High-temperature-resistant polymer, high-temperature-resistant polymer film and lithium battery

The high-temperature resistant polymer film generated by the polymerization of cyclic polyamines and multi-activated alkynes solves the thermal stability problem of lithium battery separators under high temperature conditions, achieves efficient ionic conductivity and electrochemical stability improvements, and simplifies preparation process.

CN118772401AActive Publication Date: 2024-10-15CHANGCHUN INSTITUTE OF APPLIED CHEMISTRY CHINESE ACADEMY OF SCIENCES
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410854046.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-15
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

Existing lithium battery separators have poor thermal stability under high temperature conditions and are prone to dimensional shrinkage leading to internal short circuits. The preparation process is complex and cannot meet the safety and performance requirements of electric vehicles and large energy storage systems.

Method used

The polymerization of cyclic polyamines and multi-activated alkynes is used to generate high-temperature resistant polymer films. The preparation process is simplified at room temperature through click reactions to form a cross-linked honeycomb chemical network structure, which avoids complex pore-making steps and catalyst residue problems.

Benefits of technology

It achieves high-temperature dimensional stability without obvious dimensional shrinkage at 200°C, significantly improves the ionic conductivity and electrochemical stability of the separator, simplifies the preparation process and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004917581800000031
    Figure BDA0004917581800000031
  • Figure BDA0004917581800000051
    Figure BDA0004917581800000051
  • Figure BDA0004917581800000071
    Figure BDA0004917581800000071
Patent Text Reader

Abstract

The invention provides a high-temperature-resistant polymer, a high-temperature-resistant polymer film and a lithium battery. The high-temperature-resistant polymer film provided by the invention can be obtained by addition polymerization of cyclic polyamine and multi-element activated alkyne, the steps are simple and convenient and can be carried out at room temperature in an air environment, meanwhile, the polymerization reaction does not need a catalyst, introduction of other impurities is avoided, the formula is simplified, and the production cost is reduced. The electrode side reaction possibly caused by catalyst residues is also avoided, and the obtained polymer film has a cross-linked regular honeycomb chemical network structure and good high-temperature size stability, and has no obvious size shrinkage after being heated at 200 DEG C for 1 hour.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium batteries, and in particular relates to a high temperature resistant polymer, a high temperature resistant polymer film and a lithium battery. Background Art

[0002] Due to its high energy density and long cycle life, lithium batteries are widely used in portable electronic devices, electric vehicles, energy storage devices and other fields, and have broad prospects for use. In recent years, with the gradual expansion of demand for electric vehicles and large-scale energy storage systems, the requirements for battery energy density, charge and discharge rate and safety are becoming higher and higher. The composition of lithium batteries usually includes positive electrode, negative electrode, diaphragm, electrolyte and battery casing. Among them, the diaphragm, as a material that isolates the positive and negative electrodes, is an important component to ensure the safety performance of the battery. In order to meet the battery performance, the diaphragm needs to have suitable mechanical strength, high porosity, resistance to electrochemical oxidation and good electrolyte wettability.

[0003] At present, most of the mainstream commercial diaphragms are polyolefin diaphragms, including polyethylene (PE), polypropylene (PP), and PP / PE / PP three-layer composite diaphragms. Polyolefin diaphragms are relatively low in price and have good chemical stability and mechanical properties, so they are widely used. However, due to their low polarity and low surface energy, they have poor wettability to electrolytes, resulting in low lithium ion conductivity. In addition, this type of diaphragm has poor temperature resistance. Under excessive charging and discharging or high temperature conditions, the diaphragm shrinks significantly or even melts, causing direct contact and short circuit between the positive and negative electrodes of the battery, which can easily lead to safety accidents. Therefore, the current mainstream polyolefin diaphragms can no longer meet the use and safety requirements of lithium batteries in more scenarios, and the development of diaphragms with lower internal resistance and higher temperature resistance has become an inevitable trend.

