Lithium difluoro (oxalato) borate concentrated solution as well as preparation method and application thereof
By mixing lithium tetrafluoroborate, an aprotic solvent and oxalic acid in an inert dry atmosphere, and adding silicon tetrafluoride dropwise, followed by degassing and resin treatment, a high-purity lithium difluoroborate concentrate was prepared to solve the problem. In the existing technology, the problems of cumbersome preparation process and introduction of impurities have been achieved, and the preparation of efficient and low-cost lithium difluoroxalate borate concentrate has been achieved, which is suitable for lithium-ion or sodium-ion battery electrolytes.
Patent Information
- Application Number
- CN202410908032.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-15
AI Technical Summary
The existing preparation method of lithium difluoroxaloborate is cumbersome and has a long cycle, resulting in high impurity content in the product, which affects the performance and safety of lithium (sodium) ion batteries. Moreover, when the solid lithium difluoroxaloborate solid needs to be dissolved again, impurities will be introduced. Increase usage costs.
The concentrated solution of lithium difluoroborate oxalate in the state of aprotic electrolyte is mixed with lithium tetrafluoroborate, an aprotic solvent and oxalic acid in an inert dry atmosphere, and then silicon tetrachloride is dropped in for degassing and resin treatment. A high-purity lithium difluoroxalate borate concentrate is prepared, avoiding the evaporation crystallization process and re-dissolution process.
The preparation of high-purity, low-impurity lithium difluoroborate borate concentrate is achieved, simplifying the process steps, reducing production and transportation costs, and avoiding the risk of impurity introduction. It is suitable for the preparation of electrolytes for lithium-ion or sodium-ion batteries.
Smart Images

Figure CN118772185A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of battery manufacturing, and in particular to a lithium difluorooxalatoborate concentrated solution and a preparation method and application thereof. Background Art
[0002] Lithium difluorooxalatoborate is an important electrolyte, mainly used in non-aqueous electrolytes of lithium (sodium) ion batteries, so it is required to have very high purity. Impurities in lithium difluorooxalatoborate, such as water, alkali metals, heavy metals, chloride ions, sulfate or free acid, must be strictly controlled, otherwise it will cause the battery's internal resistance to increase, the battery capacity to decay quickly, and the cycle life to shorten, thus affecting the safety of the battery.
[0003] Therefore, obtaining a lithium difluorooxalate borate product with high purity and low content of harmful impurities has important practical significance. CN109232628A discloses a method for synthesizing lithium difluorooxalate borate by a one-pot method, which mainly prepares lithium tetrafluoroborate by using lithium fluoride and boron trifluoride as raw materials, then drips hexamethyldisiloxane under the reaction of oxalic acid at 60°C to obtain a crude product, and finally precipitates the product from the crude product by adding a non-polar solvent to obtain a lithium difluorooxalate borate solid; CN112480153A discloses a method for preparing lithium difluorooxalate borate, which mainly reacts a hydrogen fluoride solution of lithium fluoride with boron trichloride and oxalic acid at 5-20°C to obtain a hydrogen fluoride solution containing lithium difluorooxalate borate and lithium tetrafluoroborate, removes the solvent, obtains a solid mixture of lithium difluorooxalate borate and lithium tetrafluoroborate, and then separates and purifies to obtain a lithium difluorooxalate borate solid. The currently disclosed preparation methods of lithium difluorooxalatoborate all produce lithium difluorooxalatoborate solid, and the solid is mainly obtained by multiple purifications, which makes the overall preparation process complicated and time-consuming.
[0004] In addition, the lithium difluorooxalate borate solid needs to be dissolved again during use, and some impurities will be introduced during the dissolution process, which increases the cost of use. Therefore, it is still necessary to provide a new solution that can directly obtain a high-purity, low-impurity lithium difluorooxalate borate solution product, simplify the preparation process steps, and realize direct application in lithium (sodium) ion batteries. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a lithium difluorooxalate borate concentrated solution, which exists in the state of aprotic electrolyte, has low acidity, low chlorine content, and high purity, and can be directly used in the preparation of lithium ion batteries or sodium ion batteries. The preparation of the lithium difluorooxalate borate concentrated solution omits the evaporation and crystallization process, thereby reducing the production cost; in addition, it can be transported by pipeline, further reducing the product transportation cost; compared with the lithium difluorooxalate borate solid, the process of re-dissolution during use is omitted, the risk of impurity introduction is avoided, and the use cost is greatly reduced.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a lithium difluorooxalate borate concentrate, wherein the lithium difluorooxalate borate concentrate is composed of lithium difluorooxalate borate and an aprotic solvent, wherein the aprotic solvent includes any one of diethyl carbonate, ethyl methyl carbonate, ethylene carbonate or propylene carbonate, or a combination of at least two thereof;
[0008] The concentration of lithium difluorooxalate borate in the lithium difluorooxalate borate concentrate is 10-30wt%, for example, 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, 20wt%, 22wt%, 24wt%, 26wt%, 28wt% or 30wt%.
