonium salt ions and trivinylbenzene structures as prepared by the preparation method as described in the above technical scheme.

[0015] Preferably, the vinyl monomer further comprises other water-soluble vinyl monomers;

[0016] The other water-soluble vinyl monomers include at least one of N-hydroxyacrylamide, acrylamide, acrylic acid and N-vinyl-2-pyrrolidone; the mass ratio of the monomer containing triquaternary ammonium salt ions and trivinylbenzene structure to the other water-soluble vinyl monomers is 1.1 to 9:1;

[0017] The mass of the initiator is 1-2% of the mass of the ethylene monomer;

[0018] The solvent includes water.

[0019] The present invention provides a method for preparing the anion exchange resin described in the above technical solution, comprising the following steps: mixing a vinyl monomer, an initiator and a solvent, and performing a free radical polymerization reaction to obtain the anion exchange resin.

[0020] Preferably, the temperature of the free radical polymerization reaction is 80-90° C., and the time is 0.5-1.5 h.

[0021] The present invention provides the use of the anion exchange resin described in the above technical solution or the anion exchange resin prepared by the preparation method described in the above technical solution in water treatment, electrolyte, material purification or oil extraction.

[0022] The monomer having a structure shown in Formula I and containing triquaternary ammonium salt ions and trivinylbenzene structures provided by the present invention contains triquaternary ammonium salt ions and trivinylbenzene structures at the same time and has high reactivity. The ionized vinylbenzene monomer can be subjected to free radical polymerization under the initiation of an initiator to prepare anion exchange resin. The three active styrenes in the monomer structure give the anion exchange membrane resin a high crosslinking density. The three quaternary ammonium salt ion structures ensure that the prepared anion exchange resin has a high ion exchange capacity. The anion exchange resin has important potential application value in the fields of environmental protection, new energy, etc.

[0023] The method for preparing a monomer containing triquaternary ammonium salt ions and trivinylbenzene structures provided by the invention has the advantages of simple synthesis process, simple operation, high product yield, easy separation, low production cost, green environmental protection and suitability for industrial production.

[0024] The anion exchange resin provided by the present invention has high cross-linking density and high ion exchange capacity, and has important potential application value in environmental protection and new energy fields such as water treatment, electrolytes, material purification, and oil extraction.

[0025] The preparation method of the anion exchange resin provided by the invention has simple process, simple operation, high product yield, easy separation, low production cost, green and environmental protection, and is suitable for industrial production.

[0026] Furthermore, the present invention introduces other water-soluble vinyl monomers into the anion exchange resin to prepare an anion exchange resin with a high cross-linking density and adjustable ion exchange capacity through free radical polymerization. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The tris(4-vinylbenzyl-N,N-dimethylmethylammonium chloride-tripropyl)amine prepared in Example 1 1 HNMR spectrum.

[0028] Figure 2 This is the infrared spectrum of tri(4-vinylbenzyl-N,N-dimethylmethylammonium chloride-tripropyl)amine prepared in Example 1. DETAILED DESCRIPTION

[0029] The present invention provides a monomer containing triquaternary ammonium salt ions and trivinylbenzene structure, the chemical name of which is tri(4-vinylbenzyl-N,N-dimethylmethylammonium chloride-tripropyl)amine, and has a structure shown in Formula I:

[0030]

[0031] In the present invention, the melting point of the monomer containing both triquaternary ammonium salt ions and trivinylbenzene structures is preferably 220-221°C.

[0032] The invention provides a method for preparing a monomer containing triquaternary ammonium salt ions and trivinylbenzene structures at the same time as described in the technical scheme, comprising the following steps: mixing tri(N,N-dimethylaminopropyl)amine, p-chloromethylstyrene and a polar organic solvent, and performing a quaternization reaction to obtain the monomer containing triquaternary ammonium salt ions and trivinylbenzene structures at the same time.

[0033] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.

[0034] In the present invention, the preparation route of the monomer containing both triquaternary ammonium salt ions and trivinylbenzene structure is as follows:

[0035]

[0036] In the present invention, the molar ratio of tris(N,N-dimethylaminopropyl)amine to p-chloromethylstyrene is preferably 1:3-4, more preferably 1:3.2-3.8, and further preferably 1:3.4-3.5.