[0004] In order to improve the thermal stability of the diaphragm, the currently widely used method is to utilize the strategy of organic / inorganic material composite to coat an inorganic filler layer on the polyolefin base film, such as aluminum oxide, zirconium oxide, silicon oxide, titanium oxide, magnesium oxide, etc. Patent CN102181204A discloses a method for preparing a high-temperature resistant diaphragm by coating a high-temperature resistant powder. Since the inorganic powder coating has high thermal stability and mechanical properties, the safety of the battery is greatly improved. However, this coating method also greatly increases the weight and thickness of the diaphragm. At the same time, the composite modification method not only requires a complex formula, but also has a relatively complicated preparation process. It needs to go through multiple steps such as dispersion, pulping, filtration, coating, and drying. The processing process is complicated, and it also faces problems such as low bonding strength between the inorganic filler coating and the polyolefin base film, and easy shedding of inorganic particles.

[0005] In view of the various problems existing in composite modified polyolefin diaphragms, people have turned their attention to finding new materials to replace polyolefins as diaphragm substrates. As a high-temperature resistant material with excellent comprehensive performance, polyimide has an operating temperature of up to 300°C and no obvious melting point. It has high insulation properties and is a potential high-temperature resistant diaphragm material. He et al. used monomers with different structures to synthesize a variety of polyimide diaphragms and found that their thermal dimensional stability, electrolyte wettability, electrolyte absorption and other performance indicators were better than those of polypropylene diaphragms (Electrochimica Acta, 2020, 337, 135838). However, the current preparation methods of polyimide diaphragms are still limited to laboratories, including template methods, phase separation methods and electrospinning methods. The processing technology is complicated and the cost is high, which limits its production and use. Cross-linked polymers are also a typical class of substances with high temperature stability. Therefore, preparing a cross-linked polymer film with a porous structure is also a strategy for preparing high-temperature resistant diaphragms. Patent CN105280866A discloses a method for preparing a cross-linked polyurethane diaphragm by foaming polyether polyol and isocyanate, which has a thickness of 5-41 μm and a porosity of 70-75%, and has the advantages of high porosity, low thickness, high liquid absorption, and low resistance. However, its preparation process is still relatively complicated, requiring multiple steps such as foaming, slicing, and stamping, and the foaming process is difficult to control, and uneven foaming voids are prone to occur. Summary of the invention

[0006] In view of this, the object of the present invention is to provide a high temperature resistant polymer, a high temperature resistant polymer film and a lithium battery. The high temperature resistant polymer separator has excellent thermal stability and is easy to prepare.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a high temperature resistant polymer obtained by polymerization of a cyclic polyamine and a polyvalent activated alkyne;

[0009] The molar ratio of the cyclic polyamine to the polyvalent activated alkyne is 1:0.8 to 1:1.2, preferably 1:1;

[0010] The cyclic polyamine is a substituted or unsubstituted C4-C30 cycloalkane containing 2 or more -NH-;

[0011] The polyvalent activated alkyne is obtained by reacting a polyol with propiolic acid, and the polyol contains 2 or more -OH groups.

[0012] Preferably, at least one of the cyclic polyamine and the polyvalent activated alkyne comprises 3 or more functional groups.

[0013] Preferably, the cyclic polyamine is selected from any one or more of the following formulae 1 to 8:

[0014]

[0015] Preferably, the polyol is selected from any one or more of ethylene glycol, 1,4-butanediol, glycerol, 1,2,4,5-tetrahydroxybenzene, dipentaerythritol or polymer-based polyol.

[0016] Preferably, the polymer-based polyol is selected from any one or more of polyether polyol, polycarbonate polyol, polycarbonate ether polyol or polyester polyol.

[0017] Preferably, the polymerization is carried out in the presence of a solvent.

[0018] Preferably, the solvent is selected from any one or more of dichloromethane, chloroform, N,N-dimethylformamide, tetrahydrofuran, ethanol or water.

