Phosphorus flame retardant and preparation method thereof
Phosphorus-based flame retardants prepared through chemical modification use PEPA and DPPC to improve compatibility with polymer materials, solve the problem of insufficient compatibility and stability of existing phosphorus-based flame retardants, and achieve excellent flame retardancy. It has excellent flame retardant properties and heat resistance, and is suitable for flame retardant modification of a variety of polymer materials, broadening the scope of applications.
Patent Information
- Application Number
- CN202410655450.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-24
- Publication Date
- 2024-10-15
AI Technical Summary
Existing phosphorus-based flame retardants have poor compatibility with polymer materials and poor thermal and light stability, which limits their use in outdoor applications and high-temperature environments.
A phosphorus-based flame retardant is prepared through chemical modification, using caged pentaerythritol phosphate (PEPA) and diphenylphosphinic acid chloride (DPPC) as the main components, and through specific chemical reactions and processes to improve its interaction with polymers. material compatibility and maintain good thermal and light stability.
It improves the compatibility of phosphorus-based flame retardants and polymer materials, achieves excellent flame retardant properties and heat resistance, is suitable for flame retardant modification of a variety of polymer materials, broadens its application scope, and the preparation process Simple, low cost, and easy to produce on a large scale.
Smart Images

Figure CN118772201A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of phosphorus flame retardants, in particular to a phosphorus flame retardant with excellent flame retardancy and heat resistance and a preparation method thereof. Background Art
[0002] Polymer materials are widely used in many industries due to their light weight and high strength. However, most polymer materials are flammable, which limits their application in certain fields with strict safety standards. Using flame retardants to modify polymer materials is one of the key methods to improve product safety and performance stability. Existing flame retardants mainly include two categories: inorganic flame retardants and organic flame retardants. Inorganic flame retardants such as aluminum hydroxide and magnesium hydroxide have good flame retardant effects, but when added in large amounts, they will seriously affect the physical properties of the material. Organic flame retardants, such as halogen compounds, have high flame retardant efficiency, but they will produce toxic gases when burned and have poor environmental friendliness. Therefore, seeking a new type of flame retardant that is efficient, environmentally friendly and has good processing performance has become a current research hotspot.
[0003] In recent years, phosphorus-based flame retardants have received widespread attention due to their high efficiency and environmental friendliness. Phosphorus-based flame retardants can promote the formation of a carbon layer during the combustion process, thereby effectively isolating oxygen and heat to achieve the purpose of flame retardancy. In particular, organic phosphorus flame retardants, due to the designability of their molecular structure, can be chemically modified to improve their compatibility with polymer materials and reduce the impact on material properties. Although phosphorus-based flame retardants have good development prospects, there are still some problems in the existing technology, such as the poor compatibility of phosphorus-based flame retardants with polymer substrates, which makes it difficult to disperse evenly in practical applications; in addition, some phosphorus-based flame retardants have poor thermal stability and light stability, which limits their use in high-temperature environments such as outdoor applications. Summary of the invention
[0004] The purpose of the present invention is to provide a phosphorus-based flame retardant to address the deficiencies of the above-mentioned prior art, which improves the compatibility with polymer materials through specific chemical modification and has excellent flame retardant and heat-resistant properties.
[0005] Another object of the present invention is to provide a method for preparing the phosphorus-based flame retardant.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is: a phosphorus-based flame retardant is prepared by chemical reaction of the following components in parts by weight: Caged Pentaerythritol Phosphate (PEPA) 45-70 parts Diphenylphosphine chloride (DPPC) 30-55 parts.
[0007] The purity of the PEPA and DPPC is preferably above 90% to ensure the high performance of the flame retardant.
[0008] A method for preparing a phosphorus-based flame retardant comprises the following steps: (1) Dispersing PEPA in an organic solvent, stirring until completely dissolved, and then transferring to a container; (2) Dissolving DPPC in an organic solvent under a nitrogen atmosphere; (3) dropping PEPA into the DPPC solution at a uniform rate, and performing a reflux reaction at a certain temperature to obtain a reaction mixture; (4) the reaction mixture is subjected to rotary distillation at 90-95° C. to obtain an oily liquid; (5) adding the oily liquid into deionized water and stirring it thoroughly, then washing it with a dilute acid solution with a pH value of 3-6 and a dilute alkali solution with a pH value of 8-11, and filtering it by suction to obtain a filter cake; (6) washing the filter cake with an organic washing solvent and filtering to obtain a white block sample; (7) The white block sample was dried at 80-85°C for 12-14 hours and then manually ground for 30 minutes to obtain the final product.