[0037] In the present invention, the polar organic solvent preferably includes at least one of N-methylpyrrolidone, N,N-dimethylacetamide and N,N-dimethylformamide. In the present invention, the mass of the polar organic solvent is preferably 2 to 4 times the total mass of tris(N,N-dimethylaminopropyl)amine and p-chloromethylstyrene, more preferably 2.5 to 3.5 times, and further preferably 3 to 3.5 times.

[0038] The present invention has no particular limitation on the mixing, as long as the raw materials can be mixed evenly, such as stirring and mixing.

[0039] In the present invention, the temperature of the quaternization reaction is preferably 40-60°C, more preferably 45-55°C, and further preferably 50°C; the time of the quaternization reaction is preferably 1-3h, more preferably 1.5-2.5h, and further preferably 2h.

[0040] After completing the quaternization reaction, the present invention preferably further comprises: cooling the reaction system obtained by the quaternization reaction to room temperature and then performing solid-liquid separation, washing the obtained solid product and then drying it to obtain the monomer containing both triquaternary ammonium salt ions and trivinylbenzene structure. In the present invention, the solid-liquid separation preferably comprises filtration, suction filtration or centrifugal separation. In the present invention, the washing solvent preferably comprises tetrahydrofuran and / or ethyl acetate. In the present invention, the drying temperature is preferably 80 to 120°C, more preferably 100 to 110°C; the drying time is preferably 4 to 10 hours, more preferably 5 to 8 hours; the drying preferably comprises vacuum drying.

[0041] The present invention provides the use of the monomer containing triquaternary ammonium salt ions and trivinylbenzene structures at the same time as described in the above technical solution or the monomer containing triquaternary ammonium salt ions and trivinylbenzene structures at the same time as described in the above technical solution prepared by the preparation method in preparing anion exchange resin.

[0042] The invention provides an anion exchange resin, wherein the preparation raw materials include a vinyl monomer, an initiator and a solvent; the vinyl monomer includes the monomer containing triquaternary ammonium salt ions and trivinylbenzene structures as described in the above technical scheme or the monomer containing triquaternary ammonium salt ions and trivinylbenzene structures as prepared by the preparation method as described in the above technical scheme.

[0043] In the present invention, the water-soluble vinyl monomer preferably also includes other water-soluble vinyl monomers; the other water-soluble vinyl monomers preferably include at least one of N-hydroxyacrylamide, acrylamide, acrylic acid and N-vinyl-2-pyrrolidone. In the present invention, when the water-soluble vinyl monomer is a monomer containing triquaternary ammonium salt ions and trivinyl benzene structure and other water-soluble vinyl monomers, the mass ratio of the monomer containing triquaternary ammonium salt ions and trivinyl benzene structure and other water-soluble vinyl monomers is preferably 1.1 to 9:1, more preferably 1:2 to 5.

[0044] In the present invention, when the vinyl monomer is a monomer containing both triquaternary ammonium salt ions and trivinylbenzene structures, the structural unit of the anion exchange resin has the structural formula shown in Formula II:

[0045]

[0046] Among them, when the vinyl monomer is a monomer containing both triquaternary ammonium salt ions and trivinylbenzene structures, Indicates the repetition of the structural unit in the polymer structure. When the vinyl monomer is a monomer containing triquaternary ammonium salt ions and trivinylbenzene structure and other water-soluble vinyl monomers, represents the repetition of the structural unit and other water-soluble vinyl monomers in the polymer structure; n is the repetition of the structural unit.

[0047] The present invention uses a monomer containing both triquaternary ammonium salt ions and trivinylbenzene as a preparation raw material, and the synergistic introduction of multiple vinylbenzenes and multiple quaternary ammonium ions can further increase the ion exchange capacity of the resin while increasing the crosslinking density of the anion exchange resin. After introducing other water-soluble vinyl monomers, the capacity of the anion exchange resin is regulated, thereby obtaining an anion exchange resin with a required ion exchange capacity.