[0019] In a second aspect, the present invention provides a high temperature resistant polymer film, which is composed of the high temperature resistant polymer involved in the above technical solution;

[0020] Preferably, the thickness of the high temperature resistant polymer film is 5 to 50 μm.

[0021] In a third aspect, the present invention provides a lithium battery, which includes a positive electrode, a negative electrode and a separator; the separator is the high temperature resistant polymer film involved in the above technical solution.

[0022] Preferably, the positive electrode includes any one of lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt manganese oxide or lithium nickel cobalt oxide.

[0023] Preferably, the negative electrode comprises any one of lithium, graphite, soft carbon, hard carbon or silicon.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The existing mainstream polyolefin diaphragms on the market have the problem of poor thermal stability and cannot be used at high temperatures or for long periods of time. They are prone to shrinkage and internal short circuits. The high-temperature resistant polymer film provided by the present invention can be obtained by addition polymerization of cyclic polyamines and polyvalent activated alkynes. The steps are simple and can be carried out at room temperature and in an air environment. At the same time, this polymerization reaction does not require a catalyst, avoiding the introduction of other impurities. It not only simplifies the formula, but also avoids electrode side reactions that may be caused by catalyst residues. The obtained polymer film has a cross-linked regular honeycomb chemical network structure and good high-temperature dimensional stability. There is no obvious dimensional shrinkage when heated at 200°C for 1 hour.

[0026] (2) Compared with the high temperature and high pressure conditions required in the preparation process of polyolefin materials, the click reaction of activated alkynes in the present invention can achieve the click reaction of polyvalent activated alkynes and cyclic polyamines within a few minutes at room temperature and in air. At the same time, this reaction does not require a catalyst, avoiding the introduction of other impurities, which not only simplifies the formula, but also avoids electrode side reactions that may be caused by catalyst residues;

[0027] (3) The existing technical solutions for preparing cross-linked polymer separators have a relatively complicated preparation process, which requires multiple steps such as pore making, slicing, and sheet pressing. The present invention utilizes the intrinsic micropores caused by the regular honeycomb chemical network structure of the high temperature resistant polymer, avoiding the complicated pore making process, and can prepare a porous film through a simple solution casting method to achieve electrolyte infiltration and absorption;

[0028] After testing, it was found that the lithium battery using the above-mentioned high-temperature resistant polymer film as the separator had a significantly improved ionic conductivity and a significantly improved electrochemical stability. DETAILED DESCRIPTION

[0029] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The present invention provides a high temperature resistant polymer obtained by polymerization of a cyclic polyamine and a polyvalent activated alkyne. The amino group in the cyclic polyamine reacts with the alkynyl group in the polyvalent activated alkyne to generate an alkenyl group. In the present invention, the molar ratio of the cyclic polyamine to the polyvalent activated alkyne is 1:0.8 to 1:1.2, preferably 1:0.9 to 1:1.1, and more preferably 1:1.

[0031] The cyclic polyamine is a substituted or unsubstituted C4-C30 cycloalkane containing 2 or more -NH- groups, so as to obtain a polymer with a cross-linked network structure. The substituted or unsubstituted group is selected from C1-C6 alkyl groups.

[0032] In some specific embodiments of the present invention, the cyclic polyamine can be selected from any one or more of the following formulae 1 to 8:

[0033]

[0034] Among them, the substance shown in formula 1 is piperazine; the substance shown in formula 2 is homopiperazine; the substance shown in formula 3 is 6-methyl-1,4-diazacycloheptane; the substance shown in formula 4 is 1,4,7-triazacyclononane; the substance shown in formula 5 is cyclopentane; the substance shown in formula 6 is 2,5,8,11-tetramethyl-1,4,7,10-pentaazacyclopentadecane; the substance shown in formula 7 is 1,4,8,11-tetraazacyclotetradecane; the substance shown in formula 8 is 1,4,7,10,13-pentaazacyclopentadecane.