[0009] The organic solvent is one or a mixed solvent of two or more of acetonitrile, acetone, N,N-dimethylformamide and N-methylpyrrolidone.
[0010] Preferably, the organic solvent in step (1) and step (2) is the same organic solvent.
[0011] The reaction temperature of step (3) is 75-120° C., and the reflux reaction time is 4-10 hours.
[0012] The dilute acid solution used in step (5) is one or more mixed acid aqueous solutions selected from hydrochloric acid solution, nitric acid solution, sulfuric acid solution, phosphoric acid solution, citric acid solution, formic acid solution, and acetic acid solution.
[0013] The dilute alkali solution used in step (5) is one or more mixed alkali aqueous solutions selected from the group consisting of sodium hydroxide solution, potassium hydroxide solution, calcium hydroxide solution, sodium bicarbonate solution, ammonia solution, and sodium carbonate solution.
[0014] The organic washing solvent in step (6) is methanol, ethanol or a mixed solvent of the two.
[0015] During the preparation process, the phosphorus-based flame retardant of the present invention is subjected to specific chemical modification to enhance its compatibility with polymer materials, while maintaining good thermal stability and light stability.
[0016] Compared with the prior art, the phosphorus-based flame retardant of the present invention has the following beneficial effects: simple preparation process, low cost, and easy large-scale production; excellent mechanical properties and flame retardant properties, and suitable for flame retardant modification of various polymer materials; improved compatibility of the phosphorus-based flame retardant with polymer materials, easy processing, while maintaining good thermal stability and light stability, thereby broadening the application range of the phosphorus-based flame retardant.
[0017] The phosphorus-based flame retardant of the present invention is suitable for flame retardant treatment of flammable polymer compounds and can be widely used in flame retardant treatment of polymer materials such as plastics, rubber, and fibers to improve their application safety in the fields of electronics, construction, and transportation. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 A schematic diagram of a synthetic route of a phosphorus-based flame retardant of the present invention;
[0019] Figure 2 is the infrared spectrum of the phosphorus flame retardant prepared in Example 1;
[0020] Figure 3 Thermogravimetric curve (TG) of the phosphorus flame retardant prepared in Example 1;
[0021] Figure 4 is the differential thermogravimetric curve (DTG) of the phosphorus flame retardant prepared in Example 1;
[0022] Figure 5 This is the H NMR spectrum of the phosphorus flame retardant prepared in Example 1;
[0023] Figure 6 This is a test chart of the mechanical properties of natural rubber with phosphorus-based flame retardants added. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments, but the given embodiments do not constitute a limitation on the scope of protection claimed by the present invention. The following numerical parameters of this application are only the values for verifying the embodiments, and the corresponding target products of this application can also be obtained by enlarging and implementing according to the numerical ratio relationship published in this application. Example 1
[0025] A method for preparing a phosphorus-based flame retardant, wherein the synthetic route is as follows: Figure 1 As shown, the steps included are as follows: (1) Disperse 45 g of PEPA in 100 mL of acetonitrile at 50 °C, stir until completely dissolved, and then transfer to a 500 mL flask; (2) Under a nitrogen atmosphere, dissolve 30 g of diphenylphosphine chloride (DPPC) in 200 mL of acetonitrile for later use; (3) using a peristaltic pump, the PEPA solution was dripped into the DPPC at a uniform rate and refluxed at 75 °C for 4 h; (4) rotary distilling the reactants at 90° C. to obtain an oily liquid; (5) adding 200 mL of deionized water to the oily liquid, stirring at 60 r / min for 20 min, washing with a dilute hydrochloric acid solution (pH=4) and a dilute sodium hydroxide solution (pH=9), and then filtering to obtain a filter cake; (6) washing the filter cake with methanol and filtering to obtain a white block sample; (7) The white block sample was dried at 85 °C for 12 h and then manually ground for 30 min to obtain the final product.