[0048] In the present invention, the initiator is preferably a water-soluble initiator, more preferably a persulfate, and more preferably ammonium persulfate and / or potassium persulfate. In the present invention, the mass of the initiator is preferably 1-2% of the mass of the water-soluble vinyl monomer, more preferably 1.2-1.8%, and more preferably 1.4-1.5%.

[0049] In the present invention, the solvent preferably includes water. In the present invention, the mass of the solvent is preferably 3 to 5 times the mass of the water-soluble vinyl monomer, more preferably 3.5 to 4.5 times, and further preferably 4 times.

[0050] The present invention provides a method for preparing the anion exchange resin described in the above technical solution, comprising the following steps: mixing a water-soluble vinyl monomer, an initiator and a solvent, and performing a free radical polymerization reaction to obtain the anion exchange resin.

[0051] The present invention has no particular limitation on the mixing, as long as the raw materials can be mixed evenly, such as stirring and mixing.

[0052] In the present invention, the temperature of the free radical polymerization reaction is preferably 80-90°C, more preferably 82-88°C, and further preferably 84-85°C; the time of the free radical polymerization reaction is preferably 0.5-1.5h, more preferably 1h; and the free radical polymerization reaction is preferably carried out under stirring conditions.

[0053] In the present invention, the preparation route of the anion exchange resin is as follows:

[0054]

[0055] The present invention provides the use of the anion exchange resin described in the above technical solution or the anion exchange resin prepared by the preparation method described in the above technical solution in water treatment, electrolyte, material purification or oil extraction.

[0056] In the present invention, the electrolyte preferably includes an electrolyte for a new energy battery.

[0057] In the present invention, the substance purification preferably includes purification of natural extracts or purification of chemically synthesized substances, and the natural extracts preferably include natural medicines.

[0058] The anion exchange resin provided by the present invention has a high cross-linking density and a high ion exchange capacity, and the ion exchange capacity of the anion exchange resin can be regulated by introducing other water-soluble vinyl monomers. The anion exchange resin provided by the present invention has important potential application value in the fields of water treatment, electrolytes, material purification, oil extraction, etc., and has important academic research and practical application value.

[0059] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described in conjunction with specific embodiments below. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Any modification, equivalent replacement, improvement, etc. made to the implementation methods of the present invention based on the technical essence and general principles of the present invention without creative work should be within the scope of protection of the present invention.

[0060] The following are the raw materials and medicines used in the examples:

[0061] p-Chloromethylstyrene (purity 99%), Shandong Xingshun New Materials Co., Ltd.;

[0062] Tris(N,N-dimethylaminopropyl)amine (purity 98%), N-hydroxyacrylamide (purity 99%), acrylamide (purity 99%), acrylic acid (purity 99%) and N-vinyl-2-pyrrolidone (purity 99%): Shanghai MacLean Biochemical Technology Co., Ltd.;

[0063] Ammonium persulfate, potassium persulfate, N-methylpyrrolidone, N,N-dimethylacetamide and N,N-dimethylformamide: Shanghai Sinopharm Chemical Reagent Co., Ltd., chemically pure.

[0064] The chloride ion exchange capacity is measured by dividing the amount of chloride ion substance (in mmol) by the mass of the resin (in g).

[0065] Example 1

[0066] 27.247 g (0.1 mol) and 61.04 g (0.4 mol) of tri(N,N-dimethylaminopropyl)amine and p-chloromethylstyrene were respectively added to a 500 mL dry three-necked flask equipped with a mechanical stirrer and a condenser, 200 mL of N-methylpyrrolidone was added, the temperature was raised to 60°C and stirred for reaction for 1 h to obtain a solid-liquid mixture, the reaction was terminated, the reaction solution was filtered, and the product was washed with tetrahydrofuran, and further dried in a vacuum oven at 80°C for 10 h to obtain tri(4-vinylbenzyl-N,N-dimethylmethylammonium chloride-tripropyl)amine containing both triquaternary ammonium salt ions and trivinylbenzene structure monomers, and the yield was 93%. 1HNMR (CDCl3, 400MHz): 7.64 (d, 6H), 7.57 (d, 6H), 6.74-6.81 (m, 3H), 5.93 (d, 3H), 5.37 (d, 3H), 4.83 (s, 6H), 3.67 (m, 6H), 3.07 (s, 18H), 2.46 (m, 6H), 1.96 (m, 6H); For details of the proton absorption peaks in the NMR spectrum, please see the attached Figure 1 FT-IR(KBr) / cm -1 :3023,2964,2827,1641,1473; 2827~3023cm in infrared spectrum -1 The absorption peak at 1641cm is the characteristic absorption peak of alkyl group. -1 The absorption peak at 1473 cm is the characteristic absorption peak of C=C double bond. -1 The absorption peak at is the characteristic absorption peak of CN.