[0035] In the present invention, the polyvalent activated alkyne is obtained by reacting a polyol with propiolic acid, and the polyol contains 2 or more -OH groups. The polyol specifically includes but is not limited to any one or more of ethylene glycol, 1,4-butanediol, glycerol, 1,2,4,5-tetrahydroxybenzene, dipentaerythritol or a polymer-based polyol; the polymer-based polyol is selected from any one or more of polyether polyol, polycarbonate polyol, polycarbonate ether polyol or polyester polyol. In some embodiments of the present invention, it is preferred that the polyol and propiolic acid react under the action of a catalyst, and the hydroxyl group in the polyol reacts with the carboxyl group of propiolic acid to form an ester bond, and the catalyst can be selected from any one or more of p-toluenesulfonic acid, 4-dimethylaminopyridine, concentrated sulfuric acid, thionyl chloride, etc.

[0036] It should be noted that in order to make the high temperature resistant polymer have a more regular honeycomb chemical network structure to form micropores, it is preferred that during the reaction of the cyclic polyamine and the polyvalent activated alkyne, at least one of the raw materials cyclic polyamine and the polyvalent activated alkyne includes 3 or more functional groups.

[0037] The present invention also provides a method for preparing the above-mentioned high temperature resistant polymer, comprising the following steps:

[0038] The cyclic polyamine and the polyvalent activated alkyne are polymerized in the presence of a solvent to obtain a high temperature resistant polymer.

[0039] According to the present invention, a polyvalent activated alkyne is first provided. In some embodiments of the present invention, it is preferred to mix a polyol, propiolic acid, a catalyst and a solvent, heat to reflux, and react to obtain a polyvalent activated alkyne. Wherein, the polyol and the catalyst are as described in the relevant contents of the above technical scheme, and are not repeated here; the solvent can be selected from toluene. The temperature of the heating reflux is 120 to 180°C, and the reaction is preferably carried out under stirring conditions, and the stirring time is 12 to 20 hours. In some preferred embodiments of the present invention, after the reaction is completed, the product is preferably washed with water and dried to obtain a polyvalent activated alkyne.

[0040] Then, according to the present invention, a cyclic polyamine and a polyvalent activated alkyne are subjected to a polymerization reaction in the presence of a solvent to obtain a high temperature resistant polymer. The cyclic polyamine and the polyvalent activated alkyne are as described in the relevant contents of the above technical scheme, and will not be repeated here; the solvent is selected from any one or more of dichloromethane, chloroform, N,N-dimethylformamide, tetrahydrofuran, ethanol or water. The polymerization reaction can be carried out at room temperature and in an air environment, and the polymerization reaction time is 5 to 30 minutes, preferably 10 to 20 minutes. In the present invention, during the above polymerization reaction, the molar ratio of the cyclic polyamine and the polyvalent activated alkyne is 1:0.8 to 1:1.2, preferably 1:1, in order to ensure that the amino group and the alkyne group react completely to obtain a polymer network with a highly cross-linked structure.

[0041] In some embodiments of the present invention, the cyclic polyamine solution and the polyvalent activated alkyne solution are preferably mixed and reacted to obtain a high temperature resistant polymer, wherein the solvents in the cyclic polyamine solution and the polyvalent activated alkyne solution are independently selected from any one or more of dichloromethane, chloroform, N,N-dimethylformamide, tetrahydrofuran, ethanol or water.

[0042] The preparation method of the high temperature resistant polymer provided by the present invention utilizes the click reaction of activated alkynes to realize the click reaction of polyvalent activated alkynes and cyclic polyamines within a few minutes under room temperature and air environment. At the same time, the reaction does not require a catalyst, thus avoiding the introduction of other impurities, which not only simplifies the formula, but also avoids electrode side reactions that may be caused by catalyst residues.

[0043] The present invention also provides a high temperature resistant polymer film, which is composed of the high temperature resistant polymer involved in the above technical solution. In the present invention, the thickness of the high temperature resistant polymer film is 5 to 50 μm, which can be 5 μm, 8 μm, 10 μm, 15 μm, 20 μm, 30 μm, 40 μm or 50 μm, etc. The above numerical values ​​are only for enumeration and are not limited thereto, and other point values ​​within the numerical range are applicable.