[0026] The above products were tested by Figure 2 and Figure 5 It can be confirmed that the target product of the present invention, phosphorus flame retardant BPA, was successfully synthesized. The thermal stability test of the prepared phosphorus flame retardant was carried out by TG instrument, the sample mass was 4-6 mg, nitrogen atmosphere, heating rate was 20°C / min, and the temperature setting range was 40-800°C. The results are as follows Figure 3 and Figure 4 As shown, the residual carbon content is about 40% at 800°C, which proves that the carbon formation is good. Example 2
[0027] A method for preparing a phosphorus-based flame retardant comprises the following steps: (1) Disperse 50 g of PEPA in 100 mL of acetonitrile at 50 °C, stir until completely dissolved, and then transfer to a 500 mL flask; (2) Under a nitrogen atmosphere, dissolve 35 g of diphenylphosphine chloride (DPPC) in 200 mL of acetone for later use; (3) using a peristaltic pump, the PEPA solution was dripped into the DPPC at a uniform rate and refluxed at 85 °C for 6 h; (4) Rotary distilling the reactants at 92° C. to obtain an oily liquid; (5) adding 200 mL of deionized water to the oily liquid, stirring at 60 r / min for 20 min, washing with a dilute nitric acid solution (pH=4) and a dilute potassium hydroxide solution (pH=9), and then filtering to obtain a filter cake; (6) washing the filter cake with methanol and filtering to obtain a white block sample; (7) The white block sample was dried at 84 °C for 12 h and then manually ground for 30 min to obtain the final product. Example 3
[0028] A method for preparing a phosphorus-based flame retardant comprises the following steps: (1) Disperse 55 g of PEPA in 100 mL of dimethylformamide at 50 °C, stir until completely dissolved, and then transfer to a 500 mL flask; (2) Under a nitrogen atmosphere, dissolve 40 g of diphenylphosphine chloride (DPPC) in 200 mL of dimethylformamide for later use; (3) PEPA was dripped into DPPC at a uniform rate using a peristaltic pump and refluxed at 95 °C for 7 h; (4) Rotary distilling the reactants at 93° C. to obtain an oily liquid; (5) adding 200 mL of deionized water to the oily liquid, stirring at 60 r / min for 20 min, washing with a dilute phosphoric acid solution (pH=4) and a dilute calcium hydroxide solution (pH=9), and then filtering to obtain a filter cake; (6) washing the filter cake with ethanol and filtering to obtain a white block sample; (7) The white block sample was dried at 83 °C for 12 h and then manually ground for 30 min to obtain the final product. Example 4
[0029] A method for preparing a phosphorus-based flame retardant comprises the following steps: (1) Disperse 60 g of PEPA in 100 mL of acetonitrile at 50 °C, stir until completely dissolved, and then transfer to a 500 mL flask; (2) Under a nitrogen atmosphere, dissolve 45 g of diphenylphosphine chloride (DPPC) in 200 mL of acetonitrile for later use; (3) PEPA was dripped into DPPC at a uniform rate using a peristaltic pump and refluxed at 105 °C for 8 h; (4) Rotary distilling the reactants at 94° C. to obtain an oily liquid; (5) adding 200 mL of deionized water to the oily liquid, stirring at 60 r / min for 20 min, washing with a dilute formic acid solution (pH = 4) and a dilute sodium bicarbonate solution (pH = 9), and then filtering to obtain a filter cake; (6) washing the filter cake with methanol and filtering to obtain a white block sample; (7) The white block sample was dried at 81 °C for 12 h and then manually ground for 30 min to obtain the final product. Example 5
[0030] A method for preparing a phosphorus-based flame retardant comprises the following steps: (1) Disperse 65 g of PEPA in 100 mL of methyl pyrrolidone at 50 °C, stir until completely dissolved, and then transfer to a 500 mL flask; (2) Under a nitrogen atmosphere, dissolve 50 g of diphenylphosphine chloride (DPPC) in 200 mL of methyl pyrrolidone for later use; (3) PEPA was dripped into DPPC at a uniform rate using a peristaltic pump and refluxed at 115 °C for 9 h; (4) Rotary distilling the reactants at 94° C. to obtain an oily liquid; (5) adding 200 mL of deionized water to the oily liquid, stirring at 60 r / min for 20 min, washing with a dilute citric acid solution (pH = 4) and a dilute sodium carbonate solution (pH = 9), and then filtering to obtain a filter cake; (6) washing the filter cake with methanol and filtering to obtain a white block sample; (7) The white block sample was dried at 85 °C for 14 h and then manually ground for 30 min to obtain the final product. Example 6
[0031] A method for preparing a phosphorus-based flame retardant comprises the following steps: (1) Disperse 70 g of PEPA in 100 mL of acetonitrile at 50 °C, stir until completely dissolved, and then transfer to a 500 mL flask; (2) Under a nitrogen atmosphere, dissolve 55 g of diphenylphosphine chloride (DPPC) in 200 mL of acetonitrile for later use; (3) PEPA was dripped into DPPC at a uniform rate using a peristaltic pump and refluxed at 120 °C for 10 h; (4) Rotary distilling the reactants at 95° C. to obtain an oily liquid; (5) adding 200 mL of deionized water to the oily liquid, stirring at 60 r / min for 20 min, washing with a dilute acetic acid solution (pH=4) and a dilute ammonia solution (pH=9), and then filtering to obtain a filter cake; (6) washing the filter cake with methanol and filtering to obtain a white block sample; (7) The white block sample was dried at 82 °C for 13 h and then manually ground for 30 min to obtain the final product.