[0009] The lithium difluorooxalate borate concentrate provided by the present invention exists in the state of aprotic electrolyte. Compared with the lithium difluorooxalate borate solid, the process of re-dissolving during use is omitted, the risk of impurity introduction is avoided, and the use cost is reduced.
[0010] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0011] Preferably, the acidity of the lithium difluorooxalatoborate concentrate is <100ppm, for example, 90ppm, 80ppm, 70ppm, 60ppm, 50ppm, 40ppm, 30ppm, 20ppm, 10ppm or 1ppm, etc., the water content is <50ppm, for example, 40ppm, 35ppm, 30ppm, 25ppm, 20ppm, 15ppm, 10ppm, 5ppm or 1ppm, etc., and the chloride ion concentration is <20ppm, for example, 19ppm, 18ppm, 17ppm, 16ppm, 15ppm, 14ppm, 13ppm, 12ppm, 11ppm, 10ppm, 9ppm, 8ppm, 7ppm, 6ppm, 5ppm, 4ppm, 3ppm, 2ppm or 1ppm, etc.
[0012] Preferably, the acidity of the lithium difluorooxalate borate concentrate is <30 ppm, the water content is <20 ppm, and the chloride ion concentration is <5 ppm.
[0013] In the present invention, the acidity, water content and chloride ion concentration of the lithium difluorooxalate borate concentrated solution are all low, thereby avoiding the influence of impurities on the performance of the electrolyte during use and meeting the use standards of battery-grade electrolyte.
[0014] In a second aspect, the present invention further provides a method for preparing the lithium difluorooxalate borate concentrate according to the first aspect, the preparation method comprising the following steps:
[0015] (1) in an inert dry atmosphere, mixing lithium tetrafluoroborate, an aprotic solvent and oxalic acid to obtain a reaction solution;
[0016] (2) maintaining an inert dry atmosphere, dropping silicon tetrachloride into the reaction solution of step (1) to react, and degassing to obtain a precursor concentrated solution;
[0017] (3) maintaining an inert dry atmosphere, and subjecting the precursor concentrate of step (2) to resin treatment to obtain a lithium difluorooxalate borate concentrate.
[0018] The preparation method of the lithium difluorooxalate borate concentrated solution provided by the present invention avoids the use of hydrogen fluoride as a raw material, and also avoids the risks caused by the use of hydrogen fluoride, thereby further improving the yield; the lithium difluorooxalate borate concentrated solution obtained by combining degassing concentration and resin treatment to remove impurities has a high purity.
[0019] In the present invention, it is necessary to ensure that the entire reaction is carried out in an inert dry atmosphere, otherwise the acidity, chloride ion and water content in the prepared lithium difluorooxalate borate concentrated solution system will be relatively high.
[0020] Preferably, the inert dry atmosphere comprises dry nitrogen or dry argon.
[0021] Preferably, the mass ratio of the lithium tetrafluoroborate to the aprotic solvent in step (1) is 1:(1-20), for example 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19 or 1:20, etc., preferably 1:(8-12).
[0022] When the mass ratio of lithium tetrafluoroborate to the aprotic solvent in the present invention is 1:(8-12), the prepared lithium difluorooxalatoborate concentrated solution has not only low acidity but also high purity.
[0023] Preferably, the molar ratio of the lithium tetrafluoroborate to the oxalic acid in step (1) is 1:(0.8-1.2), for example, 1:0.8, 1:0.85, 1:0.9, 1:0.95, 1:1, 1:1.05, 1:1.1, 1:1.15 or 1:1.2, etc., preferably 1:(0.95-1.05).
[0024] When the molar ratio of lithium tetrafluoroborate to the oxalic acid in the present invention is 1:(0.95-1.05), the prepared lithium difluorooxalatoborate concentrated solution has not only low acidity but also high purity.