[0044] The present invention also provides a method for preparing the above-mentioned high temperature resistant polymer film, comprising:

[0045] The cyclic polyamine and the polyvalent activated alkyne are polymerized in the presence of a solvent to obtain a reactant;

[0046] Place the reactants in a mold, let them stand, and then dry them after solidification.

[0047] In some embodiments of the present invention, the cyclic polyamine solution and the polyvalent activated alkyne solution are preferably mixed uniformly and then quickly poured into a polytetrafluoroethylene mold, left to stand for 5 to 30 minutes, and dried after being completely solidified to obtain a high temperature resistant polymer film.

[0048] The present invention conducts liquid absorption, corrosion resistance and heat shrinkage tests on the obtained high temperature resistant polymer film, and finds that the high temperature resistant polymer film has excellent liquid absorption rate, good electrolyte corrosion resistance and good thermal stability (no obvious dimensional shrinkage after heating at 200°C for 1h).

[0049] Based on the above-mentioned good performance of the high temperature resistant polymer film, the present invention applies it as a diaphragm in a lithium battery. Therefore, the present invention also provides a lithium battery, including a positive electrode, a negative electrode and a diaphragm; the diaphragm is a high temperature resistant polymer film. In some embodiments of the present invention, the positive electrode includes lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt manganese oxide and lithium nickel cobalt oxide. In some embodiments of the present invention, the negative electrode includes lithium, graphite, soft carbon, hard carbon and silicon.

[0050] After testing, it was found that the SS||SS symmetrical battery obtained with high-temperature resistant polymer film as the separator was subjected to ionic conductivity test and electrochemical stability test, and it was found that the ionic conductivity and electrochemical stability of the separator were significantly improved.

[0051] In order to further illustrate the present invention, the following examples are provided for detailed description. The experimental raw materials used in the following examples of the present invention are all common commercially available products.

[0052] Example 1

[0053] Step 1: Preparation of polyvalent activated alkynes

[0054] Dissolve glycerol (0.92 g, 10 mmol), propiolic acid (2.52 g, 36 mmol), and p-toluenesulfonic acid (0.10 g, 0.6 mmol) in 100 mL of toluene, heat under reflux at 120°C, and stir for 12 h; after the reaction, wash with water and dry to obtain a ternary activated alkyne;

[0055]

[0056] Step 2: Preparation of cross-linked polymer film by click polymerization

[0057] The ternary activated alkyne (2.48 g, 10 mmol) was dissolved in 5 mL of dichloromethane to obtain precursor solution A, and piperazine (1.29 g, 15 mmol) was dissolved in 5 mL of dichloromethane to obtain precursor solution B. The precursor solutions A and B were evenly mixed and quickly poured into a polytetrafluoroethylene mold, allowed to stand for 30 minutes, and dried after being completely solidified. The obtained film thickness was 8 μm.

[0058] Example 2

[0059] Step 1: Preparation of polyvalent activated alkynes

[0060] Dissolve 1,2,4,5-tetrahydroxybenzene (1.42 g, 10 mmol), propiolic acid (3.36 g, 48 mmol), and p-toluenesulfonic acid (0.14 g, 0.8 mmol) in 100 mL of toluene, heat under reflux at 120°C, and stir for 12 h; after the reaction, wash with water and dry to obtain a quaternary activated alkyne;

[0061]

[0062] Step 2: Preparation of cross-linked polymer film by click polymerization

[0063] The quaternary activated alkyne (3.50 g, 10 mmol) was dissolved in 4 mL of dichloromethane to obtain precursor solution A, and homopiperazine (2.00 g, 20 mmol) was dissolved in 5 mL of dichloromethane to obtain precursor solution B. The precursor solutions A and B were evenly mixed and quickly poured into a polytetrafluoroethylene mold, allowed to stand for 20 minutes, and dried after being completely solidified. The obtained film thickness was 10 μm.