[0067] Example 2

[0068] 27.247 g (0.1 mol) and 45.78 g (0.3 mol) of tri(N,N-dimethylaminopropyl)amine and p-chloromethylstyrene were respectively added to a 500 mL dry three-necked flask equipped with a mechanical stirrer and a condenser, and 260 mL of N,N-dimethylacetamide was added. The temperature was raised to 40°C and stirred for reaction for 3 h to obtain a solid-liquid mixture. The reaction was terminated, the reaction solution was filtered, and the product was washed with ethyl acetate, and further dried in a vacuum oven at 120°C for 4 h to obtain tri(4-vinylbenzyl-N,N-dimethylmethylammonium chloride-tripropyl)amine containing both triquaternary ammonium salt ions and trivinylbenzene structure monomers, with a yield of 91%.

[0069] Example 3

[0070] 27.247 g (0.1 mol) and 53.41 g (0.35 mol) of tri(N,N-dimethylaminopropyl)amine and p-chloromethylstyrene were added to a 500 mL dry three-necked flask equipped with a mechanical stirrer and a condenser, 240 N,N-dimethylformamide was added, the temperature was raised to 50°C and stirred for reaction for 2 h to obtain a solid-liquid mixture, the reaction was terminated, the reaction solution was filtered, and the product was washed with tetrahydrofuran, and further dried in a vacuum oven at 100°C for 6 h to obtain tri(4-vinylbenzyl-N,N-dimethylmethylammonium chloride-tripropyl)amine containing both triquaternary ammonium salt ions and trivinylbenzene structure monomers, with a yield of 92%.

[0071] The polymerization of monomers containing triquaternary ammonium salt ions and trivinylbenzene structures and the preparation of anion exchange resins are as follows.

[0072] Application Example 1

[0073] 7.3034 g (0.01 mol) of N-hydroxyacrylamide and triquaternary ammonium salt ions and tri(4-vinylbenzyl-N,N-dimethylmethylammonium chloride-tripropyl)amine are added to a 250 mL three-necked flask equipped with a mechanical stirrer and a condenser, and 3 to 5 times the weight of water of the monomer is added as a solvent. After stirring until the system becomes clear, 1 to 2% of the weight of the monomer potassium persulfate is added as an initiator, the temperature is raised to 90° C. and stirred for 0.5 h. The product is filtered and washed with water. After drying, an anion exchange resin with high crosslinking density and ion exchange capacity (chloride ion exchange capacity is 4.107 mmol / g) is obtained, and the yield is 95%.

[0074] Application Example 2

[0075] 0.8115 g (0.008 mol) of N-hydroxyacrylamide and 7.3034 g (0.01 mol) of tri(4-vinylbenzyl-N,N-dimethylmethylammonium chloride-tripropyl)amine were added to a 250 mL three-necked flask equipped with a mechanical stirrer and a condenser, and 3 to 5 times the weight of water of the monomer was added as a solvent. After stirring until the system became clear, 1 to 2% of the weight of ammonium persulfate of the monomer was added as an initiator. The temperature was raised to 85° C. and stirred for 1 hour. The product was filtered and washed with water. After drying, an anion exchange resin with high crosslinking density and ion exchange capacity (chloride ion exchange capacity of 3.697 mmol / g) was obtained, and the yield was 96%.

[0076] Application Example 3

[0077] 1.466g (0.0145mol) of N-hydroxyacrylamide and 7.3034g (0.01mol) of tri(4-vinylbenzyl-N,N-dimethylmethylammonium chloride-tripropyl)amine were added to a 250mL three-necked flask equipped with a mechanical stirrer and a condenser, and 3 to 5 times the weight of water of the monomer was added as a solvent. After stirring until the system became clear, 1 to 2% of the weight of ammonium persulfate of the monomer was added as an initiator. The temperature was raised to 80°C and stirred for 1.5h. The product was filtered and washed with water. After drying, an anion exchange resin with high crosslinking density and ion exchange capacity (chloride ion exchange capacity of 3.421mmol / g) was obtained, and the yield was 96%.