[0025] Preferably, the mixing in step (1) comprises: firstly mixing and dissolving lithium tetrafluoroborate and a non-protonic solvent, and then adding oxalic acid.
[0026] Preferably, the mixed dissolution method includes stirring.
[0027] Preferably, the stirring time is 5 to 15 min, for example, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min or 15 min.
[0028] Preferably, the molar ratio of the lithium tetrafluoroborate in step (1) to the silicon tetrachloride in step (2) is 1:(0.4-0.6), for example, 1:0.4, 1:0.42, 1:0.44, 1:0.46, 1:0.48, 1:0.5, 1:0.52, 1:0.54, 1:0.56, 1:0.58 or 1:0.6, etc., preferably 1:(0.48-0.52).
[0029] When the molar ratio of the lithium tetrafluoroborate in step (1) to the silicon tetrachloride in step (2) is 1:(0.48-0.52) in the present invention, the prepared lithium difluorooxalatoborate concentrated solution has not only low acidity but also high purity.
[0030] Preferably, the temperature of the reaction solution in step (1) is -5 to 60°C, for example, -5°C, 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C, etc.
[0031] Preferably, the reaction temperature in step (2) is -5 to 60°C, for example, -5°C, 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C, etc.
[0032] In the present invention, when the reaction temperature is -5 to 60°C, silicon tetrachloride can effectively participate in the reaction. If the temperature is too high, silicon tetrachloride will volatilize severely and fail to participate in the reaction; if the temperature is too low, the reaction speed will be slow and the reaction will be incomplete.
[0033] Preferably, the reaction time is 1 to 8 h, for example, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h or 8 h.
[0034] It should be noted that the temperature of the reaction in step (2) is consistent with the temperature of the reaction solution in step (1).
[0035] Preferably, the degassing in step (2) includes positive pressure degassing with supplementary inert gas or negative pressure degassing.
[0036] It should be noted that the positive pressure supplementary inert gas degassing or the negative pressure degassing can both be used to remove hydrogen chloride from the system after the reaction is completed, but the positive pressure supplementary inert gas degassing takes a slightly longer time.
[0037] In the present invention, degassing is used to further reduce the hydrogen chloride in the system after the reaction is completed, thereby lowering the acidity and chloride ion concentration of the system.
[0038] Preferably, the degassing pressure in step (2) is 0.5-10 kPa, for example, 0.5 kPa, 1 kPa, 1.5 kPa, 2 kPa, 2.5 kPa, 3 kPa, 3.5 kPa, 4 kPa, 4.5 kPa, 5 kPa, 5.5 kPa, 6 kPa, 6.5 kPa, 7 kPa, 7.5 kPa, 8 kPa, 8.5 kPa, 9 kPa, 9.5 kPa or 10 kPa, etc.
[0039] Preferably, the degassing temperature in step (2) is -5 to 60°C, for example, -5°C, 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C, etc.
[0040] Preferably, the degassing time in step (2) is 2 to 6 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours.
[0041] Preferably, the resin in the resin treatment in step (3) comprises a strong basic anion resin and / or a weak basic anion resin.
[0042] Preferably, before the resin treatment in step (3), the process further comprises adding an aprotic solvent.
[0043] It should be noted that before the resin treatment in step (3), the concentration of the precursor concentrate in step (2) needs to be 0.5 to 2 wt% higher than the target lithium difluorooxalate borate concentrate product concentration. If the concentration of the precursor concentrate in step (2) is too high, that is, the difference from the target lithium difluorooxalate borate concentrate product concentration exceeds 0.5 to 2 wt%, it is necessary to further add aprotic solvent.
[0044] In the present invention, the use of resin to treat the precursor concentrate can further effectively reduce the acid, chloride ion and water content in the system to meet the use standards of battery-grade electrolyte.