[0064] Example 3

[0065] Step 1: Preparation of polyvalent activated alkynes

[0066] Dissolve dipentaerythritol (2.54 g, 10 mmol), propiolic acid (5.04 g, 72 mmol), and p-toluenesulfonic acid (0.21 g, 1.2 mmol) in 100 mL of toluene, heat under reflux at 120°C, and stir for 12 h; after the reaction, wash with water and dry to obtain a six-membered activated alkyne;

[0067]

[0068] Step 2: Preparation of cross-linked polymer film by click polymerization

[0069] The six-membered activated alkyne (5.66 g, 10 mmol) was dissolved in 5 mL of dichloromethane to obtain precursor solution A, and 6-methyl-1,4-diazacycloheptane (3.42 g, 30 mmol) was dissolved in 6 mL of dichloromethane to obtain precursor solution B. The precursor solutions A and B were evenly mixed and quickly poured into a polytetrafluoroethylene mold, allowed to stand for 20 minutes, and dried after it was completely solidified. The thickness of the obtained film was 15 μm.

[0070] Example 4

[0071] Step 1: Preparation of polyvalent activated alkynes

[0072] Dissolve ethylene glycol (0.62 g, 10 mmol), propiolic acid (1.68 g, 24 mmol), and p-toluenesulfonic acid (0.069 g, 0.4 mmol) in 10 mL of toluene, heat under reflux at 120°C, and stir for 12 h; after the reaction, wash with water and dry to obtain a binary activated alkyne;

[0073]

[0074] Step 2: Preparation of cross-linked polymer film by click polymerization

[0075] The binary activated alkyne (1.66 g, 10 mmol) was dissolved in 3 mL of dichloromethane to obtain precursor solution A, and 1,4,7-triazacyclononane (0.86 g, 6.67 mmol) was dissolved in 2 mL of dichloromethane to obtain precursor solution B. The precursor solutions A and B were evenly mixed and quickly poured into a polytetrafluoroethylene mold, allowed to stand for 10 minutes, and dried after it was completely solidified. The resulting film had a thickness of 8 μm.

[0076] Example 5

[0077] Step 1: Preparation of polyvalent activated alkynes

[0078] Dissolve polyethylene glycol-400 (4.00 g, 10 mmol), propiolic acid (1.68 g, 24 mmol), and p-toluenesulfonic acid (0.069 g, 0.4 mmol) in 10 mL of toluene, heat under reflux at 120°C, and stir for 12 h; after the reaction, wash with water and dry to obtain a binary activated alkyne;

[0079]

[0080] Step 2: Preparation of cross-linked polymer film by click polymerization

[0081] The binary activated alkyne (5.40 g, 10 mmol) was dissolved in 6 mL of water to obtain precursor solution A, and the cyclopentane (0.86 g, 5 mmol) was dissolved in 1 mL of water to obtain precursor solution B. The precursor solutions A and B were evenly mixed and then quickly poured into a polytetrafluoroethylene mold, allowed to stand for 10 minutes, and dried after it was completely solidified. The resulting film had a thickness of 15 μm.

[0082] Example 6

[0083] Step 1: Preparation of polyvalent activated alkynes

[0084] Dissolve polypropylene carbonate diol-1000 (10.00 g, 10 mmol), propiolic acid (1.68 g, 24 mmol), p-toluenesulfonic acid (0.069 g, 0.4 mmol) in 20 mL of toluene, heat under reflux at 120°C, and stir for 12 h; after the reaction, wash with water and dry to obtain binary activated alkyne;

[0085]

[0086] Step 2: Preparation of cross-linked polymer film by click polymerization

[0087] The binary activated alkyne (11.40 g, 10 mmol) was dissolved in 6 mL of tetrahydrofuran to obtain precursor solution A, and 2,5,8,11-tetramethyl-1,4,7,10-tetraazacyclododecane (1.14 g, 5 mmol) was dissolved in 1 mL of water to obtain precursor solution B. The precursor solutions A and B were evenly mixed and quickly poured into a polytetrafluoroethylene mold, allowed to stand for 10 minutes, and dried after it was completely solidified. The resulting film had a thickness of 20 μm.