[0032] The phosphorus-based flame retardant prepared in the above embodiment of the present invention was added to natural rubber in an amount of 30%, and the flame retardant performance test results are shown in the following table: As shown in the table above, the flame retardant properties of pure natural rubber are greatly improved by the addition of phosphorus flame retardants.
[0033] The phosphorus flame retardant prepared in Example 1 was added in a gradient amount of 5-30%, and the prepared specimens were tested. The tensile properties of the prepared composite substrate were tested using a universal testing machine. According to the GB / T528-2009 standard, the dumbbell-shaped sample had a thickness of 1 mm, a width of 6 mm, an effective length between the clamps of 25 mm, and a tensile rate of 500 mm / min. Multiple tests were performed, and the results were as follows. Figure 6 As shown, after adding the phosphorus-based flame retardant of the present invention, the mechanical properties are also greatly improved.
[0034] The present invention and its embodiments are described schematically above, and the description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. Therefore, if a person skilled in the art is inspired by it and designs a structural method and an embodiment similar to the technical solution without creativity without departing from the purpose of the invention, they shall all fall within the protection scope of the present invention.
Claims
1. A phosphorus-based flame retardant, characterized in that: It is made by chemical reaction of the following components in parts by weight: Cage pentaerythritol phosphate 45-70 parts 30-55 parts of diphenylphosphine chloride.
2. A phosphorus-based flame retardant according to claim 1, characterized in that: The purity of the caged pentaerythritol phosphate and diphenylphosphine chloride is above 90%.
3. The method for preparing a phosphorus-based flame retardant according to claim 1 or 2, characterized in that: The steps involved are as follows: (1) dispersing caged pentaerythritol phosphate in an organic solvent; (2) dissolving diphenylphosphine chloride in an organic solvent under a nitrogen atmosphere; (3) dropping the caged pentaerythritol phosphate solution into diphenylphosphine chloride for reflux reaction to obtain a reaction mixture; (4) the reaction mixture is subjected to rotary distillation at 90-95° C. to obtain an oily liquid; (5) adding the oily liquid into deionized water and stirring it thoroughly, then washing it with a dilute acid solution with a pH value of 3-6 and a dilute alkali solution with a pH value of 8-11, and filtering it by suction to obtain a filter cake; (6) washing the filter cake with an organic washing solvent and filtering to obtain a white block sample; (7) Dry the white block sample at 80-85°C for 12-14 hours and then grind it.
4. The method for preparing a phosphorus-based flame retardant according to claim 3, characterized in that: The organic solvent is one or a mixed solvent of two or more of acetonitrile, acetone, N,N-dimethylformamide and N-methylpyrrolidone.
5. The method for preparing a phosphorus-based flame retardant according to claim 4, characterized in that: The organic solvent in step (1) and step (2) is the same organic solvent.
6. The method for preparing a phosphorus-based flame retardant according to claim 3, characterized in that: The reaction temperature of step (3) is 75-120° C., and the reflux reaction time is 4-10 hours.
7. The method for preparing a phosphorus-based flame retardant according to claim 3, characterized in that: The acid solution used in step (5) is one or more mixed acid aqueous solutions selected from hydrochloric acid solution, nitric acid solution, sulfuric acid solution, phosphoric acid solution, citric acid solution, formic acid solution, and acetic acid solution.
8. The method for preparing a phosphorus-based flame retardant according to claim 3, characterized in that: The alkaline solution used in step (5) is one or more mixed alkaline aqueous solutions selected from the group consisting of sodium hydroxide solution, potassium hydroxide solution, calcium hydroxide solution, sodium bicarbonate solution, ammonia solution, and sodium carbonate solution.
9. The method for preparing a phosphorus-based flame retardant according to claim 3, characterized in that: The organic washing solvent in step (6) is methanol, ethanol or a mixed solvent of the two.