[0045] As a preferred technical solution, the preparation method comprises the following steps:
[0046] (1) In an inert dry atmosphere, lithium tetrafluoroborate and an aprotic solvent are mixed and stirred for 5 to 15 minutes to dissolve, and then oxalic acid is added and mixed evenly, and the temperature of the resulting reaction solution is controlled to be -5 to 60°C;
[0047] Wherein, the mass ratio of the lithium tetrafluoroborate to the aprotic solvent is 1:(1-20); the molar ratio of the lithium tetrafluoroborate to the oxalic acid is 1:(0.8-1.2); the inert dry atmosphere includes dry nitrogen or dry argon;
[0048] (2) adding silicon tetrachloride dropwise into the reaction solution of step (1), reacting at -5 to 60° C. for 1 to 8 hours, and degassing at a pressure of 0.5 to 10 kPa and a temperature of -5 to 60° C. for 2 to 6 hours to obtain a precursor concentrated solution;
[0049] Wherein, the molar ratio of the lithium tetrafluoroborate in step (1) to the silicon tetrachloride in step (2) is 1:(0.4-0.6); the degassing includes positive pressure supplementary inert gas degassing or negative pressure degassing;
[0050] (3) treating the precursor concentrate of step (2) with a resin to obtain a lithium difluorooxalate borate concentrate;
[0051] Wherein, if the concentration of the precursor concentrate in step (2) is too high, that is, the difference compared with the target lithium difluorooxalate borate concentrated solution product concentration exceeds 0.5-2wt%, before the resin treatment, it also includes adding aprotic solvent, and adding aprotic solvent until the product concentration is 0.5-2wt% higher than the target lithium difluorooxalate borate concentrated solution product concentration; the resin in the resin treatment includes a strong base anion resin and / or a weak base anion resin.
[0052] In a third aspect, the present invention also provides an application of a lithium difluorooxalate borate concentrate, wherein the lithium difluorooxalate borate concentrate described in the first aspect, or the lithium difluorooxalate borate concentrate prepared by the preparation method described in the second aspect, is used to prepare a non-aqueous electrolyte for a lithium ion battery or a sodium ion battery.
[0053] Compared with the prior art, the present invention has at least the following beneficial effects:
[0054] 1) The lithium difluorooxalate borate concentrate provided by the present invention exists in the state of aprotic electrolyte, has low acidity, low chlorine content, and high purity, and can be directly used for the preparation of electrolytes for lithium ion batteries or sodium ion batteries;
[0055] 2) The lithium difluorooxalate borate concentrate provided by the present invention can be transported through pipelines, thereby reducing the transportation cost of the product; compared with the lithium difluorooxalate borate solid, the process of re-dissolving during use is omitted, the risk of impurities being introduced is avoided, and the use cost is greatly reduced;
[0056] 3) The preparation of the lithium difluorooxalate borate concentrate provided by the present invention eliminates the evaporation and crystallization process, thereby reducing the production cost;
[0057] 4) The present invention prepares a lithium difluorooxalate borate solution through a simple and efficient one-step reaction, thereby reducing production capacity loss. By controlling the ratio of reaction raw materials, the prepared lithium difluorooxalate borate solution has a lower initial acidity and chloride ion concentration. Then, through subsequent treatment, the impurity content in the system is quickly and efficiently reduced to obtain a lithium difluorooxalate borate concentrate that meets the battery electrolyte use standards. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 The lithium difluorooxalate borate concentrate prepared in Example 1 of the present invention is 11 B-NMR spectrum. DETAILED DESCRIPTION
[0059] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0060] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0061] Example 1
[0062] This embodiment provides a lithium difluorooxalate borate concentrated solution and a preparation method thereof. The lithium difluorooxalate borate concentrated solution consists of lithium difluorooxalate borate and ethyl methyl carbonate. The concentration of lithium difluorooxalate borate in the lithium difluorooxalate borate concentrated solution is 20 wt %.
[0063] The preparation method of the lithium difluorooxalate borate concentrate comprises the following steps:
[0064] (1) In a dry nitrogen atmosphere, weigh 10.00 g of lithium tetrafluoroborate and add it to a reaction flask, add 120 g of ethyl methyl carbonate, stir for 10 min to completely dissolve the lithium tetrafluoroborate, add 9.60 g of oxalic acid to the reaction flask, and keep the resulting reaction solution warm to 20° C.;
[0065] (2) After the temperature is constant, 9.06 g of silicon tetrachloride is slowly added dropwise to the reaction solution (a large amount of acidic gas is generated during the addition process). After the addition is completed, the reaction is carried out at 20° C. for 4 h, and degassing is carried out at a negative pressure of 5 kPa and 20° C. for 3 h to obtain a precursor concentrated solution.
[0066] (3) Add ethyl methyl carbonate to the precursor concentrate and perform chromatography using type A weakly basic resin to obtain a lithium difluorobis(oxalyl)phosphate concentrate.