[0088] Example 7

[0089] Step 1: Preparation of polyvalent activated alkynes

[0090] Dissolve polycarbonate ether polyol (20.00 g, 10 mmol) with a number average molecular weight of 2000 g / mol, propiolic acid (1.68 g, 24 mmol), and p-toluenesulfonic acid (0.069 g, 0.4 mmol) in 40 mL of toluene, heat under reflux at 120° C., and stir for 12 h; after the reaction, wash with water and dry to obtain a binary activated alkyne;

[0091]

[0092] Step 2: Preparation of cross-linked polymer film by click polymerization

[0093] The binary activated alkyne (21.40 g, 10 mmol) was dissolved in 10 mL of tetrahydrofuran to obtain precursor solution A, and 1,4,8,11-tetraazacyclotetradecane (1.00 g, 5 mmol) was dissolved in 1 mL of tetrahydrofuran to obtain precursor solution B. The precursor solutions A and B were evenly mixed and quickly poured into a polytetrafluoroethylene mold, allowed to stand for 30 minutes, and dried after being completely solidified. The obtained film thickness was 40 μm.

[0094] Example 8

[0095] Step 1: Preparation of polyvalent activated alkynes

[0096] Dissolve polyethylene terephthalate diol (15.00 g, 10 mmol) with a number average molecular weight of 1500 g / mol, propiolic acid (1.68 g, 24 mmol), and p-toluenesulfonic acid (0.069 g, 0.4 mmol) in 40 mL of toluene, heat under reflux at 120° C., and stir for 12 h; after the reaction, wash with water and dry to obtain a binary activated alkyne;

[0097]

[0098] Step 2: Preparation of cross-linked polymer film by click polymerization

[0099] The binary activated alkyne (16.40 g, 10 mmol) was dissolved in 10 mL of N, N-dimethylformamide to obtain precursor solution A, and 1,4,7,10,13-pentaazacyclopentadecane (0.86 g, 4 mmol) was dissolved in 1 mL of N, N-dimethylformamide to obtain precursor solution B. The precursor solutions A and B were evenly mixed and quickly poured into a polytetrafluoroethylene mold, allowed to stand for 30 minutes, and dried after being completely solidified. The obtained film thickness was 30 μm.

[0100] Liquid absorption performance test

[0101] The films prepared in Examples 1 to 8, commercial PE diaphragms and PP diaphragms (for comparison) were soaked in electrolyte for 24 hours and then taken out. The electrolyte on the surface of the film was absorbed with absorbent paper and then weighed. The liquid absorption rate of the film was calculated based on the weight change before and after the film was soaked. The specific test results are shown in Table 1 below:

[0102] Table 1

[0103] Group Liquid absorption rate (%) Example 1 200 Example 2 213 Example 3 228 Example 4 196 Example 5 240 Example 6 265 Example 7 308 Example 8 289 PE 160 PP 96

[0104] It can be seen from Table 1 that, compared with commercial PE diaphragms and PP diaphragms, the films prepared by the present invention have higher liquid absorption rates.

[0105] Corrosion resistance test

[0106] The films prepared in Examples 1 to 8 were respectively immersed in the electrolyte for 48 hours and then taken out to observe the changes in the diaphragms.

[0107] The test results showed that all films showed no morphological changes, indicating that the films prepared by this method have good resistance to electrolyte corrosion.

[0108] Heat shrinkage test

[0109] The films prepared in Examples 1 to 8, commercial PE diaphragms and PP diaphragms (for comparison) were placed in an oven at 120° C. and 200° C. for 1 hour, respectively, and their dimensional shrinkage rates were measured. The results are shown in Table 2 below:

[0110] Table 2

[0111]

[0112]

[0113] It can be seen from Table 2 that, compared with commercial PE diaphragms and PP diaphragms, the thermal shrinkage of the film prepared by the present invention is greatly improved.