[0078] Application Example 4

[0079] 6.5718 g (0.065 mol) of N-hydroxyacrylamide and 7.3034 g (0.01 mol) of tri(4-vinylbenzyl-N,N-dimethylmethylammonium chloride-tripropyl)amine were added to a 250 mL three-necked flask equipped with a mechanical stirrer and a condenser, and 3 to 5 times the weight of water of the monomer was added as a solvent. After stirring until the system became clear, 1 to 2% of the weight of ammonium persulfate of the monomer was added as an initiator. The temperature was raised to 80° C. and stirred for 1 hour. The product was filtered and washed with water. After drying, an anion exchange resin with high crosslinking density and ion exchange capacity (chloride ion exchange capacity of 2.162 mmol / g) was obtained, and the yield was 96%.

[0080] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A monomer containing triquaternary ammonium salt ions and trivinylbenzene structure, having a structure shown in Formula I:

2. The method for preparing a monomer containing triquaternary ammonium salt ions and trivinylbenzene structure according to claim 1, comprising the following steps: The tri(N,N-dimethylaminopropyl)amine, p-chloromethylstyrene and a polar organic solvent are mixed and subjected to a quaternization reaction to obtain the monomer containing both triquaternary ammonium salt ions and trivinylbenzene structures.

3. The preparation method according to claim 2, characterized in that: The molar ratio of tris(N,N-dimethylaminopropyl)amine to p-chloromethylstyrene is 1:3-4; The polar organic solvent includes at least one of N-methylpyrrolidone, N,N-dimethylacetamide and N,N-dimethylformamide.

4. The preparation method according to claim 2 or 3, characterized in that: The temperature of the quaternization reaction is 40-60° C. and the time is 1-3 hours.

5. Use of the monomer containing triquaternary ammonium salt ions and trivinylbenzene structures as claimed in claim 1 or the monomer containing triquaternary ammonium salt ions and trivinylbenzene structures obtained by the preparation method according to any one of claims 2 to 4 in the preparation of anion exchange resin.

6. An anion exchange resin, wherein the raw materials for preparing the anion exchange resin include a vinyl monomer, an initiator and a solvent; the vinyl monomer includes the monomer containing triquaternary ammonium salt ions and trivinylbenzene structures as claimed in claim 1 or the monomer containing triquaternary ammonium salt ions and trivinylbenzene structures as prepared by the preparation method according to any one of claims 2 to 4.

7. The anion exchange resin according to claim 6, characterized in that The vinyl monomer also includes other water-soluble vinyl monomers; The other water-soluble vinyl monomers include at least one of N-hydroxyacrylamide, acrylamide, acrylic acid and N-vinyl-2-pyrrolidone; the mass ratio of the monomer containing triquaternary ammonium salt ions and trivinylbenzene structure to the other water-soluble vinyl monomers is 1.1 to 9:1; The mass of the initiator is 1-2% of the mass of the ethylene monomer; The solvent includes water.

8. The method for preparing the anion exchange resin according to claim 6 or 7, comprising the following steps: The vinyl monomer, initiator and solvent are mixed and subjected to free radical polymerization reaction to obtain an anion exchange resin.

9. The preparation method according to claim 8, characterized in that: The temperature of the free radical polymerization reaction is 80-90° C. and the time is 0.5-1.5 h.

10. Use of the anion exchange resin according to any one of claims 6 to 7 or the anion exchange resin prepared by the preparation method according to any one of claims 8 to 9 in water treatment, electrolytes, material purification or oil extraction.

Citation Information

Patent Citations

  • Method for preparing vicinal diol compound through ring-opening reaction

    CN106478374A

  • Polyvinyl chloride resin multi-functional-group covalent cross-linking modification method

    CN108084317A

  • Method for removing Phosphate and Polymer Used Therefore

    US20090047233A1