[0067] Figure 1 The lithium difluorooxalate borate concentrate prepared in this example is 11 B-NMR spectrum. It can be seen from the spectrum that the integral proportion of lithium difluorooxalatoborate reaches 96.7%.
[0068] Example 2
[0069] This embodiment provides a lithium difluorooxalate borate concentrated solution and a preparation method thereof. The lithium difluorooxalate borate concentrated solution consists of lithium difluorooxalate borate and ethyl methyl carbonate. The concentration of lithium difluorooxalate borate in the lithium difluorooxalate borate concentrated solution is 20 wt %.
[0070] The preparation method of the lithium difluorooxalate borate concentrate comprises the following steps:
[0071] (1) In a dry argon atmosphere, weigh 18.00 g of lithium tetrafluoroborate and add it to a reaction flask, add 180 g of ethyl methyl carbonate, stir for 10 min to completely dissolve the lithium tetrafluoroborate, add 17.31 g of oxalic acid to the reaction flask, and keep the resulting reaction solution warm to 20° C.;
[0072] (2) After the temperature is constant, 16.51 g of silicon tetrachloride is slowly added dropwise to the reaction solution (a large amount of acidic gas is generated during the addition process). After the addition is completed, the reaction is carried out at 20° C. for 4 h, and degassing is carried out at a negative pressure of 5 kPa and 20° C. for 3 h to obtain a precursor concentrated solution.
[0073] (3) Add ethyl methyl carbonate to the precursor concentrate and perform chromatography using a type B weakly alkaline resin to obtain a lithium difluorobis(oxalyl)phosphate concentrate.
[0074] Example 3
[0075] This embodiment provides a lithium difluorooxalate borate concentrated solution and a preparation method thereof. The lithium difluorooxalate borate concentrated solution consists of lithium difluorooxalate borate and ethylene carbonate. The concentration of lithium difluorooxalate borate in the lithium difluorooxalate borate concentrated solution is 10 wt %.
[0076] The preparation method of the lithium difluorooxalate borate concentrate comprises the following steps:
[0077] (1) In a dry nitrogen atmosphere, weigh 10.00 g of lithium tetrafluoroborate and add it to a reaction flask, add 80 g of ethylene carbonate, stir for 5 min to completely dissolve the lithium tetrafluoroborate, add 9.12 g of oxalic acid to the reaction flask, and keep the resulting reaction solution warm to -5°C;
[0078] (2) After the temperature is constant, 8.70 g of silicon tetrachloride is slowly added dropwise to the reaction solution (a large amount of acidic gas is generated during the addition process). After the addition is completed, the reaction is carried out at -5°C for 8 h, and degassing is carried out at a negative pressure of 10 kPa and -5°C for 6 h to obtain a precursor concentrated solution.
[0079] (3) The precursor concentrate is chromatographed using type A weakly alkaline resin to obtain a lithium difluorobis(oxalyl)phosphate concentrate.
[0080] Example 4
[0081] This embodiment provides a lithium difluorooxalate borate concentrated solution and a preparation method thereof. The lithium difluorooxalate borate concentrated solution consists of lithium difluorooxalate borate and ethyl methyl carbonate. The concentration of lithium difluorooxalate borate in the lithium difluorooxalate borate concentrated solution is 30 wt %.
[0082] The preparation method of the lithium difluorooxalate borate concentrate comprises the following steps:
[0083] (1) In a dry argon atmosphere, weigh 10.00 g of lithium tetrafluoroborate and add it to a reaction flask, add 120 g of ethyl methyl carbonate, stir for 15 min to completely dissolve the lithium tetrafluoroborate, add 10.08 g of oxalic acid to the reaction flask, and keep the resulting reaction solution warm to 40° C.;
[0084] (2) After the temperature is constant, 9.43 g of silicon tetrachloride is slowly added dropwise to the reaction solution (a large amount of acidic gas is generated during the addition process). After the addition is completed, the reaction is carried out at 40° C. for 8 h, and degassing is carried out at a negative pressure of 0.5 kPa and 40° C. for 2 h to obtain a precursor concentrated solution.
[0085] (3) The precursor concentrate is chromatographed using a type B weakly alkaline resin to obtain a lithium difluorobis(oxalyl)phosphate concentrate.