[0114] Ionic conductivity test

[0115] The films prepared in Examples 1 to 8, commercial PE separators and PP separators (for comparison) were assembled into SS||SS symmetrical cells, and the ionic conductivity at 25° C. was measured. The results are shown in Table 3 below:

[0116] Group Ionic conductivity (mS / cm) Example 1 0.70 Example 2 0.75 Example 3 0.77 Example 4 0.69 Example 5 0.72 Example 6 0.88 Example 7 1.02 Example 8 0.93 PE 0.50 PP 0.44

[0117] It can be seen from Table 3 that, compared with commercial PE and PP membranes, the ionic conductivity of the film prepared by the present invention is significantly improved.

[0118] Electrochemical stability test

[0119] The films prepared in Examples 1 to 8, commercial PE separators and PP separators (for comparison) were subjected to linear voltammetric scanning, and the results are shown in Table 4 below:

[0120] Table 4

[0121] Group Oxidation potential (V) Example 1 4.4 Example 2 4.5 Example 3 4.4 Example 4 4.3 Example 5 4.2 Example 6 4.5 Example 7 4.4 Example 8 4.5 PE 4.2 PP 4.2

[0122] It can be seen from Table 4 that, compared with commercial PE and PP diaphragms, the electrochemical stability of the film prepared by the present invention is significantly improved.

[0123] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A high temperature resistant polymer, characterized in that: It is obtained by polymerization of cyclic polyamines and polyvalent activated alkynes; The molar ratio of the cyclic polyamine to the polyvalent activated alkyne is 1:0.8 to 1:1.2; The cyclic polyamine is a substituted or unsubstituted C4-C30 cycloalkane containing 2 or more -NH-; The polyvalent activated alkyne is obtained by reacting polyol with propiolic acid.

2. The high temperature resistant polymer according to claim 1, characterized in that: At least one of the cyclic polyamine and the polyvalent activated alkyne includes three or more functional groups.

3. The high temperature resistant polymer according to claim 1 or 2, characterized in that: The cyclic polyamine is selected from any one or more of the following formulas 1 to 8:

4. The high temperature resistant polymer according to any one of claims 1 to 3, characterized in that The polyol is selected from any one or more of ethylene glycol, 1,4-butanediol, propylene glycol, 1,2,4,5-tetrahydroxybenzene, dipentaerythritol or polymer-based polyol; The polymer-based polyol is selected from any one or more of polyether polyol, polycarbonate polyol, polycarbonate ether polyol or polyester polyol.

5. The high temperature resistant polymer according to any one of claims 1 to 4, characterized in that The polymerization is carried out in the presence of a solvent.

6. The high temperature resistant polymer according to claim 5, characterized in that: The solvent is selected from any one or more of dichloromethane, chloroform, N,N-dimethylformamide, tetrahydrofuran, ethanol or water.

7. A high temperature resistant polymer film, characterized in that: Composed of a high temperature resistant polymer as described in any one of claims 1 to 6; The thickness of the high temperature resistant polymer film is 5 to 50 μm.

8. A lithium battery, characterized in that: Including positive electrode, negative electrode and separator; The diaphragm is the high temperature resistant polymer film as described in claim 7.

9. The lithium battery according to claim 8, characterized in that: The positive electrode includes any one of lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt manganese oxide or lithium nickel cobalt oxide.

10. The lithium battery according to claim 8 or 9, characterized in that: The negative electrode includes any one of lithium, graphite, soft carbon, hard carbon or silicon.

Citation Information

Patent Citations

  • High-temperature-resistant polyarylene ether nitrile lithium ion battery diaphragm material as well as preparation method and application thereof

    CN112898560A

  • Method for preparing nitrogen-containing polymer through click polymerization reaction without catalyst

    CN114716659A

  • Process for preparing graft copolymer comprising polyethylene

    US20200262957A1