[0086] Example 5
[0087] This embodiment provides a lithium difluorooxalate borate concentrated solution and a preparation method thereof. The concentration and composition of lithium difluorooxalate borate in the lithium difluorooxalate borate concentrated solution are consistent with those in Example 1. The difference from Example 1 is that in the preparation method of the lithium difluorooxalate borate concentrated solution, the reaction solution in step (1) is kept warm to 60° C., and the remaining preparation methods and parameters are consistent with those in Example 1.
[0088] Example 6
[0089] The present embodiment provides a lithium difluorooxalate borate concentrated solution and a preparation method thereof. The concentration and composition of lithium difluorooxalate borate in the lithium difluorooxalate borate concentrated solution are consistent with those in Example 1. The difference from Example 1 is that in the preparation method of the lithium difluorooxalate borate concentrated solution, the amount of silicon tetrachloride added in step (2) is 7.95 g, and the remaining preparation methods and parameters are consistent with those in Example 1.
[0090] Example 7
[0091] The present embodiment provides a lithium difluorooxalate borate concentrated solution and a preparation method thereof. The concentration and composition of lithium difluorooxalate borate in the lithium difluorooxalate borate concentrated solution are consistent with those in Example 1. The difference from Example 1 is that in the preparation method of the lithium difluorooxalate borate concentrated solution, the amount of silicon tetrachloride added in step (2) is 9.79 g, and the remaining preparation methods and parameters are consistent with those in Example 1.
[0092] Example 8
[0093] This embodiment provides a lithium difluorooxalate borate concentrated solution and a preparation method thereof. The concentration and composition of lithium difluorooxalate borate in the lithium difluorooxalate borate concentrated solution are consistent with those in Example 1. The difference from Example 1 is that in the preparation method of the lithium difluorooxalate borate concentrated solution, the amount of oxalic acid added in step (1) is 8.64 g, and the remaining preparation methods and parameters are consistent with those in Example 1.
[0094] Example 9
[0095] This embodiment provides a lithium difluorooxalate borate concentrated solution and a preparation method thereof. The concentration and composition of lithium difluorooxalate borate in the lithium difluorooxalate borate concentrated solution are consistent with those in Example 1. The difference from Example 1 is that in the preparation method of the lithium difluorooxalate borate concentrated solution, the amount of oxalic acid added in step (1) is 11.05 g, and the remaining preparation methods and parameters are consistent with those in Example 1.
[0096] Example 10
[0097] This embodiment provides a lithium difluorooxalate borate concentrate and a preparation method thereof. The concentration and composition of lithium difluorooxalate borate in the lithium difluorooxalate borate concentrate are consistent with those in Example 1. The difference from Example 1 is that in the preparation method of the lithium difluorooxalate borate concentrate, in step (1), no dry gas is introduced, that is, the reaction is carried out under air conditions. The remaining preparation methods and parameters are consistent with those in Example 1.
[0098] Test Method
[0099] The lithium difluorooxalatoborate concentrate prepared in Examples 1 to 10 of the present invention was tested for acidity (calculated as HF ppm), chloride ion and water content by manual titration using silver ion titration method. The specific test results are shown in Table 1.
[0100] Table 1
[0101] project Acidity (calculated as HF ppm) Chloride ion (ppm) Water(ppm) Example 1 15 1 18 Example 2 18 1 12 Example 3 12 1 10 Example 4 12 1 12 Example 5 29 2 20 Example 6 17 1 18 Example 7 86 18 19 Example 8 12 18 11 Example 9 58 1 15 Example 10 73 106 210
[0102] The test results show that:
[0103] (1) It can be seen from Examples 1 to 9 that the acidity of the lithium difluorooxalate borate concentrate is ≤86ppm, the chloride ion is ≤18ppm, and the water content is ≤20ppm. More preferably, it can be seen from Examples 1 to 4 that the present invention adjusts the amount of reaction raw materials added and the reaction temperature to achieve an acidity of the lithium difluorooxalate borate concentrate of ≤18ppm, a chloride ion of ≤1ppm, and a water content of ≤18ppm.
[0104] (2) It can be seen from Examples 1 and 7 that when the amount of silicon tetrafluoride added is large, side reactions occur in the reaction system, resulting in a higher acidity of the prepared lithium difluorooxalatoborate concentrate, and the silicon tetrachloride in the concentrate cannot be completely removed, resulting in a higher chloride ion content therein.
[0105] (3) It can be seen from Examples 1 and 8 to 9 that if the amount of oxalic acid added is small, part of the silicon tetrafluoride does not participate in the reaction, resulting in a higher chloride ion content in the prepared lithium difluorooxalate borate concentrate; if the amount of oxalic acid added is large, part of the oxalic acid does not participate in the reaction, and the remaining oxalic acid cannot be completely removed, resulting in a higher acidity in the prepared lithium difluorooxalate borate concentrate.
[0106] (4) It can be seen from Examples 1 and 10 that when no dry gas is introduced and the entire reaction system contains water, the water content of the prepared lithium difluorooxalate borate concentrate is relatively high. At the same time, water can cause the hydrolysis of lithium difluorooxalate borate, resulting in an increase in its acidity.
[0107] In summary, the lithium difluorooxalate borate concentrated solution provided by the present invention exists in the state of a non-protonic electrolyte, has low acidity, low chlorine content, and high purity, and can be directly used in the preparation of electrolytes for lithium ion batteries or sodium ion batteries; the preparation of the lithium difluorooxalate borate concentrated solution omits the evaporation and crystallization process, thereby reducing the production cost; in addition, it can be transported by pipeline, further reducing the product transportation cost; compared with the lithium difluorooxalate borate solid, the process of re-dissolution during use is omitted, the risk of impurity introduction is avoided, and the use cost is greatly reduced.
[0108] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A lithium difluorooxalate borate concentrate, characterized in that: The lithium difluorooxalate borate concentrate is composed of lithium difluorooxalate borate and an aprotic solvent, wherein the aprotic solvent includes any one of diethyl carbonate, ethyl methyl carbonate, ethylene carbonate or propylene carbonate, or a combination of at least two thereof; The concentration of lithium difluorooxalate borate in the lithium difluorooxalate borate concentrated solution is 10-30 wt %.
2. The lithium difluorooxalate borate concentrate according to claim 1, characterized in that: The lithium difluorooxalate borate concentrate has an acidity of <100 ppm, a water content of <50 ppm, and a chloride ion concentration of <20 ppm.
3. A method for preparing the lithium difluorooxalate borate concentrate according to claim 1 or 2, characterized in that: The preparation method comprises the following steps: (1) in an inert dry atmosphere, mixing lithium tetrafluoroborate, an aprotic solvent and oxalic acid to obtain a reaction solution; (2) maintaining an inert dry atmosphere, dropping silicon tetrachloride into the reaction solution of step (1) to react, and degassing to obtain a precursor concentrated solution; (3) maintaining an inert dry atmosphere, and subjecting the precursor concentrate of step (2) to resin treatment to obtain a lithium difluorooxalate borate concentrate.
4. The preparation method according to claim 3, characterized in that: In step (1), the mass ratio of the lithium tetrafluoroborate to the aprotic solvent is 1:(1-20).
5. The preparation method according to claim 3, characterized in that: The molar ratio of the lithium tetrafluoroborate to the oxalic acid in step (1) is 1:(0.8-1.2).
6. The preparation method according to claim 3, characterized in that: The mixing in step (1) comprises: firstly mixing and dissolving lithium tetrafluoroborate and aprotic solvent, and then adding oxalic acid; The temperature of the reaction solution in step (1) is -5 to 60°C.
7. The preparation method according to claim 3, characterized in that: The molar ratio of the lithium tetrafluoroborate in step (1) to the silicon tetrachloride in step (2) is 1:(0.4-0.6).
8. The preparation method according to claim 3, characterized in that: The reaction temperature of step (2) is -5 to 60°C, and the reaction time is 1 to 8 hours.
9. The preparation method according to claim 3, characterized in that: The resin in the resin treatment in step (3) includes a strong alkaline anion resin and / or a weak alkaline anion resin.
10. An application of lithium difluorooxalate borate concentrate, characterized in that: The lithium difluorooxalate borate concentrate according to claim 1 or 2, or the lithium difluorooxalate borate concentrate prepared by the preparation method according to any one of claims 3 to 9, is used to prepare a non-aqueous electrolyte for lithium ion batteries or sodium ion batteries.
Citation Information
Patent Citations
Preparation method and formula of lithium ion battery electrolyte containing lithium borate
CN111463483A
Cited By
Preparation method of lithium difluorobisoxalato phosphate concentrated solution
CN120842276A
A method for preparing a lithium difluorodioxalate phosphate concentrate
CN120842276B
Method for preparing high-purity lithium difluoro (oxalato) borate solid by low-temperature melting method
CN121517447A